Wood preservatives
By using polyurethane polymers synthesized with polyoxypropylene polyols, isocyanates and blocking agents, combined with wood preservative actives, an environmentally friendly wood preservative composition is formed, which solves the toxicity and environmental pollution problems of existing wood preservatives, and realizes the realization of More effective wood protection.
Patent Information
- Application Number
- CN201980071294.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-09-28
- Filing Date
- 2019-09-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2039-09-24
AI Technical Summary
Existing wood preservatives are not very friendly from the perspective of toxicity and environmental pollution, and lack more environmentally friendly treatment methods.
Polyurethane polymers synthesized from polyoxypropylene polyols, isocyanates and blocking agents are combined with wood preservative actives such as halogenated isothiazolone, halogenated carbamate and azole fungicide to form an environmentally friendly wood preservative combination , used to treat wood.
The composition provides effective wood anti-corrosion protection, reducing the risk of environmental pollution, while improving the long-term protection of wood.
Smart Images

Figure BDA0003033069760000051 
Figure BDA0003033069760000061 
Figure BDA0003033069760000071
Abstract
Description
[0001] The present invention relates to a wood preservative composition and method for preserving wood to impart protection against wood decay organisms.
[0002] There are many methods and compositions for preserving wood before the time when wood is put into use. In addition, preservatives for treating wood in situ are available on the market, including both oil-based products and water-based products. Oil-based products are usually composed of petroleum containing pentachlorophenol or creosote. US 7,959,723 describes a composition of this type using an oil-soluble preservative for wood. From the perspective of toxicity and environmental pollution, these active ingredients are less desirable.
[0003] The problem addressed by the present invention is the need for a more environmentally friendly wood treatment composition that is able to effectively deliver active ingredients.
[0004] The present invention relates to a method for preserving wood, the method comprising contacting the wood with a wood preservative composition comprising:
[0005] a) a polyurethane polymer synthesized from a polyol containing >95% poly-propylene oxide; an isocyanate, and a capping agent; b) an organic solvent; and c) at least one wood preservative active selected from the group consisting of halogenated isothiazolone biocides, halogenated carbamate fungicides, and azole fungicides; wherein the capping agent is selected from the group consisting of: monoalcohols with an alkyl chain greater than or equal to C5 and secondary amine capping agents with an alkyl chain greater than or equal to C14, and mixtures thereof; and further wherein the molecular weight of the polyol is 2000.
[0006] The present invention further relates to a wood preservative composition comprising a) a polyurethane polymer synthesized from a polyol containing >95% poly-propylene oxide; an isocyanate, and a capping agent; b) an organic solvent; and c) at least one wood preservative active selected from the group consisting of a halogenated isothiazolone biocide, a halogenated carbamate fungicide, and an azole fungicide; wherein the capping agent is selected from the group consisting of a monoalcohol having an alkyl chain greater than or equal to C5 and a secondary amine capping agent having an alkyl chain greater than or equal to C14, and mixtures thereof; and further wherein the molecular weight of the polyol is 2000.
[0007] Unless otherwise indicated, all percentages and parts per million (ppm) values are based on the total weight of the composition. The term "a / an" refers to both the singular case and the case where more than one is present. All range endpoints are inclusive and combinable. As contained herein, all molecular weights are number average molecular weights and are determined by gel permeation chromatography (GPC). It is contemplated that one skilled in the art may select and / or combine multiple suitable and / or preferred embodiments of the present invention. Example
[0008] The wood preservative composition of the present invention comprises a polyurethane polymer synthesized by a dihydroxy-terminated polyoxypropylene macromonomer (polyol), an isocyanate and a suitable end-capping agent. As used herein, the polyurethane polymer may contain other functional groups derived from the reaction of isocyanate with other monomers, such as amide groups derived from carboxylic acids and ureas derived from amines (e.g., ethylenediamine (EDA)), or other polymers, such as polyesters, such as polyesters derived from adipic acid and 1,6-hexanediol, 1,4-butanediol and / or neopentyl glycol, or polycarbonates, such as polycarbonates derived from poly-1,6-hexanediol carbonate. Suitable isocyanates include, for example, methylenebis(4-cyclohexyl isocyanate) (MCI), methylenebis(4-phenyl isocyanate) (MDI), polymethylene polyphenol isocyanates (pMDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI) and toluene diisocyanate (TDI) and combinations thereof. Preferably, the isocyanate of the present invention is a diisocyanate. Examples of suitable diisocyanates include IPDI, pMDI, MDI and combinations thereof. More preferably, the diisocyanate is IPDI. The polyol used to prepare the polyurethane in the present invention is a >95% poly-propylene oxide having a molecular weight greater than or equal to 2000. Suitably, the molar ratio of isocyanate to polyol of the polyurethane polymer is less than 4 to greater than or equal to 1.05, alternatively less than or equal to 2 to greater than or equal to 1.05.
[0009] The polyurethane polymer of the present invention is end-capped. According to the present invention, the end-capping agent is an amine or an alcohol. Specifically, the end-capping agent is at least one of a mono-secondary alkylamine or a monoalcohol. According to the present invention, a monoalcohol having an alkyl chain greater than or equal to C5 and a secondary amine having an alkyl chain greater than or equal to C14 and a mixture thereof are suitable. The polyurethane polymer is synthesized in a non-aqueous solvent or a mixture of non-aqueous solvents. Preferably, the amount of the solvent is 60% to 90%, more preferably 70% to 90%, and most preferably 75% to 90%. Suitable solvents include ester and ether solvents having a boiling point of at least 150°C and preferably a flash point of at least 60°C. Examples of such solvents include alkanes, branched alkanes, aromatic hydrocarbons, such as mineral spirits, toluene, benzyl alcohol, xylene and alkylbenzenes. A mixture of suitable non-aqueous solvents that can be used in the present invention is Aromatic 200 (CAS No. 64742-94-5).
[0010] The wood treatment composition of the present invention, in addition to the polyurethane polymer, also contains a wood preservative active. The wood preservative active can be selected from the categories of halogenated isothiazolinone biocides, halogenated carbamate fungicides, metal salts of cyclohexane acids and azole fungicides. When the wood preservative active is a halogenated isothiazolinone biocide, it preferably contains a C4-C 12N-alkyl substituted 3-isothiazolone, more preferably chlorinated 3-isothiazolone, and most preferably 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one ("DCOIT"). Mixtures of wood preservative actives may be used. When the polyurethane polymer is combined with DCOIT, a suitable composition comprises 23% polyurethane polymer solids, 23% DCOIT, and 54% Aromatic 200.
[0011] The composition for treating wood preferably comprises 100 ppm to 40,000 ppm, more preferably 200 ppm to 30,000 ppm, and most preferably 300 ppm to 25,000 ppm of wood preservative. Preferably, the polymer solids content of the composition is 10% to 40%, more preferably 10% to 30%, and most preferably 15% to 30%. Preferably, the ratio of polymer solids to biocide is 2:1 to 1:2, more preferably 2:1 to 1:1.
[0012] Another key element of wood preservative composition is organic solvent. Polyurethane polymer is diluted with organic solvent. Suitably, organic solvent is diesel, however other organic solvents known to those skilled in the art can be used. In certain embodiments, organic solvent is not the same compound as non-aqueous solvent of the present invention. As used herein, diesel is defined as crude oil fractionation at 200°C (392°F) to 350°C (662°F) under atmospheric pressure to obtain a mixture of carbon chains typically containing 8 to 21 carbon atoms per molecule or biodiesel obtained from vegetable oil or animal fat (bio-lipid), which has been transesterified with methanol (fatty acid methyl ester (FAME)) and mixtures thereof.
[0013] The compositions used in the present invention may optionally contain additional components, including but not limited to stabilizers, dyes, water repellents, other wood biocides, fungicides and insecticides, antioxidants, metal chelators, free radical scavengers, etc. Stabilizers include, for example, organic and inorganic UV stabilizers, such as copper oxide or other copper salts or complexes that are resistant to leaching; zinc oxide; iron salts, iron oxides, iron complexes, transparent iron oxides, and nanoparticle iron oxides; titanium dioxide; benzophenones and substituted benzophenones; cinnamic acid and its esters and amides; substituted triazines, such as triphenyltriazine and substituted phenyltriazine UV absorbers, benzotriazoles and substituted benzotriazole UV absorbers; hindered amine light stabilizers, used alone or in combination. Water repellents include, for example, various wax-type water repellents, such as paraffin wax, carnauba wax, and polyethylene wax; and silicones. Other wood biocides, fungicides, such as copper metal, bethoxazin and cyproconazole, thiocarbamide, tebuconazole, propiconazole, pentachlorophenol, creosote, copper naphthenate, dialkyldimethyl quaternary ammonium carbonate / bicarbonate, and insecticides, including, for example, those listed in U.S. Pat. No. 6,610,282, such as imidacloprid, thiacloprid, permethrin and ethomethrin. Antioxidants include any commercially available antioxidant compounds, such as phosphite antioxidants (such as IRGAFOS); lactone antioxidants; phenolic antioxidants such as BHT; ascorbic acid; and IRGANOX, etc. Metal chelators include, for example, EDTA, NTA, 1,10-phenanthroline, ACUMER 3100, DEQUEST, TAMOL 731, tripolyphosphates and other inorganic and organic compounds and polymers that can be used to chelate or disperse metal salts. Free radical scavengers include, for example, TEMPO.
[0014] The preservation of wood is carried out by contacting the wood with the wood preservative composition described herein, preferably under conditions that comply with AWPA Standard T1-16 and meet the conditions of use specified in U1-16. In order to provide long-term protection, the preservative needs to be "fixed" in the wood and not lost too quickly by volatilization or by leaching when the wood becomes wet. It is expected that enhanced penetration or enhanced movement of the preservative deep into the wood during the treatment process may also result in reduced fixation of the organic wood preservative active.
[0015] Examples
[0016] Synthesis of polyurethane polymers:
[0017] The following polyurethanes were synthesized from dihydroxy terminated polyoxypropylene (polyol) and diisocyanate (IPDI). 150 mL of anhydrous polyoxypropylene, diisocyanate (2 molar equivalents of isocyanate relative to the hydroxyl groups) in aromatic 200 (solvent, 10-30 wt % solution) were charged to the reactor along with 0.003% of tin catalyst (dibutyltin dilaurate). A polyol with a molecular weight of 2000 was tested. The reactor was heated to 90°C with overhead stirring. The reaction mixture was held at 90°C for 1 h.
[0018] In the polyurethane end-capping example, Surface SWYPE TM The test strip measures the residual isocyanate. The reaction product is cooled to room temperature, and a blocking agent monoamine (1 equivalent of amine relative to the unreacted isocyanate) is added to block the remaining isocyanate groups in the reaction mixture. Alternatively, when a monool (1 equivalent of hydroxyl relative to the unreacted isocyanate) is used as a blocking agent, the monool is added at 90°C and allowed to react at 90°C for another 1h. The reaction is continued at 90°C until the SWYPE TM No free isocyanate was observed when the test strips were tested. The polymer solids of the PU solution were estimated from the conversion and the amount of reactants used for the reaction. The polymer solids were calculated as the sum of the reactive components in the polymer synthesis.
[0019] Procedure for Determining Diesel Fuel Compatibility:
[0020] In a clear 1 oz vial, 0.1 g of polymer (based on 100% polymer solids) was diluted to a 1% polymer solution with 9.9 g of diesel fuel (w / w). The sample was maintained at room temperature for 48 hours. After 48 hours, the solution was checked for incompatibility, defined as phase separation, precipitation of polymer as a solid, and / or turbidity.
[0021] Calculation of Hansen solubility parameters:
[0022] HSPiP software (purchased from https: / / www.hansen-solubility.com / ) calculated the Hansen Solubility Parameters (HSP) of various polyurethane end-capping segments. The predicted HSP (using the Y-MB method), i.e., HSP for dispersion (D), polarity (P) and hydrogen bonding (H) contributions (all SPs in MPa1 / 2), the total SP (calculated using the predicted HSP), and the "end-capping distance to diesel" were calculated. According to the HSP theory, the distance between two materials is a measure of solubility. The smaller the distance, the higher the solubility of the fluids in each other. The HSP data for "diesel" were obtained from the literature (Batista et al. J. Am. Oil Chem. Soc. [Journal of the American Petroleum Chemists Society] Vol. 92, 95, 2015).
[0023]
[0024]
[0025] δ D1 =Dispersion solubility parameter of diesel = 14.51
[0026] δ D2 = dispersion solubility parameter (δ) of a given end group D )
[0027] δ P1 = Polar solubility parameter of diesel = 3.18
[0028] δ P2 = Polar solubility parameter (δP) of a given end group
[0029] δ H1 =H bond solubility parameter of diesel = 5.97
[0030] δ H2 = H-bond solubility parameter (δ) of a given end group H )
[0031] Table 1. Diesel compatibility of PU polymers with different end-blocks with 100% p-iPO and IPDI (MW=2000)
[0032]
[0033] According to the present invention, the monoalcohol having an alkyl chain greater than or equal to C5 and the secondary amine end-capping agent having an alkyl chain greater than or equal to C14 are compatible.
[0034] Table 2. Diesel compatibility of PU polymers with different end-blocks synthesized with 100% p-iPO and MDI (MW = 2000)
[0035]
[0036] According to the present invention, the monoalcohol having an alkyl chain greater than or equal to C5 and the secondary amine end-capping agent having an alkyl chain greater than or equal to C14 are compatible.
Claims
1. A non-water-based wood preservative composition, comprising: a) A polyurethane polymer synthesized from: i) a polyol comprising > 95% poly-propylene oxide, ii) diisocyanate, and iii) a capping agent; b) an organic solvent comprising diesel fuel; and c) at least one wood preservative active selected from the group consisting of halogenated isothiazolone biocides, halogenated carbamate fungicides and azole fungicides; wherein the end-capping agent is selected from the group consisting of: a monoalcohol having an alkyl chain greater than or equal to C5 and a secondary amine end-capping agent having an alkyl chain greater than or equal to C14, and a mixture thereof; wherein the molecular weight of the polyol is greater than or equal to 2000; and The polyurethane polymer is compatible with the organic solvent.
2. The wood preservative composition according to claim 1, in, The wood antiseptic active substance is 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one.
3. The wood preservative composition according to claim 1, in, The polyol comprises 100% poly-propylene oxide.
4. The wood preservative composition according to claim 1, in, The polyol comprises 100% poly-isopropylene oxide.
5. The wood preservative composition according to claim 1, in, The diisocyanate is selected from methylene bis(4-phenylisocyanate) and isophorone diisocyanate.
6. The wood preservative composition according to claim 1, in, The organic solvent is diesel.
7. The wood preservative composition according to claim 1, in, The monoalcohol having an alkyl chain greater than or equal to C5 is selected from 1-pentanol, 1-hexanol, 1-octanol, behenyl alcohol and propylene glycol butyl ether.
8. The wood preservative composition according to claim 1, in, The secondary amine having an alkyl chain greater than or equal to C14 is selected from diheptylamine, dioctylamine and didecylamine.
9. A method for preserving wood, the method include: The wood is contacted with the non-aqueous wood preservative composition of claim 1.