A catalyst and its preparation method and application

By applying Ni1-mMom/Ce1-x-yGdxCayO2-δ-type metal-ceramic catalyst on the SOFC anode surface, the problems of anode carbon deposition and insufficient catalyst stability are solved, and efficient catalysis of hydrocarbon fuels and battery stability are achieved. promote.

CN114927706BActive Publication Date: 2024-10-11HUAIAN KUNBO INFORMATION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210484549.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-06
Publication Date
2024-10-11
Estimated Expiration
2042-05-06

AI Technical Summary

Technical Problem

When existing solid oxide fuel cells use hydrocarbon fuels, the anode carbon deposition problem leads to electrode performance decline and battery failure, and the catalyst stability is insufficient, affecting the battery's operational stability and catalytic performance.

Method used

Ni1-mMom/Ce1-x-yGdxCayO2-δ type metal-ceramic catalyst is used. By applying an independent catalytic layer on the surface of the SOFC anode, the redox cycle performance and porous structure of the ceramic phase are used to reduce the internal stress caused by structural mismatch. Improve the stability and catalytic performance of the catalyst.

Benefits of technology

It achieves efficient catalysis of complex hydrocarbon fuels at lower temperatures (600-700°C), improves the overall stability of the battery and the regeneration capacity of the catalyst, avoids the formation of anode carbon deposits, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114927706B_ABST
    Figure CN114927706B_ABST
Patent Text Reader

Abstract

The present invention discloses a catalyst, which is a metal-ceramic catalyst, and its molecular formula is Ni 1‑m Mo m / Ce 1‑x‑ y G x Ca y O 2‑δ , where 0.001≤m≤0.5, 0.005≤x≤0.20, 0.01≤y≤0.15, 1.75≤δ≤1.99. The catalyst prepared according to the technical solution of the present invention can not only achieve efficient catalysis of complex hydrocarbon fuels at a relatively low temperature (700°C), but also achieve in-situ regeneration of the catalyst, which is beneficial to improving the comprehensive stability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid oxide fuel cells, and in particular relates to a catalyst for a solid oxide fuel cell, a preparation method and an application thereof. Background Art

[0002] Solid Oxide Fuel Cell (SOFC) is a new type of energy conversion device that can directly convert chemical energy in fuel into electrical energy. It has the characteristics of high energy conversion efficiency and environmental friendliness. SOFC uses all-solid-state ceramics as battery components and has an operating temperature of 500-900°C. It can not only use hydrogen as fuel, but also use natural gas, shale gas, and natural gas hydrates to generate electricity, and has the characteristics of fuel diversity.

[0003] Solid oxide fuel cells mostly use metal Ni-based anodes as battery supports to facilitate their high electronic conductivity and efficient catalytic activity. When using hydrocarbon fuels (such as methane fuel), the metal Ni-based anode will catalyze the cracking of methane, causing the anode carbon deposition problem. On the one hand, anode carbon deposition will reduce the active catalytic reaction area on the electrode surface, block the electrode, and hinder gas diffusion, resulting in anode performance degradation; on the other hand, at the operating temperature of SOFC, carbon deposition will react with the metal Ni-based anode, causing the anode volume to expand, causing the battery to crack, and leading to battery failure.

[0004] In response to this problem, researchers at home and abroad have conducted research on the structural design of fuel cell catalytic units and proposed two types of battery configurations: external reforming catalytic SOFC and internal reforming catalytic SOFC. Among them, the internal reforming SOFC has attracted widespread attention from researchers due to its advantages such as high modularity and small battery system size. The internal reforming SOFC is to apply a reforming catalyst layer on the anode surface of a traditional SOFC single cell to achieve catalytic conversion of hydrocarbon fuels. During the operation of the battery, the complex hydrocarbon fuel is first converted into simple H through the reforming catalyst layer. 2 and CO and other fuel gases, the newly generated H 2 The CO and CO will diffuse into the anode functional layer of the fuel cell and participate in the electrochemical oxidation reaction. The use of a fuel catalytic layer can avoid the cracking of complex hydrocarbon fuels in the battery anode, reduce the risk of carbon deposition on the battery anode, and improve the stability of battery operation.

[0005] In previous studies, researchers mainly used SOFC single cells as support, prepared a catalytic layer on the anode surface, and constructed a double-layer anode structure of anode catalytic layer / anode electrochemical layer to improve the electrochemical performance of the battery in hydrocarbon fuels. For example, CN103165903A (201110422373.4) prepared a layer of Cu-LSCM-CeO on the anode surface of a traditional SOFC single cell. 2Catalytic layer to improve the catalytic performance of the fuel. However, the catalytic activity of Cu-based catalysts for complex hydrocarbon fuels is not ideal. CN110600775A (201910936331.9) discloses an in-situ reforming solid oxide fuel cell, which improves the catalytic activity of the catalyst layer by preparing a metal Ni-based catalyst on the surface of the SOFC anode. Using Ni-LaMnO 3 Catalysts can improve the chemical catalytic performance of SOFC cells, but their stability does not meet the application requirements of SOFC. Previous studies have also found that NiMo-zirconia doped cerium oxide catalysts have excellent catalytic performance for isooctane and are used in the anode catalyst layer of isooctane fuel SOFC cells. However, during the catalytic reaction, the cerium oxide-based catalyst layer will undergo oxidation and reduction processes, causing the volume of the catalyst layer to change, resulting in cracking of the catalyst layer. At this time, complex hydrocarbon gases that have not been catalytically converted can diffuse through the cracks to the anode electrochemical functional layer, inducing anode carbon deposition and causing battery performance degradation. Therefore, improving the structural stability of the catalyst layer is the focus of current research.

[0006] In recent years, researchers have proposed a porous YSZ-supported SOFC single-cell configuration based on the chemical and structural stability of yttria-stabilized zirconium dioxide (YSZ) materials, which achieves the dual functions of mechanical support and chemical catalysis by preparing catalysts in a porous YSZ support. However, porous YSZ is a catalytically inert material, and using YSZ as a support is not conducive to optimizing the catalytic performance of the battery. On the other hand, the preparation of YSZ-supported SOFCs has the problem of high-temperature co-firing of the battery catalyst layer support and the battery electrochemical functional layer, which will increase the complexity of battery preparation.

[0007] Therefore, the development of a catalyst with high catalytic efficiency and wide fuel adaptability is of great significance for the commercial application of hydrocarbon fuel SOFC systems. Summary of the invention

[0008] In order to solve the problems in the prior art, the present invention provides a catalyst, which catalytically converts hydrocarbon fuel into H by applying a catalyst layer on the anode surface of a SOFC single cell. 2 and CO to improve the electrochemical performance and stability of the battery. The operating temperature range of the catalyst of the present invention is 600-750°C. On the other hand, the present invention adopts an independent anode catalyst layer battery design, and the contact mode between the catalyst layer and the battery functional layer is physical contact, which can reduce the internal stress caused by structural mismatch and improve the stability of the battery.

[0009] Specifically, the present invention is achieved by the following method:

[0010] In one aspect, the present invention provides a catalyst, wherein the catalyst is a metal-ceramic catalyst, and its molecular formula is Ni1-m Mo m / Ce 1-x-y G x Ca y O 2-δ , where 0.001≤m≤0.5, 0.005≤x≤0.20, 0.01≤y≤0.15, 1.75≤δ≤1.99.

[0011] In the present invention, the use of Gd and Ca composite doping is beneficial to improving the catalytic performance of the catalyst. The catalyst in the prior art can effectively catalyze the conversion of hydrocarbon fuels at 750°C. When the temperature is reduced to 700°C, its catalytic activity obviously declines. In order to ensure the catalytic performance, it is necessary to add precious metal materials such as Ru to the metal phase of the catalyst. However, even without using precious metals, the catalyst of the present invention can have a catalytic reaction temperature of no more than 700°C, for example, 600-700°C, and has high catalytic activity.

[0012] The catalytic process of the catalyst of the present invention on hydrocarbon fuels involves the following basic steps: ① adsorption of hydrocarbons on the catalyst surface; ② decomposition of hydrocarbons on the catalyst surface; ③ partial oxidation of hydrocarbons on the catalyst surface and reduction of the catalyst; ④ desorption of newly generated small molecule fuel gas on the catalyst surface; ⑤ capture of oxygen source (e.g. H 2 O or CO 2 ) and is oxidized to the initial state. Among them, steps ①, ② and ④ are mainly determined by the influence of the NiMo metal phase in the catalyst on the binding energy of different gas molecules, while steps ③ and ⑤ are mainly affected by the ceramic phase (i.e. Ce 1-x- y G x Ca y O 2-δ )'s oxygen storage capacity and redox cycle performance.

[0013] The ceramic phase of the metal-ceramic catalyst of the present invention is a composite ceramic oxide with a fluorite structure, which has a large number of oxygen ions and a certain concentration of oxygen vacancies. The oxygen vacancies represent the absence of oxygen in the crystal structure, forming vacancies. 1-x- y G x Ca y O 2-δ In the formula, δ reflects the oxygen vacancy concentration in the material. During the catalytic process, hydrocarbon fuels can be oxidized on the catalyst surface (equivalent to the transfer of oxygen from the catalyst to the hydrocarbon, and the catalyst is partially reduced), and the hydrocarbon fuel undergoes partial oxidation reaction to generate H 2 and CO.

[0014] At the same time, in hydrocarbon fuels, carbon accumulation on the catalyst surface is the main cause of catalyst performance degradation (deactivation). At this time, by introducing a certain oxygen source (such as air) into the SOFC anode, the carbon accumulation is oxidized to achieve catalyst regeneration. Therefore, in the catalytic reaction, the catalyst will undergo repeated oxidation-reduction processes, and the oxygen ions and oxygen vacancies in the porous ceramic phase promote the oxidation-reduction process of the catalyst.

[0015] In traditional internal reforming catalytic SOFC, the catalyst layer and the battery anode are prepared into an integrated structure through a sintering process (equivalent to the catalyst layer and the anode layer being tightly bonded together). When the catalyst layer is regenerated in situ, the catalyst is partially oxidized (for example, an oxide layer may form on the metal phase surface, and the ceramic phase Ce 1-x-y G x Ca y O 2-δ It may also be partially oxidized, which is manifested as a change in the δ value), causing the catalyst layer to expand. Since the catalyst layer and the anode layer are tightly combined, the expansion of a single layer will induce stress, causing the catalyst layer to crack.

[0016] Furthermore, the catalyst molecular formula is Ni 0.999 Mo 0.001 / Ce 0.845 G 0.005 Ca 0.15 O 1.8475 、Ni 0.85 Mo 0.15 / Ce 0.855 G 0.095 Ca 0.05 O 1.9025 or Ni 0.5 Mo 0.5 / Ce 0.79 G 0.2 Ca 0.01 O 1.89 .

[0017] Furthermore, the Ni in the catalyst 1-m Mo m The content is 2-12wt%. The ratio of Ni and Mo in the catalyst mainly affects the performance stability of the catalyst. In the process of catalytic conversion of hydrocarbon fuels, the cracking of hydrocarbon fuels on the catalyst surface will cause carbon deposition, resulting in catalyst deactivation. Adding Mo to Ni-based metals helps to inhibit the adsorption of carbon on the catalyst surface, thereby alleviating the deactivation of the catalyst surface due to carbon deposition.

[0018] Specifically, Ni in the catalyst 1-m Mo mThe content of Ni in the catalyst is 3-11wt%, 4-10wt%, 5-9wt%, 6-8wt%; preferably, Ni 1-m Mo m The content is about 2wt%, about 3wt%, about 4wt%, about 5wt%, about 6wt%, about 7wt%, about 8wt%, about 9wt%, about 10wt%, about 11wt% or about 12wt%.

[0019] Furthermore, the catalyst has a porous structure with a pore size of 1-20 μm. The porous structure increases the specific surface area of ​​the catalyst and is more conducive to the diffusion and adsorption of hydrocarbons in the catalyst.

[0020] The present invention optimizes the catalytic performance of the catalyst by improving the composition of the catalyst ceramic phase, so that when the reaction temperature is reduced to 700° C., the catalyst can exhibit catalytic performance equivalent to that of a catalyst containing precious metals.

[0021] In one aspect, the present invention provides a method for preparing the above catalyst, comprising the following steps:

[0022] Preparation of ceramic materials:

[0023] Weighing a cerium source, a gadolinium source, and a calcium source and mixing them with a solvent to obtain a mixture;

[0024] The mixture is heated, ball-milled and calcined to obtain Ce 1-x-y G x Ca y O 2-δ Ceramic materials;

[0025] Ceramic support preparation:

[0026] Ce 1-x-y G x Ca y O 2-δ Ceramic materials and pore-forming agents are ball-milled and calcined to obtain porous Ce 1-x-y G x Ca y O 2-δ Ceramic support;

[0027] Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Catalyst preparation:

[0028] The Ni source and the Mo source are prepared into Ni-containing 2+ The solution and Mo-containing 6+ of solution;

[0029] Ni2+ Solution and Mo 6+ Solution immersed in Ce 1-x-y G x Ca y O 2-δ The catalyst is calcined in a ceramic support.

[0030] Specifically, the method for preparing the catalyst comprises the following steps:

[0031] Preparation of ceramic materials:

[0032] Using polyvinyl alcohol as a raw material, a polyvinyl alcohol aqueous solution with a concentration of 5-8 wt% is prepared;

[0033] Press Ce 1-x-y G x Ca y O 2-δ The cerium source, gadolinium source and calcium source are weighed in element stoichiometric ratio and dissolved in a polyvinyl alcohol aqueous solution to obtain a mixture, and then the mixture is heated to 100-300°C to evaporate the water and then undergo a combustion reaction to obtain a product, and the product is ball-milled and dried in anhydrous ethanol as a medium, and the dried product is calcined in an air atmosphere at 700-1000°C for 1-3h to obtain Ce 1-x-y G x Ca y O 2-δ Ceramic materials;

[0034] Ceramic support preparation:

[0035] Ce 1-x-y G x Ca y O 2-δ The ceramic material and the pore-forming agent are ball-milled, and then the mixed powder is pressed into a ceramic substrate (thickness 0.1-1.5 mm) by dry pressing, and then calcined at 1300-1500℃ for 3-5h to obtain porous Ce 1-x-y G x Ca y O 2-δ Ceramic support;

[0036] Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Catalyst preparation:

[0037] According to the element stoichiometric ratio, the Ni source and the Mo source are prepared to a concentration of 0.25-1.5 mol L -1 Ni 2+ Aqueous solution and 0.001~0.24mol L -1Mo 6+ aqueous solution, and then Ni 2+ Aqueous solution and Mo 6+ The aqueous solution is impregnated into the porous Ce 1-x-y G x Ca y O 2-δ The impregnated ceramic support is calcined in air at 500-700°C for 0.5-2h to obtain Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ catalyst.

[0038] The anode catalyst layer of traditional internal reforming catalytic SOFC is mostly supported by the battery anode (or single cell). The catalyst layer is not self-supporting, and the catalyst layer and the battery anode are prepared as one through a sintering process. The multi-layer anode structure (such as the anode catalyst layer and the anode electrochemical functional layer) must meet stringent thermal expansion coefficient matching conditions to ensure the structural stability of the battery during the heating and cooling process (if the thermal expansion coefficients of the battery anode catalyst layer and the anode electrochemical functional layer do not match, the battery may crack due to internal stress during the heating and cooling process, thereby reducing the structural stability of the battery). The catalyst material prepared in the present invention is composed of a ceramic substrate and has self-supporting characteristics. It does not need to be attached to a SOFC single cell, that is, there is no need to consider the problem of thermal expansion coefficient matching. During the battery assembly process, it is only necessary to place the anode catalyst layer of the present invention on the surface of the battery anode, and there is no need to use a sintering process to sinter the catalyst layer and the battery anode into one. Therefore, during the heating and cooling process, the expansion and contraction of the catalyst and the anode are relatively independent, thereby improving the stability of the overall battery structure.

[0039] Furthermore, in the preparation process of the ceramic material, the cerium source is selected from cerium nitrate or cerium acetate, the gadolinium source is selected from gadolinium nitrate or gadolinium acetate, and the calcium source is selected from calcium nitrate or calcium acetate; and the solvent is a polyvinyl alcohol aqueous solution with a concentration of 5-8wt%.

[0040] Furthermore, during the preparation of the ceramic material, the mixture is heated at a temperature of 100-300°C, the ball milling medium is anhydrous ethanol, the ball milling time is 12-48h, the calcination temperature is 700-1000°C, and the calcination time is 1-3h.

[0041] Specifically, during the preparation of the ceramic material, the mixture is heated to a temperature of 150-250°C; preferably, the mixture is heated to a temperature of about 100°C, about 150°C, about 200°C, about 250°C or about 300°C.

[0042] Specifically, during the preparation of the ceramic material, the calcination temperature is 750-950°C, 800-900°C or 850-900°C; preferably, the calcination temperature is about 700°C, about 750°C, about 800°C, about 850°C, about 900°C, about 950°C or about 1000°C.

[0043] Specifically, during the preparation of the ceramic material, the calcination time is 1.5-2.5 h or 1.5-2 h; preferably, the calcination time is about 1 h, about 1.5 h, about 2 h, about 2.5 h or about 3 h.

[0044] Furthermore, during the preparation of the ceramic support, the pore-forming agent is selected from polymethyl methacrylate, carbon powder or starch, the calcination temperature is 1300-1500° C., and the calcination time is 3-5 hours. During the calcination process, the pore-forming agent is ablated, thereby obtaining a porous ceramic substrate.

[0045] Specifically, during the preparation of the ceramic support, the calcination temperature is 1350-1450°C or 1350-1400°C; preferably, the calcination temperature is about 1300°C, about 1350°C, about 1400°C, about 1450°C or about 1500°C.

[0046] Specifically, during the preparation of the ceramic support, the calcination time is 3.5-4.5 h or 3.5-4 h; preferably, the calcination temperature is about 3 h, about 3.5 h, about 4 h, about 4.5 h or about 5 h.

[0047] Furthermore, Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ During the catalyst preparation process, the Ni source is selected from Ni(NO 3 ) 2 6H 2 O or nickel acetate, the Mo source is selected from (NH 4 ) 6 Mo 7 O 24 6H 2 O;Ni 2+ Solution and Mo 6+ The solution was impregnated into Ce by vacuum impregnation 1-x- y G x Ca y O 2-δ Ceramic support; calcination temperature is 500-700°C, and calcination time is 0.2-5h.

[0048] Furthermore, Ni 2+ Solution and Mo6+ The solution was impregnated into the porous Ce 1-x- y G x Ca y O 2-δ Ceramic support.

[0049] Preferably, Ni 2+ Solution is Ni 2+ Aqueous solution, Mo 6+ The solution is Mo 6+ Aqueous solution.

[0050] In another aspect, the present invention provides a battery anode, comprising an anode layer and the above-mentioned catalyst.

[0051] Furthermore, the battery anode is preferably a SOFC single cell anode.

[0052] In yet another aspect, the present invention provides a single cell, wherein the single cell comprises the battery anode described above.

[0053] Furthermore, the single cell is preferably a SOFC single cell.

[0054] According to the technical solution of the present invention, it has the following beneficial effects: it can not only realize efficient catalysis of complex hydrocarbon fuels (methanol, ethanol, isooctane, etc.) at a relatively low temperature (e.g., 600-700°C), but also realize in-situ regeneration of the catalyst, which is beneficial to improving the overall stability of the battery. On the other hand, the present invention adopts an independent design of the anode catalyst layer, which can reduce the internal stress caused by the structural mismatch in the integrated design of the anode catalyst layer / anode electrochemical functional layer, and improve the stability of the battery. The anode catalyst of the present invention is composed of porous Ce 1-x-y G x Ca y O 2-δ The ceramic support can not only provide reactive sites for hydrocarbon fuel conversion, but also inhibit the oxygen source (O 2 , H 2 O) directly contacts the anode electrochemical functional layer to avoid local oxidation of the metal-based anode; at the same time, an excess of oxidant (such as air) can be input into the anode to oxidize the carbon deposits in the catalyst layer, thereby achieving deactivation and regeneration of the catalyst and further improving the catalytic stability.

[0055] Additional aspects and advantages of the present invention will be set forth in part in, and in part will be apparent from, the description which follows. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0057] Figure 1 The three-point bending strength test results of the metal-ceramic catalyst layer of the present invention;

[0058] Figure 2 Ce prepared in the embodiment of the present invention 1-x-y G x Ca y O 2-δ XRD test results of ceramic phase;

[0059] Figure 3 Ni prepared in the embodiment of the present invention 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ XRD test results of metal-ceramic catalyst;

[0060] Figure 4 Ni prepared in Example 2 of the present invention 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ SEM test results of metal-ceramic catalyst;

[0061] Figure 5 A schematic diagram of the structure of a SOFC single cell with an independent catalyst layer prepared in an embodiment of the present invention;

[0062] Figure 6 This is a SEM photo of a SOFC single cell with an independent catalyst layer prepared in an embodiment of the present invention;

[0063] Figure 7 Ni prepared in the embodiment of the present invention 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Figure 1. Test device for the catalytic performance of the layer to hydrocarbon fuels;

[0064] Figure 8 High temperature fuel cell test device for studying the electrochemical performance of SOFC single cells;

[0065] Fig. 9 Ni prepared in Example 2 of the present invention 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ The catalytic layer is CH 4Catalytic performance test results of partial oxidation reforming reaction;

[0066] Fig.10 Ni prepared in Example 1 of the present invention at different test temperatures 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ The catalytic layer is CH 4 The catalytic performance stability test results;

[0067] Fig.11 The catalyst prepared in Example 2 of the present invention catalyzes the conversion of complex liquid hydrocarbon fuels;

[0068] Fig.12 Ni prepared in Example 3 of the present invention 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Catalytic layer for C 2 H 5 Catalytic performance test results of OH fuel;

[0069] Fig.13 Ni prepared in Example 2 of the present invention 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Catalytic layer for C 8 H 18 The catalytic performance test results of the fuel;

[0070] Fig.14 Ni prepared in Example 1 of the present invention 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ The results of the effect of the catalyst layer on the electrochemical performance of a single SOFC cell;

[0071] Fig.15 The performance stability test results of the SOFC single cell prepared in Example 1 of the present invention in 700°C methane fuel are shown. DETAILED DESCRIPTION

[0072] Embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0073] The materials mentioned above are all commercially available unless otherwise specified, and the methods mentioned above are all conventional methods unless otherwise specified.

[0074] Example 1

[0075] Preparation of ceramic materials:

[0076] Polyvinyl alcohol was used as a raw material to prepare a 5 wt% polyvinyl alcohol aqueous solution. 0.845 G 0.005 Ca 0.15 O 1.8475 7.338 g of cerium nitrate, 0.045 g of gadolinium nitrate and 0.708 g of calcium nitrate were weighed in a stoichiometric ratio of metal elements and dissolved in a polyvinyl alcohol aqueous solution. After the raw materials were completely dissolved, a mixture was obtained. The mixture was moved to a heating plate and heated to 200°C to evaporate the water until a combustion reaction occurred to obtain a combustion product. The product was ball-milled on a spheroidal graphite mill with anhydrous ethanol as a medium for 24 h. After ball milling, the product was dried at 80°C and calcined at 850°C in an air atmosphere for 2 h to obtain Ce. 0.845 G 0.005 Ca 0.15 O 1.8475 Powder.

[0077] Ceramic support preparation:

[0078] Ce 0.845 G 0.005 Ca 0.15 O 1.8475 The mixed powder was then pressed into a disc-shaped ceramic substrate with a diameter of 30 mm and a thickness of 1 mm by dry pressing. The ceramic substrate was calcined at 1400°C in air for 4 h to obtain Ce 0.845 G 0.005 Ca 0.15 O 1.8475 Ceramic substrate.

[0079] Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Catalyst preparation:

[0080] Take Ni(NO 3 ) 2 6H 2 O and (NH 4 ) 6 Mo 7 O 24 6H 2 O as raw material, according to Ni 0.999 Mo0.001 The ratio of metal elements in the mixture is 0.999 mol L -1 Ni 2+ and 0.001 mol L -1 Mo 6+ aqueous solution, Ni at a pressure of 0.1 atm 2+ and Mo 6+ Ion impregnation in porous Ce 0.845 G 0.005 Ca 0.15 O 1.8475 The Ni 0.999 Mo 0.001 / Ce 0.845 G 0.005 Ca 0.15 O 1.8475 The catalyst was impregnated 6 times to obtain a metal-ceramic type catalyst layer.

[0081] Example 2

[0082] Preparation of ceramic materials:

[0083] Polyvinyl alcohol was used as a raw material to prepare a 5 wt% polyvinyl alcohol aqueous solution. 0.855 G 0.095 Ca 0.05 O 1.9025 7.425 g of cerium nitrate, 0.858 g of gadolinium nitrate and 0.236 g of calcium nitrate were weighed in a stoichiometric ratio of metal elements and dissolved in a polyvinyl alcohol aqueous solution. After the raw materials were completely dissolved, a mixture was obtained. The mixture was moved to a heating plate and heated to 200°C to evaporate the water until a combustion reaction occurred to obtain a combustion product. The product was ball-milled on a spheroidal graphite mill with anhydrous ethanol as a medium for 24 h. After ball milling, the product was dried at 80°C and calcined at 850°C in an air atmosphere for 2 h to obtain Ce. 0.855 G 0.095 Ca 0.05 O 1.9025 Powder.

[0084] Ceramic support preparation:

[0085] Ce 0.855 G 0.095 Ca 0.05 O 1.9025 The mixed powder was then pressed into a disc-shaped ceramic substrate with a diameter of 30 mm and a thickness of 1 mm by dry pressing. The ceramic substrate was calcined at 1400°C in air for 4 h to obtain Ce 0.855 G 0.095 Ca 0.05 O1.9025 Ceramic substrate.

[0086] Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Catalyst preparation:

[0087] Take Ni(NO 3 ) 2 6H 2 O and (NH 4 ) 6 Mo 7 O 24 6H 2 O as raw material, according to Ni 0.85 Mo 0.15 The ratio of metal elements in the mixture is 0.85 mol L -1 Ni 2+ and 0.15 mol L -1 Mo 6+ aqueous solution, Ni at a pressure of 0.1 atm 2+ and Mo 6+ Ion impregnation in porous Ce 0.855 G 0.095 Ca 0.05 O 1.9025 The Ni 0.85 Mo 0.15 / Ce 0.855 G 0.095 Ca 0.05 O 1.9025 The catalyst was impregnated 6 times to obtain a metal-ceramic type catalyst layer.

[0088] Example 3

[0089] Preparation of ceramic materials:

[0090] Polyvinyl alcohol was used as a raw material to prepare a 5 wt% polyvinyl alcohol aqueous solution. 0.79 G 0.2 Ca 0.01 O 1.89The stoichiometric ratio of the metal elements was 6.861 g of cerium nitrate, 1.805 g of gadolinium nitrate and 0.047 g of calcium nitrate, which were dissolved in a polyvinyl alcohol aqueous solution. After the raw materials were completely dissolved, a mixture was obtained. The mixture was moved to a heating plate and heated to 200°C to evaporate the water until a combustion reaction occurred to obtain a combustion product. The product was ball-milled on a spheroidal graphite mill with anhydrous ethanol as a medium for 24 h. After ball milling, the product was dried at 80°C and calcined at 850°C in an air atmosphere for 2 h to obtain Ce. 0.79 G 0.2 Ca 0.01 O 1.89 Powder.

[0091] Ceramic support preparation:

[0092] Ce 0.79 G 0.2 Ca 0.01 O 1.89 The mixed powder was then pressed into a disc-shaped ceramic substrate with a diameter of 30 mm and a thickness of 1 mm by dry pressing. The ceramic substrate was calcined at 1400°C in air for 4 h to obtain Ce 0.79 G 0.2 Ca 0.01 O 1.89 Ceramic substrate.

[0093] Ni 0.5 Mo 0.5 / Ce 0.79 G 0.2 Ca 0.01 O 1.89 Catalyst preparation:

[0094] Take Ni(NO 3 ) 2 6H 2 O and (NH 4 ) 6 Mo 7 O 24 6H 2 O as raw material, according to Ni 0.5 Mo 0.5 The concentration of metal elements in the mixture is 0.5 mol L -1 Ni 2+ and 0.5 mol L -1 Mo 6+ aqueous solution, Ni at a pressure of 0.1 atm 2+ and Mo 6+ Ion impregnation in porous Ce 0.79 G 0.2 Ca 0.01 O 1.89The Ni 0.5 Mo 0.5 / Ce 0.79 G 0.2 Ca 0.01 O 1.89 The catalyst was impregnated 6 times to obtain a metal-ceramic type catalyst layer.

[0095] Performance Test:

[0096] The metal-ceramic catalyst layer prepared in Example 1 was subjected to a three-point bending strength test. The results are as follows: Figure 1 As shown. It can be seen that the fracture strength of the prepared metal-ceramic catalyst layer is 23MPa, which meets the mechanical property requirements of the SOFC support (SOFC requires the matrix fracture strength to be greater than 20MPa).

[0097] The ceramic phases prepared in Examples 1-3 were subjected to XRD testing, and the test results are as follows: Figure 2 As shown, (a) is the ceramic phase prepared in Example 1, (b) is the ceramic phase prepared in Example 2, and (c) is the ceramic phase prepared in Example 3. The XRD test results show that Ce with fluorite structure can be obtained by the polyvinyl alcohol combustion method. 1-x-y G x Ca y O 2-δ Ceramic material.

[0098] The metal-ceramic catalysts prepared in Examples 1-3 were subjected to XRD testing, and the results were as follows: Figure 3 As shown, (a) is the catalyst layer prepared in Example 1, (b) is the catalyst layer prepared in Example 2, and (c) is the catalyst layer prepared in Example 3. The XRD test results show that Ni can be observed in the range of 2θ=40-55°. 1-m Mo m The corresponding XRD diffraction peaks indicate that Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Metal-ceramic type catalyst.

[0099] The SEM test results of the metal-ceramic catalyst prepared in Example 2 are as follows: Figure 4 As shown, the results indicate that the porosity of the porous catalytic layer is 35-40%, which meets the application requirements of fuel cells. Figure 4 (b) is a high-magnification structural photograph of the catalytic layer. 0.855 G 0.095 Ca0.05 O 1.9025 Evenly distributed nano-sized Ni can be observed on the surface of the ceramic skeleton. 0.85 Mo 0.15 The SEM test results show that the preparation method of the present invention can obtain Ni with uniform distribution of metal phase. 0.85 Mo 0.15 / Ce 0.855 G 0.095 Ca 0.05 O 1.9025 Catalytic layer.

[0100] Figure 5 Schematic diagram of the structure of a SOFC single cell with an independent catalyst layer. The cell is composed of Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Catalytic layer and SOFC electrochemical functional layer (functional layer includes NiO-YSZ anode layer / (ZrO 2 ) 0.92 (Y 2 O 3 ) 0.08 / Ce 0.8 Sm 0.2 O 1.9 Double electrolyte layer / La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ cathode layer). Ni 1-m Mo m -Ce 1-x-y G x Ca y O 2-δ The thickness of the catalyst layer is 0.1-1.5 mm, the thickness of the NiO-YSZ anode layer is 0.1-1.5 mm, and the thickness of other battery functional layers is 5-100 μm.

[0101] Figure 6 This is a SEM photo of a SOFC cell with an independent catalyst layer prepared in Example 2. It can be seen from the figure that the anode and cathode of the cell have porous microstructure characteristics. 0.8 Sm 0.2 O 1.9 The electrolyte is relatively dense, and the contact between different functional layers of the battery is good. The process of the present invention can be used to prepare an anode-supported single cell. 0.85 Mo 0.15 / Ce 0.855 G 0.095 Ca0.05 O 1.9025 The anode catalyst layer is applied to the anode surface of a single cell to obtain a hydrocarbon fuel SOFC single cell with reforming catalytic function.

[0102] Figure 7 For the present invention, Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ The test device of the catalytic performance of the catalyst layer on hydrocarbon fuels is shown in Figure 1. A quartz tube reactor with an inner diameter of 7 mm is used to study the performance of the catalyst layer. First, the catalyst layer support is crushed, and 0.3 g of the crushed powder is weighed and placed in the quartz tube reactor. Quartz wool is used to fix it in the middle of the quartz tube. A K-type thermocouple is used to monitor the catalytic reaction temperature. At temperatures of 700°C and 750°C, respectively, O 2 The catalytic performance of the catalyst for reforming hydrocarbon fuels was studied using gas chromatography under the condition of a C / C ratio of 0.5.

[0103] (1) When using methane (CH 4 ) is the fuel, the flow rate of methane is 50 mL / min, the flow rate of air is 125 mL / min, and the fuel conversion rate and H are calculated using the following formula 2 And the CO yield:

[0104] Methane conversion rate = (CO and CO 2 The sum of the moles of methane) / (the moles of input methane);

[0105] H 2 Yield = H 2 Number of moles / (2*number of moles of input methane);

[0106] CO yield = number of moles of CO / number of moles of input methane.

[0107] (2) When methanol (CH 3 When OH) is used as fuel, the flow rate of liquid methanol is 0.09 mL / min, and the flow rate of nitrogen is 100 mL / min. The fuel conversion rate and H 2 And CO yield:

[0108] Methanol conversion rate = (CO and CO 2 The sum of the moles of methanol) / (the moles of methanol input);

[0109] H 2 Yield = H 2 The number of moles of methanol / (2*the number of moles of methanol obtained by input);

[0110] CO yield = number of moles of CO / number of moles of input methanol.

[0111] (3) When ethanol (C 2 H 5 OH) is used as fuel. The flow rate of liquid ethanol is 0.065 mL / min, and the air flow rate is 62.5 mL / min. The fuel conversion rate and H 2 And CO yield:

[0112] Ethanol conversion rate = (CO, CO 2 and the sum of the moles of methane) / (2*the moles of ethanol input);

[0113] H 2 Yield = H 2 The number of moles of ethanol / (3*the number of moles of ethanol input);

[0114] CO yield = number of moles of CO / (2*number of moles of ethanol input).

[0115] (4) When isooctane (C 8 H 18 ) is the fuel, the flow rate of liquid isooctane is 0.046 mL / min, the air flow rate is 125 mL / min, and the fuel conversion rate and H are calculated using the following formula 2 And CO yield:

[0116] Isooctane conversion = (CO, CO 2 and the sum of the moles of methane) / (8*the moles of input isooctane);

[0117] H 2 Yield = H 2 The number of moles of isooctane / (9*the number of moles of isooctane input);

[0118] CO yield = number of moles of CO / (8*number of moles of input isooctane).

[0119] Figure 8 In order to study the electrochemical performance of SOFC single cell, a high temperature fuel cell test device is provided. 2 O 3 The battery samples were sealed with ceramic sealant, and the battery temperature was raised to 700°C for electrochemical performance testing. When hydrogen was used as fuel, hydrogen was directly input into the anode port of the battery; when hydrocarbons were used as fuel, a mixture of hydrocarbons and air was introduced into the anode port of the fuel cell, and the O in the anode fuel was regulated by controlling the flow rate of hydrocarbons and air. 2 / C ratio.

[0120] Fig. 9At 700℃, O 2 Ni prepared in Example 2 under the test condition of a / C ratio of 0.5 0.85 Mo 0.15 / Ce 0.855 G 0.095 Ca 0.05 O 1.9025 The catalytic layer is CH 4 Catalytic performance of partial oxidation reforming reaction. 1-m Mo m When the mass fraction of H increases from 2wt% to 8wt%, the methane conversion rate gradually increases from 40% to 82%. 2 The yield increased from 29% to 75%, and the CO yield increased from 22% to 36%, indicating that the increase of Ni 1-m Mo m The content is beneficial to promote the conversion of methane in the catalytic layer. 1-m Mo m When the content reaches 12wt%, its catalytic performance does not change significantly. 1-x-y G x Ca y O 2-δ Chinese Ni 1-m Mo m The increase in the content of catalytic active centers (Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ The metal / ceramic interface is close to saturation, resulting in no significant improvement in catalytic performance; on the other hand, the introduction of too high Ni in the catalyst 1-m Mo m The metal phase content will induce high-temperature sintering of the catalyst and reduce the catalytic performance. 1-m Mo m When the content increased from 8wt% to 12wt%, the catalyst performance did not change significantly.

[0121] Fig.10 O 2 When / C is 0.5, the Ni prepared in Example 1 at different test temperatures (700°C and 750°C) 0.999 Mo 0.001 / Ce 0.845 G 0.005 Ca 0.15 O 1.8475 The catalytic layer is CH 4 The results show that at 700-750℃, Ni 1-m Mom / Ce 1-x-y G x Ca y O 2-δ The catalysts can achieve stable catalysis of methane. When the reaction temperature is 700℃, the methane conversion rate is 80%, H 2 When the reaction temperature was increased to 750℃, the methane conversion rate increased to 94%, and the H 2 The CO and CO yields were 80% and 42%, respectively.

[0122] Fig.11 The catalyst of the present invention catalyzes the conversion of complex liquid hydrocarbon fuels. Fig.11 Compared with the Ni prepared in Example 2 0.85 Mo 0.15 / Ce 0.855 G 0.095 Ca 0.05 O 1.9025 Partial oxidation reforming performance of methanol over the catalyst layer at 700℃ and 750℃. 2 Under the catalytic reaction conditions of 0.5 / C ratio, the methanol fuel conversion rate is 80-90%, and H 2 and CO yields were 70-80% and 35-40%, respectively.

[0123] Figure 12-13 Ni prepared in Example 3 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Catalytic layer for C 2 H 5 OH and Ni prepared in Example 2 0.85 Mo 0.15 / Ce 0.855 G 0.095 Ca 0.05 O 1.9025 Catalytic layer C 8 H 18 The catalytic performance test results of the fuel. Figure 12-13 As shown, in O 2 When the Ni / C ratio is 0.5 and the catalytic reaction temperature is 700-750℃, 1-m Mo m -Ce 1-x-y G x Ca y O 2-δThe catalytic layer can achieve efficient catalysis of hydrocarbon fuels. For SOFC, lowering the operating temperature is beneficial to inhibiting high-temperature aging of materials, reducing system complexity, and improving the stability of the battery system, which is of great significance to the commercialization of SOFC.

[0124] Fig.14 To study the Ni prepared in Example 1 0.999 Mo 0.001 / Ce 0.845 G 0.005 Ca 0.15 O 1.8475 The results of the effect of the catalyst layer on the electrochemical performance of SOFC single cells show that: 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ After the catalyst layer (such as Fig.14 (a) The maximum output power density of the battery in standard hydrogen fuel is 509mW / cm 2 When converting fuel into isooctane, its maximum output power density is 303mW / cm 2 , the battery can maintain 60% of its original performance (the performance of standard hydrogen fuel). Fig.14 (b)) The maximum output power density is 552 mW / cm at 700 °C in standard hydrogen fuel. 2 When converting fuel into isooctane, its maximum output power density is 250mW / cm 2 The performance was reduced by 54.7%. The maximum output power density of the battery with the catalytic layer in isooctane was 250mW / cm 2 Increased to 303mW / cm 2 , the performance was improved by 20%, confirming its efficient catalysis in fuel cells.

[0125] Fig.15 The performance stability of SOFC single cell in 700℃ methane fuel. Fig.15 (a) shows that at 300 mA / cm 2 At a discharge current density of 1.5 Å, the voltage decay rate of a single cell without a catalyst layer was 11.3 mV / h in the first 9 hours. After the anode carbon deposition was treated by in-situ activation of the anode (redox: 15 mL / min was introduced into the anode of the cell for 5 minutes to eliminate carbon deposition in the catalyst), the battery performance decayed further. For cells without a stand-alone catalyst layer, this reactivation process may lead to anode oxidation, reducing the electrochemical performance and stability of the cell. Ni prepared in Example 1 was applied to the surface of the anode of the SOFC cell.0.999 Mo 0.001 / Ce 0.845 G 0.005 Ca 0.15 O 1.8475 After the catalytic layer, Fig.15 (b) shows that the battery exhibits excellent performance stability during the first 16 hours of operation at 300 mA / cm 2 At a current density of 1.5 Å, the voltage decay rate was only 1.8 mV / h. After adding the catalyst in-situ activation treatment (redox: 15 mL / min was introduced into the battery anode for 5 minutes), the comprehensive voltage decay was reduced to 1.1 mV / h, and the battery voltage decay rate was reduced by 39%. This result confirms the role of catalyst in-situ activation in promoting battery stability.

[0126] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A catalyst for hydrocarbon fuels, characterized in that: The catalyst is a metal-ceramic catalyst, and its molecular formula is Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ , where 0.001≤m≤0.5, 0.005≤x≤0.20, 0.01≤y≤0.15, 1.75≤δ≤1.99; The catalyst is composed of a ceramic substrate and has a self-supporting property; the catalyst has a porous structure with a pore size of 1-20 μm.

2. The catalyst according to claim 1, characterized in that The molecular formula of the catalyst is Ni 0.999 Mo 0.001 / Ce 0.845 Gd 0.005 Ca 0.15 O 1.8475 、Ni 0.85 Mo 0.15 / Ce 0.855 Gd 0.095 Ca 0.05 O 1.9025 或Ni 0.5 Mo 0.5 / Ce 0.79 Gd 0.2 Ca 0.01 O 1.89 。 3. The catalyst according to claim 1 or 2, characterized in that The Ni in the catalyst 1-m Mo m The content is 2-12wt%.

4. The method for preparing the catalyst according to any one of claims 1 to 3, characterized in that: The following steps are involved: Preparation of ceramic materials: Weighing a cerium source, a gadolinium source, and a calcium source and mixing them with a solvent to obtain a mixture; The mixture is heated, ball-milled and calcined to obtain Ce 1-x-y G x Ca y O 2-δ Ceramic materials; Ceramic support preparation: Ce 1-x-y G x Ca y O 2-δ Ceramic materials and pore-forming agents are ball-milled and calcined to obtain porous Ce 1-x-y G x Ca y O 2-δ Ceramic support; Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ Catalyst preparation: The Ni source and the Mo source are prepared into Ni-containing 2+ Solutions and Mo-containing 6+ of solution; Ni 2+ Solution and Mo 6+ Solution immersed in Ce 1-x-y G x Ca y O 2-δ The catalyst is calcined in a ceramic support.

5. The preparation method according to claim 4, characterized in that: In the preparation process of the ceramic material, the cerium source is selected from cerium nitrate or cerium acetate, the gadolinium source is selected from gadolinium nitrate or gadolinium acetate, and the calcium source is selected from calcium nitrate or calcium acetate; the solvent is a polyvinyl alcohol aqueous solution with a concentration of 5-8wt%.

6. The preparation method according to claim 4, characterized in that: During the preparation of the ceramic material, the mixture is heated at a temperature of 100-300° C., the ball milling medium is anhydrous ethanol, the ball milling time is 12-48 hours, the calcination temperature is 700-1000° C., and the calcination time is 1-3 hours.

7. The preparation method according to claim 4, characterized in that: In the process of preparing the ceramic support, the pore-forming agent is selected from polymethyl methacrylate, carbon powder or starch, the calcination temperature is 1300-1500° C., and the calcination time is 3-5 hours.

8. The preparation method according to claim 4, characterized in that: Ni 1-m Mo m / Ce 1-x-y G x Ca y O 2-δ During the catalyst preparation process, the Ni source is selected from Ni(NO3)2·6H2O or nickel acetate, and the Mo source is selected from (NH4)6Mo7O 24 6H2O; Ni 2+ Solution and Mo 6+ The solution was impregnated into Ce by vacuum impregnation 1-x-y G x Ca y O 2-δ Ceramic support; calcination temperature is 500-700°C, and calcination time is 0.2-5h.

9. A battery anode, characterized in that: The battery anode comprises an anode layer and the catalyst according to any one of claims 1 to 3.

10. A single battery, characterized in that: The single cell comprises the battery anode of claim 9.