A fullerene powder material and its preparation method and application

By mixing fullerene and mesoporous dispersion materials to prepare fullerene powder materials, the problem of limited use of fullerene composite materials in cosmetics in the existing technology is solved, and its effective application and stability in cosmetics are achieved. , significantly improves the antioxidant and whitening effects.

CN114948762BActive Publication Date: 2024-10-11SUZHOU RENSHENG ZEFA BIOTECHNOLOGY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111681972.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-10-11
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

The existing preparation methods of fullerene composite materials cannot fully exert their efficacy, and their use in cosmetics is limited, especially the limited solubility of C60 and the hindrance of compounding with polymer compositions.

Method used

Using the preparation method of fullerene powder materials, by mixing fullerene with mesoporous dispersion materials such as silica or titanium dioxide, and after stirring, centrifugation and washing steps, a powder with a fullerene content of 0.01%-10% is prepared. Bulk materials with particle sizes from 0.1μm to 10μm for applications in cosmetics.

Benefits of technology

It achieves the effective dispersion and stable presence of fullerene in cosmetics, significantly improves its antioxidant, free radical scavenging and ultraviolet absorption properties, enhances the whitening and protective effects of cosmetics, and at the same time improves the stability and performance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114948762B_ABST
    Figure CN114948762B_ABST
Patent Text Reader

Abstract

The present disclosure relates to a fullerene powder material and a preparation method thereof. The fullerene powder material comprises fullerene and a dispersion material. The present disclosure also relates to a powder material for cosmetics or a cosmetic comprising the fullerene powder material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of material chemistry, and in particular to a method for preparing a fullerene powder material, and a compounding method and application thereof with other raw materials. Background Art

[0002] In 1985, scientists Kroto, Smalley, Curl and others discovered C60 fullerene while studying carbon in deep space. In 1996, the three won the Nobel Prize in Chemistry for this. Fullerene, diamond and graphite are allotropes of carbon. C60 is a spherical molecule composed of 60 carbon atoms, consisting of 12 pentagons and 20 hexagons. Each carbon atom forms a bond with three adjacent carbon atoms through SP2 hybridization. It is called soccerene because of its soccer-like shape.

[0003] The large π-bond conjugated system composed of multiple P orbitals of fullerene makes it have a strong ability to accept electrons. Due to its unique structure and physical and chemical properties, it has excellent free radical scavenging performance and is called a "free radical sponge". It also exhibits excellent antioxidant properties, making it widely concerned in cosmetic materials, biomedicine, etc.

[0004] By embedding C60 into surfactants, C60 can still eliminate reactive oxygen species in cells, inhibit mitochondrial depolarization, activation of cysteine ​​proteases, exposure of phosphatidylserine on cell membranes, and DNA fission, and C60 has shown the effect of protecting cells from oxidative apoptosis. C60 liposome complexes play an antioxidant role by defending against UVA damage to skin structure, cell nuclei and collagen fibers, and penetration into human skin tissue. It is hundreds of times more potent than vitamin C and can quench free radicals. Fullerene, as a non-polar molecule, has a strong ability to absorb ultraviolet rays and can remove free radicals generated by the skin, thereby playing an anti-photodamage and whitening role.

[0005] Professor Fathi Moussa has been engaged in the research of C60 for a long time. As the first person to dissolve fullerene in olive oil for research, they fed mice once every two weeks for 10-17 months (4 mg of fullerene per kg of body weight). The control group mice died at 17-38 months, while the life span of the experimental group was extended to 59-66 months. They found that fullerene has the function of longevity and health care. During this period, there was no abnormality in body weight and physiological performance. C60 was not found to be toxic and bio-genetic. On the contrary, a certain amount of C60 has the ability to scavenge free radicals, thus protecting animals from the harm of excessive free radicals.

[0006] As external products, patents have reported fullerene-related products, such as C60-PVP, application number: 200480005008.1, 200580049615.2. Due to the preparation process and the composite characteristics of PVP and C60, the content of C60 in the composite does not exceed 1%. 201810871219.7, due to the compounding with the polymer composition, excessive application on the surface of the skin will have a certain hindering effect on the efficacy of certain cosmetics. C60-squalane, application number 201510427642.4, but the solubility of C60 in squalane is limited, and squalane is an oil solution, which limits the use of this series of products.

[0007] In the preparation of fullerene composite materials, existing commercially available products cannot fully exert the efficacy of fullerene composite products, nor can they effectively combine fullerene composite products, and they are prone to phase separation. Summary of the invention

[0008] In order to solve the problems existing in the above-mentioned prior art, the purpose of the present disclosure is to provide a fullerene powder material and a preparation method thereof, wherein the fullerene powder material comprises fullerene and a dispersion material. The fullerene powder material is directly added as a raw material during use without modification or optimization.

[0009] The present disclosure also aims to provide a powder material for cosmetics comprising the fullerene powder material of the present disclosure, and use thereof in preparing cosmetics.

[0010] In one aspect of the present disclosure, a fullerene powder material is provided, wherein the fullerene powder material comprises fullerene and a dispersion material.

[0011] In one aspect of the present disclosure, the fullerene is selected from C 60 Fullerene, C 70 One or more of fullerenes or metallofullerenes.

[0012] In one aspect of the present disclosure, the dispersed material comprises a mesoporous dispersed material.

[0013] In one aspect of the present disclosure, the mass ratio of the fullerene to the dispersed material is 0.01%-10%.

[0014] In another aspect of the present disclosure, the mass ratio of the fullerene to the dispersed material is 0.01%-5%.

[0015] In another aspect of the present disclosure, the mass ratio of the fullerene to the dispersed material is 0.01%-2%.

[0016] In one aspect of the present disclosure, the dispersing material is selected from one or more of silicon dioxide, titanium dioxide, talc, mica, sericite, and kaolin.

[0017] In one aspect of the present disclosure, the dispersed material is selected from one or more of mesoporous silica, mesoporous titanium dioxide, talc, and sericite.

[0018] In another aspect of the present disclosure, the silica is mesoporous silica.

[0019] In another aspect of the present disclosure, the titanium dioxide is mesoporous titanium dioxide.

[0020] In one aspect of the present disclosure, the particle size of the fullerene powder material is 0.1 μm to 10 μm.

[0021] In another aspect of the present disclosure, the particle size of the fullerene powder material is 0.5 μm to 5 μm.

[0022] A fullerene powder material for cosmetics, characterized in that the fullerene powder material comprises fullerene and silicon dioxide and / or titanium dioxide.

[0023] A fullerene powder material for cosmetics, characterized in that the fullerene powder material comprises fullerene and mesoporous silica and / or mesoporous titanium dioxide.

[0024] In one aspect of the present disclosure, a method for preparing a fullerene powder material is provided, the method comprising the steps of preparing a dispersion material and mixing the dispersion material with a fullerene solution.

[0025] In one aspect of the present disclosure, a method for preparing a fullerene powder material is provided, the preparation method comprising the following steps:

[0026] S1: preparing dispersed material;

[0027] S2: mixing the dispersed material with the fullerene solution, stirring and centrifuging to obtain a precipitate and a supernatant;

[0028] S3: adding the fullerene solution to the supernatant again, repeating the stirring and centrifugation steps until the supernatant becomes colorless to obtain a precipitate;

[0029] S4: washing the precipitate obtained in S2 and the precipitate obtained in S3 to obtain a total precipitate;

[0030] S5: drying and dehydrating the total precipitate to obtain the fullerene powder material.

[0031] In a specific embodiment of the present disclosure, the dispersed material comprises a mesoporous dispersed material.

[0032] In a specific embodiment of the present disclosure, the dispersed material comprises mesoporous silica and / or mesoporous titania.

[0033] In a specific embodiment of the present disclosure, the mesoporous silica and / or mesoporous titania is prepared by a hydrothermal method.

[0034] In a specific embodiment of the present disclosure, the preparation method comprises the following steps:

[0035] S1: preparing mesoporous silica and / or mesoporous titania by a hydrothermal method in the device;

[0036] S2: mixing the mesoporous silica and / or mesoporous titanium dioxide with the fullerene solution, stirring and centrifuging to obtain a precipitate and a supernatant;

[0037] S3: adding the fullerene solution to the supernatant again, repeating the stirring and centrifugation steps until the supernatant becomes colorless to obtain a precipitate;

[0038] S4: washing the precipitate obtained in S2 and the precipitate obtained in S3 to obtain a total precipitate;

[0039] S5: drying and dehydrating the total precipitate to obtain the fullerene powder material.

[0040] In one aspect of the present disclosure, in step S1, the equipment is selected from one or more of a glass reactor or a stainless steel reactor.

[0041] In one aspect of the present disclosure, in step S1, the temperature of the heating process of the hydrothermal method is selected from 10°C, 20°C, 40°C, 60°C, 80°C, 100°C, and 120°C.

[0042] In another aspect of the present disclosure, in step S1, the temperature of the heating process of the hydrothermal method is 60°C.

[0043] In another aspect of the present disclosure, in step S1, the temperature of the heating process of the hydrothermal method is 120°C.

[0044] In one aspect of the present disclosure, in step S1, the heating time of the hydrothermal method is selected from 1 hour, 2 hours, 4 hours, 5 hours, and 6 hours.

[0045] In another aspect of the present disclosure, in step S1, the heating process of the hydrothermal method is carried out for 4 hours.

[0046] In another aspect of the present disclosure, in step S1, the heating process of the hydrothermal method is carried out for 5 hours.

[0047] In another aspect of the present disclosure, in step S2 and step S3, the stirring rate of the stirring process is selected from 500 r / min, 750 r / min, 1000 r / min, and 1500 r / min.

[0048] In another aspect of the present disclosure, in step S2 and step S3, the stirring rate of the stirring process is selected from 1000 r / min to 1500 r / min;

[0049] In one aspect of the present disclosure, in step S2 and step S3, the centrifugal device is selected from one or more of a tubular centrifuge, a plate filter or a desktop filter.

[0050] In one aspect of the present disclosure, in step S6, the drying equipment is selected from one or more of a rotary evaporator, a freeze dryer, a spray dryer or a thin film evaporator.

[0051] In one aspect of the present disclosure, a fullerene powder material is provided, characterized in that it is prepared by any of the aforementioned preparation methods.

[0052] In one aspect of the present disclosure, a powder material for cosmetics is provided, characterized in that it comprises the fullerene powder material described in the present disclosure.

[0053] In one aspect of the present disclosure, a powder material for cosmetics is provided, wherein the powder material further comprises other auxiliary materials for cosmetics.

[0054] In one aspect of the present disclosure, the cosmetic auxiliary material is selected from one or more of mica powder, titanium dioxide, talc, sericite powder, silica, etc.

[0055] In one aspect of the present disclosure, the weight percentage of the fullerene powder material to the cosmetic auxiliary material is 1:200 to 1:1.

[0056] In another aspect of the present disclosure, the weight percentage of the fullerene powder material to the cosmetic auxiliary material is 1:100 to 1:5.

[0057] In one aspect of the present disclosure, the present disclosure provides uses of the fullerene powder material and the powder material for cosmetics in preparing cosmetics.

[0058] In another aspect of the present disclosure, there is provided a use of any of the aforementioned fullerene powder materials in preparing cosmetics.

[0059] In another aspect of the present disclosure, there is provided use of any of the aforementioned powder materials for cosmetics in preparing cosmetics.

[0060] In one aspect of the present disclosure, the cosmetic includes, but is not limited to, any dosage form of solutions, suspensions, emulsions, ointments, gels, creams, lotions, powders, soaps, surfactant-containing cleansers, oils, powder foundations, lotions, foundations, wax-based foundations, sprays, liniments, pastes, and poultices.

[0061] In another aspect of the present disclosure, the cosmetic includes, for example, loose powders, creams, composite emulsions, anhydrous compositions, aqueous dispersions, oils, emulsions, balms, foams, lotions, gels, cream gels, hydroalcoholic solutions, hydroglycolic solutions, liniments, saline solutions, soaps, shampoos, conditioners, serums, ointments, mousses, ointments, powders, sticks, pens, sprays, aerosols, capsules, gelatin capsules, tablets, sugar-coated tablets, powders, granular forms, chewing gums, solutions, suspensions, emulsions, syrups, polysaccharide films, jellies, gelatin, Ointments, creams, softening lotions, nourishing lotions, facial masks, essences, hair growth agents, shampoos, rinses, conditioners, hair care agents, gels, skin lotions, skin softeners, toners, astringents, lotions, milk lotions, moisturizing lotions, nourishing lotions, massage creams, nourishing creams, moisturizing creams, hand creams, foundation creams, nourishing essences, sunscreens, soaps, cleansing foams, cleansing milks, cleansing creams, body lotions and body cleansers, eye bag removers, makeup foundations, makeup removing washes, makeup removing lotions, eye shadows, lipsticks, lip glosses and lip powders.

[0062] In another aspect of the present disclosure, the efficacy of the beauty or cosmetic products includes but is not limited to: at least one of skin whitening, improving pigmentation, treating acne, improving wrinkles, improving rough skin, improving oily skin, improving dry skin, shrinking pores, treating scars, treating facial flushing, treating hair loss, promoting hair growth, treating burns, sterilizing the skin, killing skin mites, improving skin pits, anti-acne, and preventing haze.

[0063] In one aspect of the present disclosure, the material of the present disclosure can also be used together with other auxiliary materials, including hyaluronic acid, oils, surfactants, preservatives, fragrances, adhesives, thickeners, complexing agents, and pH regulators.

[0064] In one aspect of the present disclosure, the material of the present disclosure can be used together with a surfactant, wherein the surfactant is selected from at least one of anionic surfactants, cationic surfactants, amphoteric surfactants, lipophilic nonionic surfactants, hydrophilic nonionic surfactants, and natural surfactants. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 The electron paramagnetic resonance (EPR) spectrum of the fullerene powder material disclosed in the present invention for quenching hydroxyl radicals.

[0066] Figure 2This is a photo of the fullerene powder material disclosed in the present invention after ultrasonic treatment.

[0067] Figure 3 This is a photo of an existing product (Veil Fullerene from Mitsubishi, Japan) after ultrasonic treatment.

[0068] Figure 4 This is the ultraviolet absorption spectrum of the fullerene powder material disclosed in the present invention.

[0069] Figure 5 This is a photo showing the antioxidant capacity of the fullerene powder material disclosed in the present invention.

[0070] Figure 6 This is a scanning electron microscope image of the fullerene powder material disclosed in the present invention. DETAILED DESCRIPTION

[0071] According to the above contents of the present disclosure, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present disclosure, other various forms of modifications, replacements or changes may be made.

[0072] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0073] I. Implementation Methods

[0074] In one embodiment, a fullerene powder material is provided, wherein the fullerene powder material comprises fullerene and a dispersion material.

[0075] In one embodiment, wherein the fullerene is selected from C 60 Fullerene, C 70 One or more of fullerenes or metallofullerenes.

[0076] In one embodiment, the dispersed material comprises a mesoporous dispersed material.

[0077] In one embodiment, the mass ratio of the fullerene to the dispersed material is 0.01% to 10%.

[0078] In one embodiment, the mass ratio of the fullerene to the dispersed material is 0.01% to 5%.

[0079] In one embodiment, the mass ratio of the fullerene to the dispersed material is 0.01%-2%.

[0080] In one embodiment, the dispersed material is selected from one or more of silicon dioxide, titanium dioxide, talc, mica, sericite, and kaolin.

[0081] In one aspect of the present disclosure, the dispersed material is selected from one or more of mesoporous silica, mesoporous titanium dioxide, talc, and sericite.

[0082] In one embodiment, the silica is mesoporous silica.

[0083] In one embodiment, the titanium dioxide is mesoporous titanium dioxide.

[0084] In one embodiment, the particle size of the fullerene powder material is 0.1 μm to 10 μm.

[0085] In one embodiment, the particle size of the fullerene powder material is 0.5 μm to 5 μm.

[0086] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising a process of controlling a mixed solution to react at different reaction temperatures.

[0087] In one embodiment, the reaction temperature of the mixed solution is 10°C, 20°C, 40°C, 60°C, 80°C, 100°C, 120°C, preferably 60°C or 120°C.

[0088] In one embodiment, the reaction time of the mixed solution is 1 hour, 2 hours, 4 hours, 5 hours, 6 hours, preferably 4 hours or 5 hours.

[0089] In one embodiment, the mixed solution is reacted in an apparatus such as a glass reactor or a stainless steel reactor.

[0090] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising subjecting a mixed liquid to multiple high-speed centrifugation processes in a device to obtain a mesoporous dispersed material precipitate.

[0091] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising mixing the mesoporous dispersed material precipitate with a fullerene solution, stirring the mixture, and then centrifuging the mixture to obtain a precipitate and a supernatant.

[0092] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising adding the fullerene solution to the supernatant again, stirring and centrifuging until the supernatant becomes colorless to obtain a precipitate.

[0093] In one embodiment, the stirring rate of the stirring process is 500 r / min, 750 r / min, 1000 r / min, 1500 r / min; preferably 1000 r / min to 1500 r / min.

[0094] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising a process of washing the obtained precipitate with ethanol.

[0095] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising drying the washed precipitate to obtain the fullerene powder material.

[0096] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising the following steps:

[0097] S1: preparing mesoporous silica and / or mesoporous titania by a hydrothermal method in the device;

[0098] S2: mixing the mesoporous silica and / or mesoporous titanium dioxide with the fullerene solution, stirring and centrifuging to obtain a precipitate and a supernatant;

[0099] S3: adding the fullerene solution to the supernatant again, repeating the stirring and centrifugation steps until the supernatant becomes colorless to obtain a precipitate;

[0100] S4: washing the precipitate obtained in S2 and the precipitate obtained in S3 to obtain a total precipitate;

[0101] S5: drying and dehydrating the total precipitate to obtain the fullerene powder material.

[0102] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising the following steps:

[0103] S1: Mix the silicon-containing raw material, short-chain alcohol and water, heat them to 60°C in the equipment, and stir them at a rate of 1000 r / min for 4 hours until no precipitation is generated to obtain a mixed solution;

[0104] S2: obtaining a dispersed material by subjecting the mixed solution to multiple high-speed centrifugal processes in a device;

[0105] S3: After the dispersed material and the fullerene solution are mixed, a stirring process is performed at a stirring rate of 1000 r / min for a stirring time of 2 hours, and then a centrifugal process is performed to obtain a precipitate and a supernatant;

[0106] S4: adding the fullerene solution to the supernatant again, stirring at a rate of 1000 r / min, and centrifuging until the supernatant becomes colorless to obtain a precipitate;

[0107] S5: washing the precipitate obtained in S3 and the precipitate obtained in S4 with ethanol;

[0108] S6: Drying the washed precipitate to obtain a titanium dioxide fullerene material.

[0109] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising the step of preparing mesoporous silica. Preferably, the preparation of mesoporous silica comprises a process of mixing a silicon-containing raw material such as ethyl orthosilane with water and different short-chain alcohols to form a mixed solution.

[0110] In one embodiment, the short-chain alcohol is selected from ethanol, butanediol, propylene glycol, isopropanol, n-hexane, pentanediol, preferably isopropanol.

[0111] In one embodiment, the present disclosure provides a method for preparing a fullerene powder material, the preparation method comprising the following steps:

[0112] S1: Mix the titanium-containing raw material and water, heat to 120°C in the equipment, react for 5 hours, and obtain a dispersed material after cooling;

[0113] S2: After the dispersed material and the fullerene solution are mixed, a stirring process is performed at a stirring rate of 1000 r / min, and then a centrifugal process is performed to obtain a precipitate and a supernatant;

[0114] S3: adding the fullerene solution to the supernatant again, stirring at a rate of 1000 r / min, and centrifuging until the supernatant becomes colorless to obtain a precipitate;

[0115] S4: washing the precipitate obtained in S3 and the precipitate obtained in S4 with ethanol;

[0116] S5: Drying the washed precipitate to obtain a titanium dioxide fullerene material.

[0117] In one aspect, the present disclosure provides a fullerene powder material, characterized in that it is prepared by any of the aforementioned preparation methods.

[0118] In one embodiment, the present disclosure provides a powder material for cosmetics, which comprises the fullerene powder material described above.

[0119] In one embodiment, the present disclosure provides a powder material for cosmetics, wherein the powder material for cosmetics further comprises other cosmetic auxiliary materials.

[0120] In one embodiment, the present disclosure provides a powder material for cosmetics, wherein other cosmetic auxiliary materials contained in the powder material for cosmetics are selected from one or more of mica powder, titanium dioxide, talcum powder, sericite powder, silica and silicon-treated powder.

[0121] In one embodiment, the present disclosure provides a loose powder material, in which the weight percentage of the fullerene powder material to other cosmetic auxiliary materials is 1:200 to 1:1.

[0122] In one embodiment, the present disclosure provides use of fullerene powder materials in the preparation of cosmetics.

[0123] In one embodiment, the cosmetic includes, but is not limited to, any dosage form of solutions, suspensions, emulsions, ointments, gels, creams, lotions, powders, soaps, surfactant-containing cleansers, oils, powder foundations, lotions, foundations, wax-based foundations, sprays, liniments, pastes, and poultices, such as loose powders, creams, composite emulsions, anhydrous compositions, aqueous dispersions, oils, emulsions, balms, foams, lotions, gels, cream gels, hydroalcoholic solutions, hydroglycolic solutions, liniments, saline solutions, soaps, shampoos, conditioners, serums, ointments, mousses, ointments, powders, sticks, pens, sprays, aerosols, capsules, gelatin capsules, tablets, sugar-coated tablets, powders, granular forms, chewing gum, solutions, suspensions, emulsions, syrups, polysaccharide films, jelly, gelatin, ointments, creams, softening lotions, nutritional lotions, facial masks , essence, hair growth agent, shampoo, rinse, conditioner, hair care agent, gel, skin lotion, skin softener, toner, astringent, lotion, milk lotion, moisturizing lotion, nutrient lotion, massage cream, nutrient cream, moisturizing cream, hand cream, foundation cream, nutrient essence, sunscreen, soap, cleansing foam, cleansing milk, cleansing cream, body lotion and body cleanser, eye bag remover, makeup foundation, makeup remover wash, makeup remover lotion, eye shadow, lipstick, lip gloss and lip powder; the effects of the beauty or cosmetic products include but are not limited to: skin whitening, improving pigmentation, treating acne, improving wrinkles, improving rough skin, improving oily skin, improving dry skin, shrinking pores, treating scars, treating facial flushing, treating hair loss, promoting hair growth, treating burns, skin sterilization, skin mite killing, improving skin pits, anti-acne, and anti-haze.

[0124] In one embodiment, the material of the present disclosure can also be used together with other auxiliary materials, including hyaluronic acid, oils, surfactants, preservatives, fragrances, adhesives, thickeners, complexing agents, and pH regulators.

[0125] In one embodiment, the material of the present disclosure can be used together with a surfactant selected from at least one of anionic surfactants, cationic surfactants, amphoteric surfactants, lipophilic nonionic surfactants, hydrophilic nonionic surfactants, and natural surfactants.

[0126] II. Embodiment

[0127] The present disclosure is further explained below with reference to examples. The description of specific exemplary embodiments of the present disclosure is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present disclosure to the precise form disclosed, and it is clear that many changes and variations can be made according to the teachings of this application specification. The purpose of selecting and describing exemplary embodiments is to explain the specific principles of the present disclosure and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present disclosure and various different selections and changes.

[0128] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0129] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0130] Example 1: Preparation of fullerene powder material disclosed herein

[0131] Mixing tetraethyl orthosilicate, isopropanol and water, controlling the temperature at 60° C. in the device, stirring for 4 hours to obtain a mixed solution; and obtaining a mesoporous silica precipitate by centrifuging the mixed solution at high speed multiple times in the device;

[0132] The mesoporous silica precipitate is mixed with the fullerene solution, stirred at a rate of 500 r / min, and then centrifuged to obtain a precipitate and a supernatant;

[0133] The precipitate was taken out, and the fullerene solution was added to the supernatant again, and the mixture was stirred at a rate of 1500 r / min and then centrifuged until the supernatant became colorless to obtain a precipitate;

[0134] The precipitate obtained in the two steps is washed with ethanol, and the washed precipitate is dried to obtain silica fullerene.

[0135] Example 2: Preparation of fullerene powder material disclosed herein

[0136] After taking 200mL of tetrabutyl titanate with a measuring tube and pouring it into the inner lining of the reactor, take 2L of distilled water at a volume ratio of 1:10, pour the distilled water into the inner lining and mix with tetrabutyl titanate, and then put it into the oven. The reaction temperature is 120℃ and the reaction time is 5h. After the sample is cooled naturally, it is cooled with distilled water and anhydrous ethanol to obtain the mesoporous titanium dioxide material;

[0137] The mesoporous titanium dioxide material and the fullerene solution are mixed, stirred at a rate of 1000 r / min, and then centrifuged to obtain a precipitate and a supernatant;

[0138] The precipitate was taken out, and the fullerene solution was added to the supernatant again, and the mixture was stirred at a rate of 1000 r / min and then centrifuged until the supernatant became colorless to obtain a precipitate;

[0139] The precipitate obtained in the two steps is washed with ethanol, and the washed precipitate is dried to obtain titanium dioxide fullerene.

[0140] Example 3: Preparation of fullerene powder material disclosed herein

[0141] After 100 mL of tetra-n-butyl titanate was measured with a measuring tube and poured into the inner lining of the reactor, 1 L of distilled water was measured at a volume ratio of 1:5, the distilled water was poured into the inner lining and the mixture of tetra-n-butyl titanate was put into an oven, the reaction temperature was 120°C and the reaction time was 4 h. After the sample was naturally cooled, it was cooled with distilled water and anhydrous ethanol to obtain a mesoporous titanium dioxide material;

[0142] The mesoporous titanium dioxide material, talc powder and fullerene solution are mixed, stirred at a rate of 1000 r / min and then centrifuged to obtain a precipitate and a supernatant;

[0143] The precipitate was taken out, and the fullerene solution was added to the supernatant again, and the mixture was stirred at a rate of 1500 r / min and then centrifuged until the supernatant became colorless to obtain a precipitate;

[0144] The precipitate obtained in the two steps is washed with ethanol, and the washed precipitate is dried to obtain composite powder fullerene.

[0145] Example 4: Preparation of fullerene powder material disclosed herein

[0146] Mixing tetraethyl orthosilicate, n-butanol and water, controlling the temperature at 60° C. in the device, stirring for 2 hours to obtain a mixed solution; and obtaining a mesoporous silica precipitate by centrifuging the mixed solution at high speed multiple times in the device;

[0147] After mixing the mesoporous silica, talc, sericite and fullerene solution, stirring at a rate of 1500 r / min and then centrifuging to obtain a precipitate and a supernatant, the precipitate is taken out;

[0148] Add the fullerene solution to the supernatant again, continue stirring at a rate of 1500 r / min and then centrifuge until the supernatant becomes colorless to obtain a precipitate;

[0149] The precipitate obtained in the two steps is washed with ethanol, and the washed precipitate is dried to obtain composite powder fullerene.

[0150] Example 5: Free radical quenching experiment of fullerene powder material disclosed in the present invention

[0151] Electron paramagnetic resonance (EPR) test was used to detect the quenching effect of fullerene powder materials.

[0152] Experimental principle: Under ultraviolet (UV) irradiation, H2O2 generates a large number of hydroxyl radicals, which are immediately captured by DMPO to generate DMPO-OH, which is detected by electron paramagnetic resonance (EPR). The spin capture method uses the short-lived free radicals and a special compound to generate relatively stable free radicals, so that the short-lived free radicals can be detected by the ESR method.

[0153] 1. Preparation of DMPO solution: add 5.5 μL DMPO stock solution to 250 μL ultrapure water;

[0154] 2. Sample preparation: Take 20 mg of the product of Example 1 and the reference substance (VeilFullerene, a product of Mitsubishi, Japan) and add 1000 μL of ultrapure water for ultrasonic dispersion. Immediately take 25 μL of the mixed solution and mix it evenly with 25 μL of H2O2 (100 mM), and then add 10 μL of DPMO solution.

[0155] 3. Irradiate the solution under 500 W UV light for 4 min, and then record the X-band EPR spectrum in the dark.

[0156] Conclusion: If Figure 1 As shown, it can be observed that the fullerene powder material disclosed in the present invention has an obvious free radical quenching effect, which is stronger than the free radical quenching effect of the reference product. It also confirms that only fullerene that can be dispersed in water can play the role of quenching free radicals.

[0157] Example 6: Stability test and hydrophilicity test of the fullerene powder material disclosed in the present invention

[0158] Take 1.25g of the product of Example 2 and the reference substance (Veil Fullerene, a product of Mitsubishi, Japan) respectively, add 25g of deionized water into a 100mL volumetric flask, shake well; put it into an ultrasonic machine for 30 minutes, let it stand after ultrasonication, and observe the state of the solution. The product of Example 2 and its stability are as follows: Figure 2 As shown, the reference product and its stability are as follows Figure 3 shown.

[0159] 20 ml of toluene solution was added to two conical flasks respectively, the precipitated substance was extracted, rotary evaporated, and weighed to finally obtain the weight of the precipitate.

[0160] Conclusion: If Figure 2-3 As shown, due to the strong ultrasonic effect, the fullerene in the product can be separated from other auxiliary materials, and the fullerene separation material disclosed in the present invention can be evenly and stably dispersed in water, the solution is beige, and no fullerene is found in the solution; while a large number of black particles are precipitated in the control product, and the product stability is poor. It can be seen that the fullerene material disclosed in the present invention has better hydrophilicity and stability.

[0161]

[0162] Example 7: Ultraviolet absorption experiment of the fullerene powder material disclosed in the present invention

[0163] Take 2.5g of the product of Example 4, add 50g of toluene into a 100mL volumetric flask, shake well; put it into an ultrasonic machine for 30 minutes, let it stand after ultrasonication, take the supernatant for detection, and use ultraviolet visible absorption spectroscopy (UV-Vis) to detect the absorption of ultraviolet rays by the product. The experimental results are as follows: Figure 4 shown.

[0164] Conclusion: Figure 4 It can be seen that the fullerene powder material disclosed in the present invention has a relatively good ultraviolet absorption effect, and the ultraviolet absorbance at 10 ppm reaches 0.7, which indicates that the fullerene powder material disclosed in the present invention has a strong effect of resisting ultraviolet damage.

[0165] Example 8: Antioxidation test of the fullerene powder material disclosed herein

[0166] Take 2.49g KI solid and 0.75g Example 1 or reference substance (Veil Fullerene, a product of Mitsubishi, Japan), and then add 26.76g deionized water into a 50mL beaker; use a dropper to add 3 drops of hydrogen peroxide solution to the solution, shake well, and observe the color change of the solution. The solution changes as shown in Figure 5 shown.

[0167] Conclusion: Figure 5 It can be seen that after 8 hours of dripping hydrogen peroxide, the color of the solution to which the fullerene powder material of the present disclosure was added did not change, proving that the fullerene powder material of the present disclosure still has strong antioxidant capacity after 8 hours; while the reference product has no antioxidant capacity whether it is 5 minutes or 8 hours after dripping hydrogen peroxide. It can be seen that the fullerene powder material of the present disclosure has a more excellent antioxidant capacity, and the antioxidant capacity also verifies that the fullerene powder material of the present disclosure has good dispersibility in water.

[0168] Example 9: Experiment on the waterproof and oil-proof effect of cosmetics prepared from the fullerene powder material disclosed herein

[0169] Compounding of loose powder products: The fullerene powder materials or reference substances of Examples 1-3 above were respectively compounded with 600 g of mica, 120 g of pearl powder, 10 g of lycopene, 6 g of zinc oxide, 12 g of titanium dioxide powder, 40 g of magnesium stearate, 8 g of talc, 10 g of a hydrophobic film-forming agent, and 10 g of a natural pigment to form a loose powder product.

[0170] 30 volunteers were selected and randomly divided into 3 groups, 10 in each group. The skin was first dyed with ink, and then the fullerene powder was applied to the dyed part of the skin of each group of volunteers. Then the test part was alternately washed with clean water and water containing oil, and the color of the test part was observed. Professional testers scored, with 0 points for no color and 10 points for the same color as before washing. Then the average score of each group was calculated. The darker the color of the test part, the better the waterproof and oil-proof performance of the product, and the stronger the protective effect on the skin. The test results are shown in Table 1 below.

[0171] [Table 1]

[0172]

[0173] Conclusion: The loose powder products prepared from the products of Examples 1-3 have excellent hydrophobicity and oleophobicity, and can prevent sweat or oil secreted by the skin from destroying the effects of the cosmetics prepared therefrom.

[0174] Example 10: Experimental results of cosmetics prepared from the fullerene powder material disclosed herein

[0175] Compounding of loose powder products: The fullerene powder materials or reference substances of Examples 1-3 above were respectively compounded with 550 g of mica, 100 g of pearl powder, 10 g of lycopene, 10 g of zinc oxide, 10 g of titanium dioxide powder, 40 g of magnesium stearate, 5 g of iron oxide, 8 g of talc, 10 g of hydrophobic film-forming agent, and 10 g of natural pigment to form loose powder products.

[0176] 60 volunteers aged 25-35 were selected and randomly divided into 3 groups, each with 20 volunteers. The 3 groups of volunteers used the loose powder products of Examples 1-3 respectively for 3 months, with an average of one use per day per person. A satisfaction test was conducted, in which the criteria for satisfaction with the use effect were that the foundation had good smoothness and spreadability when applied and no irritation to the skin; it felt comfortable, breathable and natural after use without dry lines; it effectively kept the makeup from coming off, and had a whitening effect after a period of use. The results of the satisfaction test are shown in Table 2 below:

[0177] [Table 2]

[0178] Samples to be tested Example 1 Example 2 Example 3 Reference Satisfaction 84% 87% 95% 76%

[0179] Conclusion: The loose powder products prepared from the fullerene powder materials of Examples 1-3 are non-irritating to the skin, have a smooth touch, good skin-fitting and breathability, good spreadability, natural makeup, and can effectively prevent makeup from coming off. Long-term use has a certain whitening effect.

[0180] Example 11: Product morphology test

[0181] The product of Example 1 was dispersed with ethanol, and then the dispersion was dipped onto a silicon wafer using a capillary. After the ethanol evaporated naturally, a scanning electron microscope test was performed. The results are as follows: Figure 6 shown.

[0182] Conclusion: The fullerene-silica composite material is spherical with a particle size of about 200nm.

[0183] The above embodiments are merely descriptions of specific implementation methods of the present disclosure, and are not intended to limit the scope of the present disclosure. Those skilled in the art may make various modifications and changes based on the prior art. Without departing from the design spirit of the present disclosure, various modifications and improvements made to the technical solutions of the present disclosure by ordinary engineering and technical personnel in this field shall all fall within the protection scope determined by the claims of the present disclosure.

Claims

1. A method for preparing a fullerene powder material, wherein: The preparation method comprises: After measuring 200 mL of tetra-n-butyl titanate with a measuring cylinder and pouring it into the inner lining of the reactor, 2 L of distilled water was measured at a volume ratio of 1:10, and the distilled water was poured into the inner lining and the tetra-n-butyl titanate, and then the mixture was put into an oven; the reaction temperature was 120°C and the time was 5 hours; after the sample was naturally cooled, it was cooled with distilled water and anhydrous ethanol to obtain a mesoporous titanium dioxide material; The mesoporous titanium dioxide material and the fullerene solution were mixed, stirred at a rate of 1000 r / min, and then centrifuged to obtain a precipitate and a supernatant; The precipitate was taken out, and the fullerene solution was added to the supernatant again, and the mixture was stirred at a rate of 1000 r / min and then centrifuged until the supernatant became colorless to obtain a precipitate; The precipitate obtained in the two steps is washed with ethanol, and the washed precipitate is dried to obtain titanium dioxide fullerene.

2. Fullerene powder material, characterized in that: Prepared according to the preparation method according to claim 1.

3. A powder material for cosmetics, characterized in that: The invention comprises the fullerene powder material according to claim 2 and cosmetic auxiliary materials.

4. The powder material for cosmetics according to claim 3, wherein: The cosmetic auxiliary material is selected from one or more of mica powder, titanium dioxide, talcum powder, sericite powder and silica.

5. The powder material for cosmetics according to claim 4, wherein: The weight percentage of the fullerene powder material to the cosmetic auxiliary material is 1:200 to 1:

1.

6. The powder material for cosmetics according to claim 4, wherein: The weight percentage of the fullerene powder material to the cosmetic auxiliary material is 1:100 to 1:

5.

7. Use of the fullerene powder material according to claim 2 or the powder material for cosmetics according to any one of claims 3 to 6 in the preparation of cosmetics.