Polyimide resin, polyimide film and preparation method thereof, copper clad plate
Polyimide resin is formed through the condensation of specific diamines and tetracarboxylic dianhydride, which solves the problem of low haze of polyimide films, achieves high haze and improved light transmittance, simplifies the process and reduces Reduce costs and avoid filler-related risks.
Patent Information
- Application Number
- CN202210700216.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-06-20
AI Technical Summary
The haze of existing polyimide films is low, which makes it difficult to meet the needs of optoelectronic applications. Fillers are often needed to increase the haze, resulting in complex processes and high costs, as well as the risk of filler removal.
Polyimide resin is formed by condensing specific diamine and tetracarboxylic dianhydride, introducing non-planar structure and hydrophobic side groups, increasing the gap and free volume between molecular chains, allowing the solvent and moisture to be quickly diffused and removed during the film forming process to form High haze light control structure avoids filler dispersion.
It achieves high haze and good light transmittance, reduces the production and application costs of the polyimide film, improves safety, and avoids the risk of filler decomposition or precipitation.
Smart Images

Figure CN114854012B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polyimide films, and in particular to a polyimide resin, a polyimide film and a preparation method thereof, and a copper clad plate. Background Art
[0002] Light diffusion is a process that uses chemical or physical means to utilize the physical phenomena of refraction, reflection and scattering when light encounters two media with different refractive indices during its travel, thereby changing the path of light and achieving full dispersion of incident light to produce an optical diffusion effect. The current method for preparing light diffusion materials is to add light diffusers to resin materials such as polycarbonate (PC), polymethyl methacrylate and polystyrene to achieve the purpose of light scattering.
[0003] Polyimide (PI) has excellent comprehensive properties, especially high and low temperature resistance, dimensional stability, mechanical properties, radiation resistance, etc., because its molecules contain stable aromatic heterocyclic structures, and is widely used in electronics, electrical appliances, aerospace and other fields. With the rapid development of the economy and the continuous improvement of people's living standards, people have higher and higher requirements for the comprehensive performance of materials. In addition to its own unique excellent properties, high-haze polyimide film also has the characteristics of high haze and high light transmittance, so it can be widely used in optics, electronics and other fields with high requirements for haze.
[0004] The Chinese patent application with publication number CN110372901A provides a high haze polyimide film and a preparation method thereof, wherein PS (polystyrene) microspheres are dispersed in a polyimide glue solution, and the PS microspheres are removed in a subsequent heat treatment, leaving a hollow spherical structure. The PS microspheres have a small particle size, and are easily agglomerated during the dispersion process, resulting in uneven dispersion, and the dispersion is difficult. The subsequent high-temperature removal of the PS microspheres is likely to cause problems such as blistering of the polyimide film.
[0005] At present, the haze value of general polyimide films is still relatively low, which is difficult to meet the use requirements in the optoelectronic application field. Fillers are usually needed to improve the haze of polyimide films, which makes the production process of polyimide ink more complicated and costly. At the same time, there is a high risk of filler removal. Summary of the invention
[0006] The main purpose of the present invention is to provide a polyimide resin, a polyimide film and a preparation method thereof, and a copper clad plate, so as to solve the problem of low haze of the polyimide film in the prior art.
[0007] In order to achieve the above object, according to one aspect of the present invention, a polyimide resin is provided, wherein the polyimide resin has a structure shown in the following structural formula I:
[0008]
[0009] Wherein, n≥20, Ar includes any one or more of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride residue, 4,4'-biphenyl ether dianhydride residue, bisphenol A diether dianhydride residue, 4,4'-(hexafluoroisopropyl) diphthalic acid dianhydride residue and a combination of pyromellitic acid dianhydride residue; R includes any one or two of 4,4'-diamino-2,2'-dimethylbiphenyl residue and 2,2'-bis(trifluoromethyl)diaminobiphenyl residue.
[0010] Furthermore, the molar content of the residues of pyromellitic dianhydride accounts for 1% to 50% of the molar amount of Ar, preferably 20% to 30%; preferably, R also includes the residues of modified diamine compounds, and the modified diamine compounds are selected from any one or more of 4,4'-diaminodiphenyl ether, p-phenylenediamine, and bisphenol A. Further preferably, the molar amount of the residues of the modified diamine compounds accounts for 0.1% to 20% of the molar amount of R, and further preferably 5% to 10%.
[0011] According to another aspect of the present invention, a polyimide film is provided. The polyimide film contains any one of the above-mentioned polyimide resins.
[0012] Furthermore, the imidization degree of the polyimide film is 97% to 99%, and preferably the water content of the polyimide film is 0.1% to 0.2%.
[0013] According to another aspect of the present invention, there is provided a method for preparing a polyimide film, the method comprising:
[0014] Step S1, in an inert gas environment, mixing a dianhydride compound, a diamine compound and a solvent to obtain a precursor solution of a polyimide, wherein the dianhydride compound includes any one or more of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 4,4'-biphenyl ether dianhydride, bisphenol A diether dianhydride, and 4,4'-(hexafluoroisopropyl) diphthalic acid dianhydride in combination with pyromellitic acid dianhydride, and the diamine compound includes any one or two of 4,4'-diamino-2,2'-dimethylbiphenyl and 2,2'-bis(trifluoromethyl)diaminobiphenyl;
[0015] Step S2, coating the polyimide precursor solution on the carrier, drying and imidizing, to obtain a polyimide film attached to the carrier.
[0016] Further, step S1 includes:
[0017] Step S11, dissolving a diamine compound in a solvent to obtain a diamine compound solution, preferably the percentage of the diamine compound in the diamine compound solution is 5wt% to 13wt%, the diamine compound further comprises a modified diamine compound, the modified diamine compound is selected from any one or more of 4,4'-diaminodiphenyl ether, p-phenylenediamine, and bisphenol A, preferably the molar amount of the modified diamine compound accounts for 0.1% to 20% of the molar amount of the diamine compound, more preferably 5% to 10%;
[0018] Step S12, adding the dianhydride compound to the diamine compound solution in multiple times, the molar ratio of the dianhydride compound to the diamine compound is 0.9:1 to 1.1:1, reacting for 4 to 48 hours, the reaction temperature is 0 to 50°C, to obtain a precursor solution of a polyimide resin; preferably, the dianhydride compound is added three times, and the amount added three times is 50% to 70%, 20% to 40%, and 5% to 20% of the total weight, respectively, and it is further preferred that the molar content of pyromellitic dianhydride accounts for 1% to 50% of the molar amount of the dianhydride compound, preferably 20% to 30%.
[0019] Furthermore, the solvent is selected from any one or more of N,N-dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone and m-cresol.
[0020] Further, step S2 includes:
[0021] Step S21, coating a polyimide precursor solution on a carrier to obtain a wet film layer, and drying the wet film layer in an environment of 80-150° C. to obtain a polyimide resin precursor dry film layer, wherein the polyimide resin precursor dry film layer preferably has a solvent content of 25wt%-35wt%;
[0022] Step S22, placing the precursor dry film layer of the polyimide resin in an environment of 350-400°C for thermal curing to obtain a polyimide film attached to the carrier. Preferably, the thermal curing time is 5-15 minutes, and more preferably, the thickness of the polyimide film attached to the carrier is 12-50 μm.
[0023] Furthermore, the carrier is a glass plate, copper foil or aluminum foil.
[0024] Furthermore, the method further comprises step S3, separating the polyimide film layer from the carrier; preferably, a boiling method is used to separate the polyimide film from the carrier.
[0025] According to another aspect of the present invention, a flexible copper clad laminate is provided. The flexible copper clad laminate contains any one of the above-mentioned polyimide resins.
[0026] The technical scheme of the present invention is applied, the above-mentioned polyimide resin is formed by condensation of specific diamine and tetracarboxylic dianhydride, the polymer chain segment is structurally designed, a non-planar structure and a hydrophobic side group are introduced, the gap and free volume between the molecular chains are increased, so that the film formed by the polyimide resin can be quickly diffused / volatized and removed from the inside of the polyimide film during the molding process of the residual solvent and the water generated by the reaction, and the polymer chain segment is quickly accumulated to form a high-fog light-regulating structure; at the same time, due to the fast curing speed of the polyimide resin, the channels and concave-convex surfaces generated by the diffusion process of the solvent and water can be partially retained, and the density of the polymer chain segments accumulated in the channel is small, forming an uneven optical structure, thereby further improving the haze of the film formed by the polyimide resin. The polyimide film made of the polyimide resin provided by the present application does not need to add fillers, that is, it has a higher haze and better light transmittance, that is, it does not need filler dispersion operation, and there is no risk of filler decomposition or precipitation. It can be prepared by a traditional casting method, which can effectively reduce the production and application costs of the polyimide film and improve the safety of use. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0028] Figure 1 Optical photographs of polyimide films according to Example 1, Example 2 and Comparative Example 1 of the present invention are shown;
[0029] Figure 2 The UV-visible spectra of the polyimide films according to Example 1 and Example 2 of the present invention are shown. DETAILED DESCRIPTION
[0030] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0031] According to the analysis of the background technology of the present application, the prior art has the problem that the haze of the polyimide film is relatively low. In order to solve this problem, the present application provides a polyimide film, a preparation method thereof and a copper clad plate having the same.
[0032] In a typical embodiment of the present application, a polyimide resin is provided, and the polyimide resin has a structure shown in the following structural formula I:
[0033]
[0034] Wherein, n is ..., Ar includes any one or more of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride (BPDA) residue, 4,4'-biphenyl ether dianhydride (ODPA) residue, bisphenol A type diether dianhydride residue, 4,4'-(hexafluoroisopropyl) diphthalic acid dianhydride (6FDA) residue and a combination of pyromellitic acid dianhydride (PMDA) residue; R includes any one or two of 4,4'-diamino-2,2'-dimethylbiphenyl (M-Tolidine) residue and 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFMB) residue.
[0035] The polyimide resin of the present application is formed by condensation of specific diamine and tetracarboxylic dianhydride, and the polymer segment is structurally designed, a non-planar structure and a hydrophobic side group are introduced, and the gap and free volume between the molecular chains are increased, so that during the molding process of the film formed by the polyimide resin, the residual solvent and the moisture generated by the reaction can be quickly diffused / volatilized from the inside of the polyimide film, and the polymer segment is quickly accumulated to form a high-fog light-regulating structure; at the same time, due to the fast curing speed of the polyimide resin, the channels and concave-convex surfaces generated by the diffusion process of the solvent and moisture can be partially retained, and the density of the polymer segment accumulated in the channel is relatively small, forming an uneven optical structure, thereby further improving the haze of the film formed by this type of polyimide resin. The polyimide film made of the polyimide resin provided by the present application does not need to add fillers, that is, it has a higher haze and better light transmittance, that is, it does not need filler dispersion operation, and there is no risk of filler decomposition or precipitation. It can be prepared by a traditional casting method, which can effectively reduce the production and application costs of polyimide films and improve the safety of use.
[0036] In some embodiments of the present application, the molar content of the residues of isomellitic dianhydride in the above-mentioned polyimide resin is 1% to 50% of the molar amount of Ar, such as 5%, 10%, 20%, 25%, 30%, 40%, preferably 20% to 30%. This composition is beneficial to improving the comprehensive performance of polyimide.
[0037] In some embodiments of the present application, R in the above-mentioned polyimide resin also includes the residue of a modified diamine compound, and the modified diamine compound is selected from any one or more of 4,4'-diaminodiphenyl ether (ODA), p-phenylenediamine (PDA), and bisphenol A. Preferably, the molar amount of the residue of the modified diamine compound accounts for 0.1% to 20% of the molar amount of R, and further preferably 5% to 10%, such as 1%, 5%, 10%, 15%, and 18%. The resin containing the above-mentioned modified diamine compound can improve the peel strength, and can also adjust the thermal expansion coefficient and improve the dimensional stability.
[0038] In another typical embodiment of the present application, a polyimide film is provided. The polyimide film contains any one of the above-mentioned polyimide resins.
[0039] The polyimide film provided in the present application contains the above-mentioned polyimide resin and does not require the addition of fillers, that is, it has a higher haze and better light transmittance, that is, it does not require filler dispersion operations, and there is no risk of filler decomposition or precipitation. It can be prepared by a traditional casting method, which can effectively reduce the production and application costs of the polyimide film and improve the safety of use.
[0040] In some preferred embodiments of the present application, the imidization degree of the above-mentioned polyimide film is 97% to 99%, and the unreacted carboxyl groups and amino groups can destroy the uniformity of the polyimide, thereby increasing the haze; preferably, the water content of the polyimide film is 0.1% to 0.2%, for example, 0.15%. The water content of the polyimide film is controlled within the above-mentioned range so that the polyimide film contains an appropriate amount of unreacted amino and carboxyl groups, which changes the uniformity of the film, thereby further improving the haze of the polyimide film.
[0041] In another typical embodiment of the present application, a method for preparing a polyimide film is provided, which comprises: step S1, in an inert gas environment, mixing a dianhydride compound, a diamine compound and a solvent to obtain a precursor solution of a polyimide, wherein the dianhydride compound comprises any one or more of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 4,4'-biphenyl ether dianhydride, bisphenol A type diether dianhydride, and 4,4'-(hexafluoroisopropyl) diphthalic acid dianhydride in combination with isophthalic acid dianhydride, and the diamine compound comprises any one or two of 4,4'-diamino-2,2'-dimethylbiphenyl and 2,2'-bis(trifluoromethyl)diaminobiphenyl; step S2, coating the polyimide precursor solution on a carrier, drying, and imidizing to obtain a polyimide film attached to the carrier.
[0042] The polyimide resin formed by the condensation of specific diamine and tetracarboxylic dianhydride is prepared by the above-mentioned preparation method, the structure of the polymer chain segment is designed, a non-planar structure and a hydrophobic side group are introduced, the gap and free volume between the molecular chains are increased, and during the molding process of the polyimide film, the residual solvent and the moisture generated by the reaction can be quickly diffused / volatilized and removed from the inside of the polyimide film, and the polymer chain segments are quickly accumulated to form a light-regulating structure with high haze; at the same time, due to the fast curing speed of the polyimide resin, the channels and concave-convex surfaces generated by the diffusion process of the solvent and moisture can be partially retained, the density of the polymer chain segments accumulated in the channels is relatively small, and an uneven optical structure is formed, thereby further improving the haze of the film formed by this type of polyimide resin.
[0043] The present application adopts a mature casting method to prepare a polyimide film with high haze, which has a short process time and is easy to operate. In addition, the polyimide film made of the polyimide resin provided by the present application does not require the addition of fillers, that is, it has a higher haze and better light transmittance, which can effectively reduce the production and application costs of the polyimide film and improve the safety of use.
[0044] The above-mentioned step S1, mixing the dianhydride compound, the diamine compound and the solvent, can be carried out according to the existing technology, such as selecting to be carried out under a nitrogen environment. In some embodiments of the present application, step S1 includes: step S11, dissolving the diamine compound in the solvent to obtain a diamine compound solution, preferably the percentage of the diamine compound in the diamine compound solution is 5wt% to 13wt%, the diamine compound also includes a modified diamine compound, the modified diamine compound is selected from any one or more of 4,4'-diaminodiphenyl ether, p-phenylenediamine, and bisphenol A, preferably the molar amount of the modified diamine compound accounts for 0.1% to 20% of the molar amount of the diamine compound, and more preferably 5% to 10%, such as 1%, 5%, 10%, 15%, 18%; step S12, adding the dianhydride compound to the diamine compound solution in multiple times In the solution, the molar ratio of the dianhydride compound to the diamine compound is 0.9:1-1.1:1, preferably 0.95:1-1.05:1, and the reaction is carried out for 4-48 hours at a reaction temperature of 0-50°C to obtain a precursor solution of a polyimide resin; preferably, the dianhydride compound is added three times, and the amount added three times is 50%-70%, 20%-40%, and 5%-20% of the total weight, respectively. For example, the amount added three times is 60%, 30%, and 10%, or 55%, 38%, and 7%, respectively. Adding the dianhydride compound in multiple times is beneficial to controlling the reaction speed of the dianhydride and the diamine compound solution, preventing the polymerization reaction from being too fast, and preventing the reaction system temperature from being too high due to the too fast reaction speed. When adding in multiple batches, the dianhydride compound added in each batch can be one dianhydride or a mixture of multiple dianhydrides, which is not limited here. It is further preferred that the molar content of pyromellitic dianhydride accounts for 1% to 50% of the molar amount of the dianhydride compound, preferably 20% to 30%, such as 5%, 10%, 20%, 30%, 40%.
[0045] The above-mentioned solvent can be selected from the prior art. In some embodiments of the present application, the solvent is selected from any one or more of N,N-dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone (NMP), and m-cresol. These solvents have strong polarity and strong solubility for dianhydride and diamine, which is beneficial to the acylation reaction. They also have small molecular volume, which is convenient for subsequent separation.
[0046] The specific operation method of the above-mentioned step S2 can be carried out according to the existing technology. In some embodiments of the present application, step S2 also includes: step S21, coating the precursor solution of polyimide on the carrier to obtain a wet film layer, and drying the wet film layer in an environment of 80 to 150°C to obtain a precursor dry film layer of polyimide resin, preferably, the solvent content of the precursor dry film layer of polyimide resin is 25 to 35wt%; step S22, placing the precursor dry film layer of polyimide resin in an environment of 350 to 400°C for thermal curing to obtain a polyimide film attached to the carrier, preferably, the thermal curing time is 5 to 15 minutes, and further preferably, the thickness of the polyimide film attached to the carrier is 12 to 50μm. Since the polyimide resin of the present application is formed by condensation of the above-mentioned specific diamine and tetracarboxylic dianhydride, the gaps and free volumes between the molecular chains are large, the residual solvent in the molding process and the moisture generated in the imidization process are easy to remove, and the imidization of the resin can be completed through the above-mentioned thermal curing process. Compared with the traditional polyimide thermal curing which requires gradual heating in a vacuum oven or a nitrogen-filled oven for imidization, the energy consumption is greatly reduced and the preparation efficiency is significantly improved.
[0047] The carrier can be selected from the prior art, such as a glass plate. If the polyimide film is used to make a copper clad laminate, the polyimide precursor solution can also be coated on a copper foil, and a flexible copper clad laminate can be obtained after drying and imidization.
[0048] In some embodiments of the present application, the method for preparing the polyimide film further comprises step S3, separating the polyimide film layer from the carrier; preferably, a boiling method is used to separate the polyimide film from the carrier.
[0049] In another typical embodiment of the present application, a flexible copper clad laminate is provided. The flexible copper clad laminate contains any one of the above-mentioned polyimide resins.
[0050] The polyimide resin of the present application is formed by condensation of specific diamines and tetracarboxylic dianhydride. The polymer chain segments are structurally designed, non-planar structures and hydrophobic side groups are introduced, and the gaps and free volumes between the molecular chains are increased, so that during the molding process of the polyimide film, the residual solvent and the moisture generated by the reaction can be quickly diffused / volatilized and removed from the inside of the polyimide film, and the polymer chain segments are quickly accumulated to form a light-regulating structure with high haze; at the same time, due to the fast curing speed of the polyimide resin, the channels and concave-convex surfaces generated by the diffusion process of the solvent and moisture can be partially retained, and the density of the polymer chain segments accumulated in the channels is relatively small, forming an uneven optical structure, thereby further improving the haze of the film formed by this type of polyimide resin.
[0051] The polyimide resin provided in the present application is applied to copper-clad laminates, and bubbles are not easily generated during high-temperature treatment, the film has good dimensional stability, and has a certain shielding effect on the surface texture of the copper foil. The prepared polyimide film does not need to add fillers, that is, it has a high haze and good light transmittance, which can effectively reduce the production and application costs of the polyimide film and improve the safety of use.
[0052] The achievable beneficial effects of the present application will be further illustrated below in conjunction with embodiments and comparative examples.
[0053] Example 1
[0054] 1) Under nitrogen atmosphere, 0.06 mol of TFMB was dissolved in 200 g of NMP, and after being stirred evenly on a stirring table, 0.042 mol of BPDA was added thereto, and stirred for 1 hour; then 0.018 mol of PMDA was added, and stirred at a temperature of 20 to 30° C. for 12 hours to obtain a light yellow polyamic acid solution, i.e., a precursor solution of polyimide;
[0055] 2) Spinning the polyimide precursor solution on a glass plate with a spin coater at a speed of 500-800 rpm, and then removing the solvent at 125° C. for 25 min to obtain a precursor dry film layer of polyimide resin, wherein the solvent content in the precursor dry film layer is 35±2%;
[0056] 3) directly placing the glass plate coated with the precursor dry film layer of the polyimide resin into an oven at 370° C. for thermal curing for a total time of 7 minutes, wherein the precursor dry film layer of the polyimide resin is cured to form a polyimide film layer with a film thickness of 25±2 μm;
[0057] 4) The polyimide film attached to the glass plate is cooled to room temperature, and the glass plate is placed in water to peel off the film, thereby obtaining a polyimide film with high haze.
[0058] The weight loss ratio in different temperature ranges was tested by a thermogravimetric analyzer (TGA) to obtain the water content of the polyimide film, and then the imidization degree was calculated based on the water content and the molecular weight ratio of the imide group in the structural formula.
[0059] In this embodiment, the molecular weight of a polyamic acid (PAA) residue is 591.6, the molecular weight of a polyimide (PI) residue is 555.6, and PAA is completely imidized to PI, and its dehydration specific gravity is (591.6-555.6) / 591.6=6.08%. The thermal weight loss curve of the sample of this embodiment shows that the subsequent imidization can still dehydrate 0.15%, that is, its imidization degree is 1-0.15 / 6.08=97.5%.
[0060] The obtained polyimide film is characterized by transmission spectrum using an ultraviolet spectrophotometer. In the visible light range, the average haze can reach 93%, and the average transmittance can reach 50%.
[0061] Example 2
[0062] 1) Under nitrogen atmosphere, 0.06 mol of M-Tolidine was dissolved in 173 g of NMP, and after being stirred evenly on a stirring table, 0.042 mol of BPDA was added thereto, and stirred for 1 hour; then 0.018 mol of PMDA was added, and stirred at 20-30° C. for 12 hours to obtain a light yellow polyamic acid solution, i.e., a precursor solution of polyimide;
[0063] 2) Spin coating the polyimide precursor solution on a glass plate using a spin coater at a rotation speed of 500-800 rpm, and then removing the solvent at 125° C. for 25 minutes to obtain a precursor dry film layer of polyimide resin, wherein the solvent content in the precursor dry film layer is 35±2%;
[0064] 3) directly placing the glass plate coated with the precursor dry film layer of the polyimide resin into an oven at 370° C. for thermal curing for a total time of 7 minutes, wherein the precursor dry film layer of the polyimide resin is cured to form a polyimide film layer with a film thickness of 25±2 μm;
[0065] 4) The polyimide film attached to the glass plate is cooled to room temperature, and the glass plate is placed in water to peel off the film, thereby obtaining a polyimide film with high haze.
[0066] The prepared polyimide composite film is characterized by transmission spectrum, and the average haze in the visible light range can reach 70%, and the average transmittance can reach 65%.
[0067] like Figure 1 As shown in the optical photographs, the polyimide films of Example 1 (a in the figure) and Example 2 (b in the figure) have higher haze, which is significantly better than ordinary polyimide films.
[0068] Figure 2 The UV-visible light spectra of the polyimide films of Example 1 and Example 2 show that the average haze in the visible light wavelength range is as high as over 70%.
[0069] Example 3
[0070] 1) Under nitrogen atmosphere, 0.06 mol of TFMB was dissolved in 200 g of NMP, and after being stirred evenly on a stirring table, 0.042 mol of BPDA was added thereto, and stirred for 1 hour; then 0.018 mol of PMDA was added, and stirred at 20-30° C. for 12 hours to obtain a light yellow polyamic acid solution, i.e., a precursor solution of polyimide;
[0071] 2) The polyimide precursor solution is uniformly coated on a 12 μm thick electrolytic copper foil, and the copper foil coated with the polyimide precursor solution is dried at 125° C. for 25 min to obtain a precursor dry film layer of the polyimide resin, wherein the solvent content in the precursor dry film layer is 35±2%;
[0072] 3) The copper foil coated with the precursor dry film layer of the polyimide resin is directly placed in an oven at 370° C. for thermal curing for a total time of 7 minutes. The precursor dry film layer of the polyimide resin is cured to form a polyimide film layer, thereby obtaining a single-sided adhesive-free flexible copper clad laminate product.
[0073] The single-sided adhesive-free flexible copper-clad laminate consists of a layer of electrolytic copper and a layer of polyimide film. In an embodiment, the polyimide film has a thickness of 25±2 um, a tensile strength of more than 150 MPa, and a thermal expansion coefficient of 25-35 ppm / K.
[0074] Example 4
[0075] 1) Under nitrogen atmosphere, 0.06 mol of M-Tolidine was dissolved in 200 g of NMP, and after being stirred evenly on a stirring table, 0.042 mol of BPDA was added thereto, and stirred for 1 hour; then 0.018 mol of PMDA was added, and stirred at 20-30° C. for 12 hours to obtain a light yellow polyamic acid solution, i.e., a polyimide precursor solution;
[0076] 2) The polyimide precursor solution is uniformly coated on a 12 μm thick electrolytic copper foil, and the copper foil coated with the polyimide precursor solution is dried at 125° C. for 25 min to obtain a polyimide resin precursor dry film layer.
[0077] 3) The copper foil coated with the precursor dry film layer of the polyimide resin is directly placed in an oven at 370° C. for thermal curing; the total time is 7 minutes; the precursor dry film layer of the polyimide resin is cured to form a polyimide film layer; and a single-sided adhesive-free flexible copper clad laminate product is obtained.
[0078] Example 5
[0079] The difference from Example 1 is that the added amounts of BPDA and PMDA are each 0.03 mol.
[0080] Example 6
[0081] The difference from Example 1 is that the added amounts of BPDA and PMDA are 0.059 mol and 0.001 mol respectively.
[0082] Example 7
[0083] The difference from Example 1 is that 0.048 mol of TFMB and 0.012 mol of 4,4'-diaminodiphenyl ether are used instead of 0.06 mol of TFMB.
[0084] Example 8
[0085] The difference from Example 1 is that 0.054 mol of TFMB and 0.006 mol of 4,4'-diaminodiphenyl ether are used instead of 0.06 mol of TFMB.
[0086] Example 9
[0087] The difference from Example 1 is that 0.054 mol of TFMB and 0.006 mol of p-phenylenediamine are used instead of 0.06 mol of TFMB.
[0088] Example 10
[0089] The difference from Example 1 is that the added amounts of BPDA and PMDA are 0.048 mol and 0.012 mol respectively.
[0090] Embodiment 11
[0091] The difference from Example 1 is that the amount of solvent NMP added is 385 g, the time for removing the solvent is 15 min, and the solvent content in the precursor dry film layer is 43±2%.
[0092] Example 12
[0093] The difference from Example 1 is that the amount of solvent NMP added is 150 g, the time for removing the solvent is 35 min, and the solvent content in the precursor dry film layer is 28±2%.
[0094] Embodiment 13
[0095] The difference from Example 1 is that the added amounts of BPDA and PMDA are 0.040 mol and 0.017 mol respectively.
[0096] Embodiment 14
[0097] The difference from Example 1 is that the added amounts of BPDA and PMDA are 0.044 mol and 0.019 mol respectively.
[0098] Embodiment 15
[0099] The difference from Example 1 is that in step 1), the stirring time after adding BPDA and PMDA is 4 hours.
[0100] Example 16
[0101] The difference from Example 1 is that in step 1), the stirring time after adding BPDA and PMDA is 48 hours.
[0102] Embodiment 17
[0103] The difference from Example 1 is that in step 1), the reaction temperature is 0-5°C.
[0104] Embodiment 18
[0105] The difference from Example 1 is that in step 1), the reaction temperature is 40-50°C.
[0106] Embodiment 19
[0107] The difference from Example 1 is that in step 2), the temperature for removing the solvent is 80°C.
[0108] Embodiment 20
[0109] The difference from Example 1 is that in step 3), the temperature for heat curing in the oven is 350°C.
[0110] Embodiment 21
[0111] The difference from Example 1 is that in step 3), the temperature for thermal curing in the oven is 400°C.
[0112] Embodiment 22
[0113] The difference from Example 1 is that the added amounts of BPDA and PMDA are 0.036 mol and 0.024 mol respectively.
[0114] Comparative Example 1
[0115] The difference from Example 1 is that the added amounts of BPDA and PMDA are 0.006 mol and 0.054 mol respectively.
[0116] The optical photograph of the polyimide film (c in the figure) prepared in this comparative example is as follows Figure 1 As shown, the haze is obviously inferior to that of the polyimide film of Example.
[0117] The imidization degree, water content, average haze in the visible light region, and average transmittance in the visible light region of the above embodiments and comparative examples are shown in Table 1 below. The overall performance of polyimide is comprehensively determined by the two indicators of average haze in the visible light region and average transmittance in the visible light region.
[0118] Table 1
[0119]
[0120]
[0121] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: the polyimide resin of the present application is formed by condensation of a specific diamine and tetracarboxylic dianhydride, the polymer chain segment is structurally designed, a non-planar structure and a hydrophobic side group are introduced, the gap and free volume between the molecular chains are increased, so that during the molding process of the polyimide film, the residual solvent and the water generated by the reaction can be quickly diffused / volatilized from the inside of the polyimide film, and the polymer chain segments are quickly accumulated to form a high-fog light-regulating structure; at the same time, due to the fast curing speed of the polyimide resin, the channels and concave-convex surfaces generated by the diffusion process of the solvent and water can be partially retained, and the density of the polymer chain segments accumulated in the channel is small, forming an uneven optical structure, thereby further improving the haze of the film formed by the polyimide resin. The polyimide film made of the polyimide resin provided by the present application does not need to add fillers, that is, it has a higher haze and better light transmittance, that is, it does not require filler dispersion operations, and there is no risk of filler decomposition or precipitation. It can be prepared by a traditional casting method, which can effectively reduce the production and application costs of the polyimide film and improve the safety of use.
[0122] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A polyimide film, characterized in that: The polyimide film contains a polyimide resin having a structure shown in the following structural formula I: Structural Formula I Wherein, n≥20, Ar comprises any one or more of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride residue, 4,4'-biphenyl ether dianhydride residue, bisphenol A diether dianhydride residue, 4,4'-(hexafluoroisopropyl) diphthalic acid dianhydride residue and pyromellitic acid dianhydride residue, and the molar content of the pyromellitic acid dianhydride residue accounts for 20% to 30% of the molar amount of Ar; R includes any one or both of a 4,4'-diamino-2,2'-dimethylbiphenyl residue and a 2,2'-bis(trifluoromethyl)diaminobiphenyl residue; The imidization degree of the polyimide film is 97% to 99%, and the water content is 0.1% to 0.2%.
2. The polyimide film according to claim 1, characterized in that The R also includes a residue of a modified diamine compound, and the modified diamine compound is selected from any one or more of 4,4'-diaminodiphenyl ether and p-phenylenediamine.
3. The polyimide film according to claim 2, characterized in that: The molar amount of the residue of the modified diamine compound accounts for 0.1% to 20% of the molar amount of R.
4. The polyimide film according to claim 2, characterized in that: The molar amount of the residue of the modified diamine compound accounts for 5% to 10% of the molar amount of R.
5. A method for preparing a polyimide film according to any one of claims 1 to 4, characterized in that: include: Step S1, in an inert gas environment, mixing a dianhydride compound, a diamine compound and a solvent to obtain a precursor solution of a polyimide, wherein the dianhydride compound includes any one or more of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 4,4'-biphenyl ether dianhydride, bisphenol A diether dianhydride, and 4,4'-(hexafluoroisopropyl) diphthalic acid dianhydride in combination with pyromellitic acid dianhydride, and the molar content of the pyromellitic acid dianhydride accounts for 20% to 30% of the molar amount of the dianhydride compound, and the diamine compound includes any one or two of 4,4'-diamino-2,2'-dimethylbiphenyl and 2,2'-bis(trifluoromethyl)diaminobiphenyl; Step S2, coating the polyimide precursor solution on a carrier, drying, and imidizing to obtain a polyimide film attached to the carrier.
6. The preparation method according to claim 5, characterized in that: The step S1 comprises: Step S11, dissolving the diamine compound in a solvent to obtain a diamine compound solution, wherein the diamine compound further comprises a modified diamine compound, and the modified diamine compound is selected from any one or more of 4,4'-diaminodiphenyl ether, p-phenylenediamine, and bisphenol A; Step S12, adding the dianhydride compound to the diamine compound solution in multiple times, wherein the molar ratio of the dianhydride compound to the diamine compound is 0.9:1-1.1:1, reacting for 4-48 hours at a reaction temperature of 0-50° C., to obtain a precursor solution of a polyimide resin.
7. The preparation method according to claim 6, characterized in that: The percentage of the diamine compound in the diamine compound solution is 5 wt % to 13 wt %.
8. The preparation method according to claim 6, characterized in that: The molar amount of the modified diamine compound accounts for 0.1% to 20% of the molar amount of the diamine compound.
9. The preparation method according to claim 6, characterized in that: The molar amount of the modified diamine compound accounts for 5% to 10% of the molar amount of the diamine compound.
10. The preparation method according to claim 6, characterized in that: The dianhydride compound is added in three times, and the addition amounts of the three times are 50%-70%, 20%-40%, and 5%-20% of the total weight respectively.
11. The preparation method according to any one of claims 5 to 10, characterized in that: The solvent is selected from any one or more of N,N-dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone and m-cresol.
12. The preparation method according to claim 5, characterized in that: The step S2 comprises: Step S21, coating the polyimide precursor solution on a carrier to obtain a wet film layer, and drying the wet film layer in an environment of 80-150° C. to obtain a polyimide resin precursor dry film layer; Step S22 , placing the precursor dry film layer of the polyimide resin in an environment of 350-400° C. for thermal curing to obtain the polyimide film attached to the carrier.
13. The preparation method according to claim 12, characterized in that: The solvent content of the precursor dry film layer of the polyimide resin is 25wt%-35wt%.
14. The preparation method according to claim 12, characterized in that: The thermal curing time is 5 to 15 minutes.
15. The preparation method according to claim 12, characterized in that: The thickness of the polyimide film attached to the carrier is 12-50 μm.
16. The preparation method according to claim 5, characterized in that: The carrier is a glass plate, copper foil or aluminum foil.
17. The preparation method according to claim 5, characterized in that: The method further comprises step S3 of separating the polyimide film layer from the carrier.
18. The preparation method according to claim 17, characterized in that: The polyimide membrane is separated from the carrier by a water boiling method.