Gallium nitride-based transistor structure and fabrication method with buried drain electrode layer
By introducing a P-type buried layer into the composite buffer layer of a gallium nitride-based transistor to form a PIN diode, the problem of insufficient breakdown voltage in gallium nitride-based HEMT devices is solved. This achieves suppression of leakage current at the drain electrode and improvement of breakdown voltage, thus avoiding degradation of conduction characteristics.
Patent Information
- Application Number
- CN202210425090.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-21
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-04-21
AI Technical Summary
The breakdown voltage of existing gallium nitride-based high electron mobility transistors (HEMTs) is much lower than the theoretical value, and conventional improvement methods suffer from problems such as increased capacitance, complex processes, and high costs.
A P-type buried layer connected to the drain electrode is introduced into the composite buffer layer to form a PIN diode, which suppresses electron leakage from the drain electrode in the off state. The PIN diode, composed of the P-type buried layer, gallium nitride channel layer and two-dimensional electron gas channel, expands the space charge region of the device and improves the breakdown voltage.
It effectively reduces leakage current at the drain electrode, increases device breakdown voltage, avoids degradation of conduction characteristics, and improves overall device performance.
Smart Images

Figure CN114843342B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor device technology, specifically relating to a gallium nitride-based transistor that can be used in power electronic systems. Background Technology
[0002] Gallium nitride (GaN), as a typical third-generation semiconductor material, possesses excellent characteristics such as a large bandgap, high electron mobility, and high electron saturation velocity, making it highly promising for applications in next-generation radio frequency devices and power electrical devices. Due to its inherent polarization effect, GaN heterojunction structures with different bandgap widths can form a high-concentration, high-electron-mobility two-dimensional electron gas at the junction interface, even without intentional doping. This allows for the fabrication of high electron mobility transistors (HEMTs) based on GaN heterojunction structures, which exhibit high breakdown voltage, low on-resistance, high switching frequency, small size, and the ability to operate at high temperatures, high frequencies, strong radiation, and high power. HEMTs are considered candidate core switching devices for next-generation power electronic systems and are suitable for applications in consumer electronics, data center power supplies, home appliances, electric vehicles, rail transportation, and smart grids. Although GaN-based power electronic devices have achieved good breakdown characteristics, comparisons with other excellent GaN materials reveal that the breakdown voltage of currently fabricated devices is still far below the theoretical value of 3.3 MV / cm.
[0003] Gallium nitride (GaN) breakdown typically results from impact ionization caused by a localized high electric field, leading to avalanche breakdown. GaN-based high electron mobility transistors (HEMTs) are lateral devices. In the off-state with a high reverse drain voltage, a depletion layer forms between the gate and the drain electrode. The positive charge in the depletion region and the negatively charged gate electrode create electric field lines, resulting in an electric field peak at the gate electrode edge on the drain side. When the drain voltage is very high, this electric field peak exceeds the material's critical breakdown electric field strength, causing impact ionization of charge carriers in that region, leading to avalanche breakdown. Furthermore, conventional HEMT devices require annealing after the ohmic contact metals evaporate from the source and drain electrodes to form a true ohmic contact. During annealing, the different depths of the source and drain metals within the material create metal spikes, further contributing to impact ionization and avalanche breakdown. Currently, the introduction of gate or drain field plates can effectively improve the breakdown characteristics of devices. However, these technologies have some drawbacks. For example, the introduction of field plates will introduce additional capacitance, reducing the frequency characteristics of the device. In addition, in silicon-based gallium nitride HEMT devices, substrate transfer technology is used to completely remove the original silicon substrate and transfer the HEMT structure to an insulating bulk wafer. Although this method can improve the breakdown characteristics, it is relatively complex and costly in terms of process. Although some methods to increase the thickness of the buffer layer can also control the leakage current in the vertical direction of the device, the improvement capability is limited. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of the prior art by providing a gallium nitride-based transistor structure and fabrication method with a buried drain electrode layer, thereby reducing the leakage current of the drain electrode, increasing the device breakdown voltage, and preventing the degradation of the device's conduction characteristics.
[0005] The technical approach to achieving the objective of this invention is as follows: By introducing a P-type buried layer connected to the drain electrode in the composite buffer, electrons leaking from the drain electrode during the off state are effectively suppressed, reducing the drain electrode leakage current; the PIN diode, composed of the P-type buried layer, gallium nitride channel layer, and two-dimensional electron gas channel, helps the device deplete the two-dimensional electron gas in the channel, expanding the space charge region of the device and thus improving the device breakdown voltage; by designing the P-type buried layer only near the drain electrode, at a slightly farther distance from the 2DEG channel, the PIN diode is forward biased in the forward direction, reducing the impact on the on-resistance of the device and avoiding severe degradation of the device's conduction characteristics.
[0006] Based on the above ideas, the technical solution of the present invention is as follows:
[0007] 1. A gallium nitride-based transistor with a buried drain electrode, comprising, from bottom to top: a substrate 1, a composite buffer layer 2, a channel layer 3, a barrier layer 4, and a passivation layer 5, wherein a source electrode 7, a gate electrode 9, and a drain electrode 8 are disposed on the surface of the barrier layer, and the gate electrode forms a Schottky contact with the barrier layer, while the source electrode and the drain electrode both form ohmic contacts with the barrier layer; a heterojunction is formed between the channel layer and the barrier layer, and a two-dimensional electron gas channel is formed on one side of the channel layer 3 at the heterojunction interface due to polarization effect, characterized in that:
[0008] The composite buffer layer 2 is provided with a P-type buried layer 6. The P-type buried layer 6, together with the channel layer 3 and the heterojunction interface, form a two-dimensional electron gas channel to form a PIN diode, which suppresses electrons leaking from the drain electrode in the off state and improves the off-state breakdown voltage.
[0009] The drain electrode 8 passes through the barrier layer and the channel layer, and enters the composite buffer layer to connect with the P-type buried layer 6.
[0010] The barrier layer 4, the channel layer 3, and the composite buffer layer 2 are made of group III nitride semiconductors, namely gallium nitride, aluminum nitride, indium nitride, or a multi-component compound composed of two or more of them.
[0011] Furthermore, the P-type buried layer 6 is made of gallium nitride or aluminum gallium nitride, with a P-type doping type and a doping concentration of 1x10⁻⁶. 16 -1x10 20 cm -3 The thickness is 50-1000nm.
[0012] Furthermore, the substrate 1 is made of one of silicon, silicon carbide, sapphire, and diamond.
[0013] Furthermore, the composite buffer layer 2 includes a nucleation layer 21, a transition layer 22, and a buffer layer 23 from bottom to top, and the P-type buried layer 6 is disposed in the buffer layer 23.
[0014] Furthermore, the nucleation layer 21 is made of aluminum nitride with a thickness of 100-300 nm; the transition layer 22 is made of graded aluminum gallium nitride with an aluminum composition that gradually changes from 0.75 to 0.15 and a thickness of 200-1000 nm; the buffer layer 23 is made of gallium nitride or aluminum gallium nitride, with a main trap doping of 1×10⁻⁶. 15 cm -3 -1×10 17 cm -3 The thickness is 100-3000nm.
[0015] Furthermore, the channel layer 3 is made of gallium nitride or indium gallium nitride, with a thickness of 50nm-500nm; the barrier layer 4 is made of aluminum gallium nitride, indium aluminum nitride, aluminum nitride, or indium aluminum gallium nitride, with a thickness of 2-40nm; and the passivation layer 5 is made of SiN or SiO2.
[0016] Furthermore, the bottommost first layer of the gate electrode 9 is any one of Ti, Ni, Al, Ta, TiN, or TaN; the bottom two layers of the source electrode 7 and the drain electrode 8, from bottom to top, are Ti / Al, Ta / Al, or Mo / Al, respectively.
[0017] 2. A method for fabricating a gallium nitride-based transistor with a buried drain electrode layer, characterized by comprising the following steps:
[0018] S1: A composite buffer layer is formed by sequentially growing a group III nitride nucleation layer, a transition layer, and a buffer layer on the substrate using metal-organic chemical vapor deposition (MOCVD).
[0019] S2: A P-type buried layer is fabricated on the surface of the buffer layer using ion implantation. The doping concentration of this buried layer is 1x10⁻⁶. 16 -1x10 20 cm-3, with a thickness of 50-1000 nm;
[0020] S3: Channel layer and barrier layer are epitaxially grown on buffer layer using metal-organic chemical vapor deposition (MOCVD).
[0021] S4: Reactive ion etching (RIE) is used for etching isolation. The barrier layer, channel layer and part of the buffer layer are etched away in the right region of the barrier layer. The etching depth is 150nm. The mesa should have neat edges and steep sidewalls.
[0022] S5: Prepare a source electrode on the surface of the barrier layer and perform high-temperature thermal annealing to form an ohmic contact with the two-dimensional electron gas;
[0023] S6: Photolithography is used to form a drain electrode region on the right side of the barrier layer to form a drain groove. The depth of the drain groove reaches the buried layer 6. Metal is filled in the drain groove. A multilayer metal system is grown on the heterojunction by electron beam evaporation to prepare the drain electrode. High-temperature annealing is then performed to form an ohmic contact with the two-dimensional electron gas.
[0024] S7: A nitride film is deposited between the source and drain electrodes on the surface of the barrier layer using PECVD deposition to form a passivation layer;
[0025] S8: A gate pattern is photolithographically patterned on the passivation layer, and then the exposed passivation layer is removed using reactive ion etching. Finally, the gate metal is fabricated to form a Schottky contact with the barrier layer, completing the device fabrication. This invention has the following advantages compared to existing technologies:
[0026] First, by introducing a P-type buried layer into the composite buffer and connecting it to the drain electrode, the present invention effectively suppresses electrons leaking from the drain electrode during the off state and reduces the leakage current of the drain electrode.
[0027] Secondly, since the present invention consists of a P-type buried layer, a gallium nitride channel layer and a two-dimensional electron gas channel forming a PIN diode, it can help the device deplete the two-dimensional electron gas in the channel, expand the space charge region of the device, increase the breakdown voltage of the device, and improve the overall performance of the device.
[0028] Third, because the P-type buried layer is designed only near the drain electrode and is slightly farther away from the 2DEG (two-dimensional electron gas) channel, the PIN diode is forward biased when in the forward direction, which has little impact on the on-resistance of the device and will not cause serious degradation of the device's conduction characteristics. Attached Figure Description
[0029] Figure 1 This is a schematic diagram of the transistor structure of the present invention;
[0030] Figure 2 This is a schematic diagram of a transistor representing a composite buffer layer structure in this invention;
[0031] Figure 3 This is a schematic diagram illustrating the fabrication process of a gallium nitride-based transistor with a buried drain electrode layer, as per the present invention. Detailed Implementation
[0032] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0033] Reference Figure 1 and Figure 2The present invention relates to a gallium nitride-based transistor with a buried drain electrode, comprising a substrate 1, a composite buffer layer 2, a channel layer 3, a barrier layer 4, a passivation layer 5, a P-type buried layer 6, a source electrode 7, a drain electrode 8, and a gate electrode 9, wherein:
[0034] The substrate 1 may be made of silicon, sapphire, silicon carbide, or diamond.
[0035] The composite buffer layer 2, located on the substrate 1, comprises three layers: a nucleation layer 21, a transition layer 22, and a buffer layer 23. The nucleation layer is made of aluminum nitride and has a thickness of 100-300 nm. The transition layer uses graded aluminum gallium nitride, with the aluminum composition gradually changing from 0.75 to 0.15, and has a thickness of 200-1000 nm. The buffer layer uses gallium nitride or aluminum gallium nitride and is doped with a main trap doping of 1×10⁻⁶. 15 cm -3 -1×10 17 cm -3 The thickness is 100-3000nm.
[0036] The channel layer 3, located above the buffer layer 23, is made of gallium nitride or aluminum gallium nitride, with a thickness of 50-500 nm and a host trap doping of 1×10⁻⁶. 15 cm -3 -1×10 17 cm -3 This is used to reduce leakage current in the buffer layer;
[0037] The barrier layer 4 is located above the channel layer 3, and a heterojunction is formed between it and the channel layer. A two-dimensional electron gas channel is formed on one side of the channel layer 3 at the interface of the heterojunction due to the polarization effect. The barrier layer is made of aluminum gallium nitride, or indium aluminum nitride, or aluminum nitride, or indium aluminum gallium nitride, and has a thickness of 2-40nm.
[0038] The passivation layer 5, located above the barrier layer 4, is made of SiN or SiO2.
[0039] The P-type buried layer 6 is located within the buffer layer 23. It is made of gallium nitride or aluminum gallium nitride, with P-type doping and a doping concentration of 1x10⁻⁶. 16 -1x10 20 cm -3 The thickness is 50-1000nm. The two-dimensional electron gas channel formed by the P-type buried layer 6, the channel layer 3 and the heterojunction interface constitutes a PIN diode to suppress electrons leaking from the drain electrode in the off state and improve the off-state breakdown voltage.
[0040] The source electrode 7 is located on one side of the surface of the passivation layer 5 and forms an ohmic contact with the barrier layer. The source electrode uses four metal layers: Ti / Al / Ni / Au, where the bottom two layers are Ti / Al, Ta / Al, or Mo / Al.
[0041] The drain electrode 8 is located on the other side of the passivation layer 5. It passes through the barrier layer 4 and the channel layer 3 in sequence, and extends into the buffer layer 23 to connect with the P-type buried layer and form an ohmic contact with the barrier layer. The drain electrode uses four metal layers of Ti / Al / Ni / Au, of which the bottom two layers are Ti / Al, Ta / Al, or Mo / Al.
[0042] The gate electrode 9 is located between the source and drain electrodes on the surface of the passivation layer 5, and forms a Schottky contact with the barrier layer. The gate electrode uses two metal layers: the upper metal layer is Au, and the lower metal layer is Ti, Ni, Al, Ta, TiN, or TaN.
[0043] Reference Figure 3 The present invention provides the following three embodiments for fabricating the above-mentioned device:
[0044] Example 1: A silicon substrate with a thickness of 675 μm, an aluminum nitride nucleation layer with a thickness of 100 nm, an aluminum gallium nitride transition layer with a thickness of 200 nm, and a gallium nitride buffer layer with a thickness of 100 nm and acceptor trap doping of 1 × 10⁻⁶ μm were fabricated. 15 cm -3、 The GaN channel layer is 50 nm thick, the AlGaN barrier layer is 10 nm thick, the SiN passivation layer is 50 nm thick, and the GaN p-type buried layer is 50 nm thick with a doping concentration of 1 x 10⁶. 16 -cm -3 The transistor has Ti / Al as the bottom two layers of the source and drain electrodes and Ti as the bottom layer of the gate electrode.
[0045] Step 1: Clean the silicon substrate, such as... Figure 3 As shown in a.
[0046] At a high temperature of 1000℃, hydrogen gas is introduced into the reaction chamber to remove contaminants from the surface of silicon substrate 1 and form a microscopic step structure on the substrate surface so that various epitaxial layers can be grown in subsequent epitaxial processes.
[0047] Step 2: Epitaxially grow composite buffer layer 2 on substrate 1, such as... Figure 3 As shown in b.
[0048] The composite buffer layer 2 consists of three layers, namely, an aluminum nitride nucleation layer 21 with a thickness of 100 nm is first grown on the substrate using the MOCVD method at a low temperature of 500℃.
[0049] Then, the temperature was raised to 1000℃, and Al with a thickness of 200 nm was grown on the nucleation layer using the MOCVD method. 0.75 Ga 0.25 N transition layer 22, and then GaN buffer layer 23 with a thickness of 100nm is grown on the transition layer;
[0050] Finally, the acceptor trap doping concentration of the buffer layer 23 material was increased to 2 × 10⁻⁶ using ion implantation. 15 cm -3 .
[0051] Step 3, fabricate P-type embedded layer 6, as follows Figure 3 As shown in c.
[0052] Ion implantation was used to form a 1x10⁻¹⁰ doped layer on the right side of the surface of buffer layer 23. 16 cm -3 The P-type gallium nitride region is used to form a P-type buried layer 6.
[0053] Step four, fabricate channel layer 3 and barrier layer 4, as follows: Figure 3 As shown in d.
[0054] Using the MOCVD method, a GaN channel layer 3 with a thickness of 50 nm was first grown on the buffer layer at a temperature of 1000 °C; then, a 10 nm thick AlGaN barrier layer 4 was epitaxially grown on the gallium nitride channel layer 3.
[0055] Step 5: Cleaning.
[0056] After completing the above steps, the sample is first placed in acetone to remove organic contaminants from the surface, then placed in an acidic solvent to remove the surface oxide layer and inorganic contaminants, and finally the surface solvent is removed with deionized water and dried in a nitrogen atmosphere.
[0057] Step six: Etch the platform to create an isolation layer, such as... Figure 3 As shown in e.
[0058] Reactive ion etching (RIE) equipment and technology are used to etch away the entire AlGaN barrier layer, GaN channel layer and part of GaN buffer layer in the etching area on the right side of the barrier layer surface, etching out a mesa with a depth of 150nm, neat edges and steep sidewalls, forming an isolation region between different transistors.
[0059] Step 7: Fabricate the source electrode, such as... Figure 3 As shown in f.
[0060] Using photolithography etching, the photoresist on the left side of the barrier region is etched away, exposing the area where the source electrode 7 is to be fabricated.
[0061] Then, a multilayer metal Ti / Al / Ni / Au layer is grown in this region by electron beam evaporation, namely, Ti with a thickness of 20 nm, Al with a thickness of 120 nm, Ni with a thickness of 40 nm, and Au with a thickness of 50 nm from bottom to top, forming the source electrode 7.
[0062] Then, rapid thermal annealing is performed for 30 seconds in a nitrogen atmosphere at 850°C to form an ohmic contact between the source electrode and the barrier layer.
[0063] Step 8: Fabricate the drain electrode.
[0064] The drain electrode pattern 8 is etched in the right region of the barrier layer using photolithography etching. Then, a drain groove with a depth reaching the buried layer 6 is etched in this region. Figure 3 As shown in g;
[0065] Next, metal is filled into the drain trench, specifically by growing a multilayer metal system Ti / Al / Ni / Au at the drain trench using electron beam evaporation. From bottom to top, the layers are: Ti with a thickness of 20 nm, Al with a thickness of 290 nm, Ni with a thickness of 40 nm, and Au with a thickness of 50 nm, forming the drain electrode 8. Figure 3 h;
[0066] Finally, a rapid thermal annealing process was performed at 850°C in a nitrogen atmosphere for 30 seconds to create an ohmic contact between the drain electrode and the buried layer.
[0067] Step 9: Fabricate the gate electrode 9.
[0068] A 50 nm thick silicon nitride film was deposited between the source and drain electrodes on the surface of the barrier layer using PECVD deposition to form a passivation layer 5. Figure 3 As shown in i; _
[0069] Next, a gate pattern is photolithographically etched onto the silicon nitride thin film in the middle region of the passivation layer, and the exposed passivation layer is removed using reactive ion etching. Then, a Ti / Au combined gate metal is fabricated using magnetron sputtering, where the Ti thickness is 50 nm and the Au thickness is 280 nm, forming gate electrode 9. Figure 3 As shown in j;
[0070] Finally, the device is thermally annealed at 460°C for 10 minutes to form a Schottky contact between the gate electrode and the barrier layer, thus completing the fabrication of the entire device.
[0071] Example 2: The substrate was silicon carbide with a thickness of 300 μm; the nucleation layer was aluminum nitride with a thickness of 200 nm; the transition layer was aluminum gallium nitride with a thickness of 500 nm; the buffer layer was gallium nitride with a host trap doping of 1 × 10⁻⁶. 16 cm -3、 The thickness is 1000nm; the channel layer material is gallium nitride, with a thickness of 300nm; the barrier layer material is aluminum gallium nitride, with a thickness of 20nm; the passivation material is SiO2, with a thickness of 150nm; the p-type buried layer 6 uses gallium nitride with concentrated doping. Spend 1x10 17 cm -3 The transistor has a thickness of 300nm; the two layers below the source and drain electrodes are Ta / Al, and the bottom layer of the gate electrode is Ti.
[0072] Step 1, cleaning the silicon carbide substrate, such as... Figure 3 As shown in a.
[0073] The silicon carbide substrate was washed in an organic acetone solution to remove surface grease and contaminants, then rinsed with flowing deionized water, and finally dried with high-purity nitrogen.
[0074] Step 2, epitaxially grow composite buffer layer 2 on substrate 1, such as Figure 3 As shown in b.
[0075] 2.1) An aluminum nitride nucleation layer 21 of 200 nm was grown on the surface of substrate 1 using the MOCVD method at a low temperature of 600 °C.
[0076] 2.2) The temperature was raised to 1000℃, and 500 nm Al atoms were sequentially grown on the aluminum nitride nucleation layer using MOCVD. 0.75 Ga 0.25 N transition layer 22 and GaN buffer layer 23 with a thickness of 1000 nm;
[0077] 2.3) The acceptor trap concentration of the buffer layer 23 material was increased to 2 × 10⁻⁶ using ion implantation. 16 cm -3 This forms a three-layer composite buffer layer 2.
[0078] Step 3, fabricate P-type embedded layer 6, as follows Figure 3 As shown in c.
[0079] Ion implantation was used to form a 1x10⁻¹⁰ doped layer on the right side of the surface of buffer layer 23. 17 cm -3 The P-type gallium nitride region is used to form the P-type buried layer region.
[0080] Step 4, fabricate channel layer 3 and barrier layer 4, as follows: Figure 3 As shown in d.
[0081] 4.1) Using the MOCVD method, the temperature was set to 1000℃ to grow a GaN channel layer with a thickness of 300nm on the buffer layer.
[0082] 4.2) Using the same process conditions as 4.1), a 20 nm thick AlGaN barrier layer 4 is epitaxially grown on the gallium nitride channel layer 3;
[0083] Step 5, cleaning.
[0084] The specific implementation of this step is the same as step five in Example 1.
[0085] Step 6: Etch the platform to create an isolation layer, such as... Figure 3 As shown in e.
[0086] Reactive ion etching technology and equipment are used to etch the mesa. The entire AlGaN barrier layer, GaN channel layer and part of GaN buffer layer are etched away in the etching area on the right side of the barrier layer surface to form a mesa with neat edges, steep sidewalls and a depth of 150nm, so as to isolate different transistors.
[0087] Step 7, fabricate the source electrode, such as Figure 3 As shown in f.
[0088] 7.1) Use photolithography etching process to etch away the photoresist on the left side of the barrier region to expose the area where the source electrode is to be fabricated;
[0089] 7.2) A multilayer metal Ta / Al / Ni / Au layer is grown in the source electrode region by electron beam evaporation, i.e. from bottom to top: 20nm thick Ta, 120nm thick Al, 40nm thick Ni, and 50nm thick Au, forming the source electrode 7; then, rapid thermal annealing is performed in a nitrogen atmosphere at 850℃ for 30s to form an ohmic contact between the source electrode and the barrier layer.
[0090] Step 8, fabricate the drain electrode, such as Figure 3 g- Figure 3 As shown in h.
[0091] 8.1) Using photolithography etching, a drain electrode pattern 8 is etched in the region to the right of the barrier layer. Then, a drain groove with a depth reaching the buried layer 6 is etched in this region, such as... Figure 3 As shown in g;
[0092] 8.2) A multilayer metal system Ta / Al / Ni / Au, consisting of a 20 nm thick Ta, a 290 nm thick Al, a 40 nm thick Ni, and a 50 nm thick Au, is grown from bottom to top at the drain groove using electron beam evaporation to form the drain electrode 8.
[0093] 8.3) Rapid thermal annealing is performed in a nitrogen atmosphere at 850°C for 30 seconds to make the drain electrode 8 form an ohmic contact with the two-dimensional electron gas.
[0094] Step 9: Fabricate the gate electrode.
[0095] 9.1) A silicon dioxide thin film with a thickness of 150 nm is deposited between the source and drain electrodes on the surface of the barrier layer using PECVD deposition to form a passivation layer 5, as shown below. Figure 3 As shown in i;
[0096] 9.2) A gate pattern is photolithographically formed on the silicon dioxide thin film region in the middle of the passivation layer, and then the exposed passivation layer is removed by reactive ion etching.
[0097] 9.3) The gate metal was fabricated using magnetron sputtering, employing a Ti / Au combination, with 50nm Ti and 280nm Au. Figure 3 As shown in j;
[0098] 9.4) Perform thermal annealing at 460°C for 10 minutes to form a Schottky contact between the gate electrode and the barrier layer, thus completing the fabrication of the entire device.
[0099] Example 3: The substrate was sapphire with a thickness of 400 μm; the nucleation layer material was aluminum nitride with a thickness of 300 nm; the transition layer material was aluminum gallium nitride with a thickness of 1000 nm; the buffer layer material was gallium nitride with an acceptor trap doping of 1 × 10⁻⁶. 17 cm -3 The channel layer is 3000 nm thick; the barrier layer is 500 nm thick, made of gallium nitride; the passivation layer is 40 nm thick, made of aluminum gallium nitride; the passivation layer is 300 nm thick, made of SiO2; the p-type buried layer 6 is made of gallium nitride with high doping concentration. The degree is 1x10 20 cm -3 A transistor with a thickness of 1000nm, consisting of two layers of Ta / Al below the source and drain electrodes and a bottom layer of Ni at the gate electrode.
[0100] Step A, clean the sapphire substrate, such as... Figure 3 As shown in a.
[0101] The sapphire substrate is cleaned by removing oil, sweat, and other impurities from its surface using organic substances such as acetone, and then dried with nitrogen.
[0102] Step B, epitaxially grow composite buffer layer 2 on substrate 1, such as Figure 3 As shown in b.
[0103] First, an aluminum nitride nucleation layer 21 of 300 nm was grown on substrate 1 using MOCVD at a low temperature of 650 °C.
[0104] The temperature was then increased to 1100℃, and a 1000nm thick Al layer was grown using the MOCVD method. 0.75 Ga 0.25 N transition layer 22, and then a GaN buffer layer 23 with a thickness of 3000 nm is grown on the transition layer;
[0105] Finally, the acceptor trap concentration of buffer layer 23 was adjusted to 2 × 10⁻⁶ using ion implantation. 17 cm -3 .
[0106] Step C, fabricate P-type embedded layer 6, as follows Figure 3 As shown in c.
[0107] Ion implantation was used to form a 1x10⁻¹⁰ doped layer on the right side of the surface of buffer layer 23. 19cm -3 The P-type gallium nitride region is used to form a P-type buried layer.
[0108] Step D, fabricate channel layer 3 and barrier layer 4, as follows Figure 3 As shown in d.
[0109] First, a GaN channel layer 3 with a thickness of 500 nm was grown on the buffer layer using the MOCVD method at a temperature of 1000℃. Then, a 40 nm thick AlGaN barrier layer 4 was epitaxially grown on the GaN channel layer 3 using the same MOCVD method.
[0110] Step E: Cleaning.
[0111] The specific implementation of this step is the same as step five in Example 1.
[0112] Step F: Etch the mesa to create an isolation layer, such as... Figure 3 As shown in e.
[0113] The mesa is etched using RIE equipment and technology. This involves etching away the entire AlGaN barrier layer, GaN channel layer, and part of the GaN buffer layer in the etching area on the right side of the barrier layer surface. The etching depth is 150nm. The mesa should have neat edges and steep sidewalls to form electrical isolation between different transistors.
[0114] Step G: Fabricate the source electrode, such as... Figure 3 As shown in f.
[0115] First, a photolithography etching process is used to etch away the photoresist on the left side of the barrier region, exposing the area where the source electrode is to be fabricated.
[0116] Then, multilayer metal Ta / Al / Ni / Au is grown in the region where the source electrode is to be fabricated using electron beam evaporation;
[0117] Finally, rapid thermal annealing was carried out at 850℃ in a nitrogen atmosphere for 30 seconds to form ohmic contacts. The metal thicknesses used, from bottom to top, were: 20nm Ta, 120nm Al, 40nm Ni, and 50nm Au.
[0118] Step H, fabricate the drain electrode, such as Figure 3 g- Figure 3 As shown in h.
[0119] Using photolithography etching, a drain electrode pattern 8 is etched in the region to the right of the barrier layer. Then, a drain groove is etched in this region, reaching the depth of the buried layer 6. Figure 3 As shown in g;
[0120] Then, metal is filled into the drain trench, and a multilayer metal system Ta / Al / Ni / Au is grown at the drain trench using electron beam evaporation. The metal thicknesses used, from bottom to top, are: 20 nm Ta, 290 nm Al, 40 nm Ni, and 50 nm Au, as follows: Figure 3 h;
[0121] Finally, a rapid thermal annealing process was carried out in a nitrogen atmosphere at 850°C for 30 seconds to allow the drain electrode 8 to form an ohmic contact with the two-dimensional electron gas.
[0122] Step 1: Fabricate the gate electrode.
[0123] A 300 nm thick silicon dioxide film was deposited between the source and drain electrodes on the barrier layer surface using PECVD deposition to form a passivation layer 5. Figure 3 As shown in i;
[0124] Next, a gate pattern is photolithographically etched onto the silicon dioxide thin film in the middle region of the passivation layer. Then, reactive ion etching is used to remove the exposed passivation layer. Finally, the gate electrode is fabricated using magnetron sputtering. The gate metal uses a Ni / Au combination, where the Ni thickness is 50 nm and the Au thickness is 280 nm. Figure 3 As shown in j;
[0125] Finally, thermal annealing at 460℃ for 10 minutes allows the gate electrode to form a Schottky contact with the barrier layer, completing the fabrication of the entire device.
[0126] The above description is merely three specific examples of the present invention and does not constitute any limitation on the present invention. Obviously, those skilled in the art, after understanding the content and principle of the present invention, may make various modifications and changes in form and detail without departing from the principle and structure of the present invention. For example, in addition to silicon, silicon carbide, and sapphire, the substrate 1 can also be a diamond substrate; in addition to gallium nitride, the material of the buffer layer 23 can also be aluminum gallium nitride; in addition to aluminum gallium nitride, the barrier layer 4 can also be indium aluminum nitride, aluminum nitride, or indium aluminum gallium nitride; in addition to gallium nitride, the channel layer 4 can also be aluminum gallium nitride; in addition to gallium nitride, the buried layer 6 can also be aluminum gallium nitride; in addition to Ti / Al and Ta / Al, the bottom two metal layers of the source electrode 7 and drain electrode 8 can also be Mo / Al; in addition to Ti and Ni, the bottom layer of the gate electrode 9 can also be Al, Ta, TiN, or TaN. Furthermore, the thickness of each epitaxial layer only needs to meet the scope of the technical solution in the specification. However, these modifications and changes based on the concept of the present invention are still within the protection scope of the claims of the present invention.
Claims
1. A gallium nitride-based transistor having a buried drain electrode layer, comprising, from bottom to top: The substrate (1), composite buffer layer (2), channel layer (3), barrier layer (4), and passivation layer (5) are provided with a source electrode (7), a gate electrode (9), and a drain electrode (8) on the surface of the barrier layer. The gate electrode forms a Schottky contact with the barrier layer, and the source electrode and drain electrode form an ohmic contact with the barrier layer. A heterojunction is formed between the channel layer and the barrier layer, and a two-dimensional electron gas channel is formed on one side of the channel layer (3) at the heterojunction interface due to the polarization effect. The feature is that: The composite buffer layer (2) is provided with a P-type buried layer (6), which forms a PIN diode with the two-dimensional electron gas channel formed by the P-type buried layer (6), the channel layer (3) and the heterojunction interface, in order to suppress electrons leaking from the drain electrode in the off state and improve the off-state breakdown voltage. The drain electrode (8) passes through the barrier layer and the channel layer and enters the composite buffer layer to connect with the P-type buried layer (6); The barrier layer (4), channel layer (3), and composite buffer layer (2) are made of group III nitride semiconductors, namely gallium nitride, aluminum nitride, indium nitride, or a multi-component compound composed of two or more of them.
2. The transistor according to claim 1, characterized in that, The P-type buried layer (6) is made of gallium nitride or aluminum gallium nitride, with a P-type doping type and a doping concentration of 1x10⁻⁶. 16 -1x10 19 cm -3 The thickness is 50-1000nm.
3. The transistor according to claim 1, characterized in that: The substrate (1) is one of silicon carbide, sapphire, or diamond.
4. The transistor according to claim 1, characterized in that, The composite buffer layer (2) includes a nucleation layer (21), a transition layer (22) and a buffer layer (23) from bottom to top, and the P-type buried layer (6) is disposed in the buffer layer (23).
5. The transistor according to claim 4, characterized in that: The nucleation layer (21) is made of aluminum nitride and has a thickness of 100-300 nm; The transition layer (22) is made of graded aluminum gallium nitride, with the aluminum composition gradually changing from 0.75 to 0.15 and a thickness of 200-1000 nm. The buffer layer (23) is made of gallium nitride or aluminum gallium nitride, and the main trap doping is 1×10⁻⁶. 15 cm -3 -1×10 17 cm -3 The thickness is 100-3000nm.
6. The transistor according to claim 1, characterized in that: The channel layer (3) is made of gallium nitride or indium gallium nitride, with a thickness of 50nm-500nm; The barrier layer (4) is one of aluminum gallium nitride, indium aluminum nitride, aluminum nitride, and indium aluminum gallium nitride, with a thickness of 2-40 nm; The passivation layer (5) is made of SiN or SiO2.
7. The transistor according to claim 1, characterized in that: The first layer below the gate electrode (9) is any one of Ti, Ni, Al, Ta, TiN, and TaN; The bottom two layers of the source electrode (7) and drain electrode (8) are Ti / Al, or Ta / Al, or Mo / Al.
8. A method for fabricating a gallium nitride-based transistor with a buried drain electrode layer, characterized in that, Includes the following steps: S1: A composite buffer layer is formed by sequentially growing a group III nitride nucleation layer, a transition layer, and a buffer layer on the substrate using metal-organic chemical vapor deposition (MOCVD). S2: A P-type buried layer is fabricated on the surface of the buffer layer using ion implantation. The doping concentration of this buried layer is 1x10⁻⁶. 16 -1x10 20 cm-3, with a thickness of 50-1000 nm; S3: Channel layer and barrier layer are epitaxially grown on buffer layer using metal-organic chemical vapor deposition (MOCVD). S4: Reactive ion etching (RIE) is used for etching isolation. The barrier layer, channel layer and part of the buffer layer are etched away in the right region of the barrier layer. The etching depth is 150nm. The mesa should have neat edges and steep sidewalls. S5: Prepare a source electrode on the surface of the barrier layer and perform high-temperature thermal annealing to form an ohmic contact with the two-dimensional electron gas; S6: Photolithography is used to form the drain electrode region on the right side of the barrier layer to form a drain groove. The depth of the drain groove reaches the buried layer. Metal is filled in the drain groove. A multilayer metal system is grown on the heterojunction by electron beam evaporation to prepare the drain electrode. High-temperature annealing is then performed to form an ohmic contact with the two-dimensional electron gas. S7: A nitride film is deposited between the source and drain electrodes on the surface of the barrier layer using PECVD deposition to form a passivation layer; S8: The gate pattern is photolithographically patterned on the passivation layer, and then the exposed passivation layer is removed by reactive ion etching. Finally, the gate metal is prepared to form a Schottky contact with the barrier layer, thus completing the device fabrication.
9. The method according to claim 8, characterized in that, In step S1, metal-organic chemical vapor deposition (MOCVD) is used. First, a nucleation layer is grown using MOCVD at a low temperature of 500-650℃. Then, the temperature is increased to 1000-1100℃ to grow a transition layer and a buffer layer using MOCVD. Finally, acceptor doping of the buffer layer material is performed using ion implantation.
Citation Information
Patent Citations
Single-particle-radiation-resistant reinforced enhanced GaN power device
CN114220794A
Gallium nitride high-electron mobility transistors with p-type layers and process for making the same
US20170373176A1