A method for selectively leaching and recovering lithium from black powder of waste lithium iron phosphate power batteries using Acidithiobacillus ferrooxidans

Through the selective leaching and recovery method of Thiobacillus ferrooxidans, using improved 9K culture medium and pH control, the problem of lithium recovery in lithium iron phosphate batteries is solved, efficient and environmentally friendly lithium recovery is achieved, and the traditional wet The use of strong oxidants and pollution problems in the method.

CN114959304BActive Publication Date: 2024-09-24SHANGHAI SECOND POLYTECHNIC UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210298042.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-25
Publication Date
2024-09-24
Estimated Expiration
2042-03-25

AI Technical Summary

Technical Problem

Existing technology has not yet been able to effectively use microbial methods to recover lithium from the cathode material of lithium iron phosphate batteries, and traditional wet recovery requires the addition of strong oxidants, which involves high costs and risks of contamination.

Method used

Thiobacillus ferrooxidans is used for selective leaching and recovery of lithium in the black powder of waste lithium iron phosphate power batteries. Through the improved 9K culture medium and the method of controlling the pH value, the bacterial liquid itself is used to oxidize Fe2+ to Fe3+, and pass NaOH and saturated sodium carbonate precipitation achieve efficient recovery of lithium.

Benefits of technology

It achieves efficient and selective extraction of lithium, with a leaching rate of 97.5%. There is no need to add strong oxidants. It is simple to operate, low in cost, environmentally friendly, and avoids secondary pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114959304B
    Figure CN114959304B
Patent Text Reader

Abstract

The present invention discloses a method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder using Acidithiobacillus ferrooxidans. The method comprises: A.f bacterium Carry out preliminary training and improve A.f The bacterial culture that had been cultured to the logarithmic phase was inoculated into the improved 9K medium (without FeSO 4 7H 2 O) and add battery black powder to adjust the pH. Use alkali to adjust the pH to make Fe 3+ Formation of Fe(OH) 3 After filtering the precipitate, add saturated Na 2 CO 3 Li precipitates from the solution 2 CO 3 , realizing selective recovery of lithium. The advantages of the present invention are: no need to add a large amount of FeSO 4 7H 2 O, and the PO contained in lithium iron phosphate 4 3‑ It can be used as an energy source for bacteria. The method is simple to operate, has low leaching energy consumption and low cost, avoids secondary pollution, and realizes the efficient recovery of lithium from waste lithium iron phosphate power batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of microbial hydrometallurgy and relates to a method for selectively leaching and recovering lithium from black powder of waste lithium iron phosphate power batteries by utilizing Acidithiobacillus ferrooxidans. Background Art

[0002] The cathode materials of lithium-ion power batteries include lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium iron phosphate and ternary materials. Among them, lithium iron phosphate is safe, has a long life, low raw material price, is environmentally friendly and has mature technology. It is a battery material with a large stock on the market. The theoretical life of lithium iron phosphate batteries is 7 to 8 years. At present, retired lithium iron phosphate batteries account for about 65% of the total retired batteries. Large-scale lithium iron phosphate batteries will face scrapping.

[0003] Microbial recycling is achieved by utilizing the metabolic process of microorganisms. Compared with traditional industrial treatment, it is low-cost, green and environmentally friendly, and has a relatively high metal leaching rate. Microbial leaching has received increasing attention in recent years. Among them, there are relatively many studies on the leaching of metals such as lithium, nickel, cobalt, gold, and copper from electronic waste such as discarded circuit boards and waste batteries. Zhang Haojing et al. used a strain of Thiobacillus ferrooxidans with strong metal tolerance obtained through long-term screening and domestication, and used acid leaching-bioleaching process to treat the positive electrode materials of waste lithium-ion batteries. The leaching rates of Co and Ni were 99.93% and 99.46%, respectively, and the leaching rate of Cu in the negative electrode material was 99.78% (Journal of Environmental Science, 2016, 36(11):4102-4111). Niu et al. used alicyclic Bacillus as SOB (sulfur oxidizing bacteria) and acidophilic sulfur bacillus as IOB (iron oxidizing bacteria). After 30 days of mixed culture, Co and Li in waste lithium-ion batteries were leached. SOB and IOB were used as mixed culture medium, and sulfur and pyrite were inoculated respectively. The experiment showed that compared with traditional chemical leaching, it has greater potential. The process of biological leaching performance was explored at a solid-liquid ratio of 2%. The experiment showed that the maximum leaching rates of Li and Co were 89% and 72%, respectively (Chemosphere, 2014, 109: 92-98). Guo et al. used three different systems (acidophilic sulfur oxidizing Bacillus), (acidophilic ferrooxidizing Bacillus), (mixed bacterial system) to conduct leaching experiments on NCM ternary materials. The main leaching mechanism was H produced by bacteria. 2 SO 4 The contact mechanism with bacteria produces bioleaching performance, while Fe 2 +As a reducing agent, NCM can be reduced and leached (Journal of Cleaner Production, 2016, 116: 249-258). The above pH value is adjusted to make the positive electrode materials currently used in microbial leaching to recover lithium batteries all ternary materials, lithium cobalt oxide, etc., and there is no research result on the application of microbial leaching to recover lithium iron phosphate positive electrode materials. Summary of the invention

[0004] The purpose of the present invention is to provide a method for leaching and recovering lithium from waste lithium iron phosphate power battery black powder using Acidithiobacillus ferrooxidans. The present invention applies microbial leaching technology to the metal system in the battery black powder leached by Acidithiobacillus ferrooxidans, thereby improving the leaching efficiency and expanding the use of microbial leaching. In addition, the use of Acidithiobacillus ferrooxidans to leach battery black powder does not pollute the leaching system, has low processing costs, is environmentally friendly, and is easy to control. Compared with the traditional 9K culture medium for culturing Acidithiobacillus ferrooxidans, it eliminates the need to add a large amount of FeSO 4 The strains used in the present invention A. ferrooxidans This is a domesticated strain that has improved its tolerance to lithium through preliminary cultivation.

[0005] To achieve this purpose, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder by using Thiobacillus ferrooxidans, comprising the following steps: mixing lithium iron phosphate battery black powder and Thiobacillus ferrooxidans ( A. ferrooxidans ) The bacterial solution was added to the improved FeSO-free 4 7H 2 O in a conical flask with 9K culture medium, and then solid-liquid separation is performed after the reaction to obtain a leachate and a filter residue, and then NaOH solution is dropped into the leachate to adjust the pH so that Fe 3+ Formation of Fe(OH) 3 After filtering the precipitate, add saturated Na 2 CO 3 Li precipitates from the solution 2 CO 3 , to achieve the recovery of lithium in lithium-ion battery black powder.

[0007] Preferably, the lithium iron phosphate battery black powder is obtained by discharging, disassembling, crushing and sorting waste lithium iron phosphate power batteries to obtain battery black powder mixed with positive and negative electrode materials.

[0008] Preferably, the method for culturing Thiobacillus ferrooxidans to the logarithmic phase in the early stage is as follows:

[0009] Improved FeSO-free 4 7H 2O 9K medium was added to a conical flask and placed in a shaking table. Thiobacillus ferrooxidans was inoculated at an inoculation rate of 20 vol%, and waste lithium iron phosphate power battery black powder was added at a solid-liquid mass ratio of 30 g / L. The pH of the reaction system was maintained between 1.5 and 2. The culture temperature was 30°C to 35°C and the stirrer speed was 100 to 150 rpm. The culture was carried out for 1 to 3 days to allow the bacteria to enter the logarithmic phase with good bacterial activity and stress resistance, thereby improving A. ferrooxidans Tolerance to lithium.

[0010] Preferably, Thiobacillus ferrooxidans ( A. ferrooxidans ) The conditions for the leaching reaction of the bacterial solution on the black powder of the lithium iron phosphate battery are as follows:

[0011] Inoculate the bacterial solution that has been cultured to the logarithmic phase at an inoculum rate of 10 vol% to 20% into the improved FeSO-free 4 7H 2 O in a 9K culture medium; waste lithium iron phosphate power battery black powder is added, and the solid-liquid mass ratio is 20g / L-40g / L; the pH value of the reaction system is maintained between 1.5 and 2, the culture temperature is 30°C-35°C, the stirrer speed is 100-150rpm, the leaching time is 5-8 days, and the leaching solution and leaching residue are obtained by filtering and washing, respectively.

[0012] Preferably, the pH value of the reaction system is independently adjusted by adding 5 mol / L H 2 SO 4 Maintain between 1.50 and 2.

[0013] Preferably, the improved 9K medium without FeSO4·7H2O comprises: (NH 4 ) 2 SO 4 3g / L, MgSO4·7H 2 O 0.50g / L, KCl 0.10g / L, Ca(NO 3 ) 2 0.01g / L, K 2 HPO 4 0.50g / L; prepared with deionized water and 5mol / L H 2 SO 4 The pH value of the culture medium was maintained between 1.5 and 2.

[0014] Preferably, the concentration of the NaOH solution is 5-10 mol / L, and the pH of the NaOH solution is adjusted to 4.5.

[0015] Preferably, the precipitation time of adding saturated sodium carbonate is 60 to 180 minutes.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. The present invention provides an improved 9K culture medium without the need to add a large amount of FeSO 4 The iron contained in the lithium iron phosphate in the battery black powder treated by the leaching technology of Thiobacillus ferrooxidans is Fe 2+ , which can be oxidized to Fe by Thiobacillus ferrooxidans 3+ At the same time, the PO contained in lithium iron phosphate 4 3- It can also be used as an energy source for Thiobacillus ferrooxidans.

[0018] 2. The present invention provides a new technology for selectively recovering lithium from lithium iron phosphate. The traditional wet method for recovering lithium iron phosphate requires the addition of sulfuric acid and excessive strong oxidants, such as H 2 O 2 、Na 2 S 2 O 8 Compared with the traditional wet recovery, the present invention does not need to add strong oxidants, but utilizes the metabolism of Thiobacillus ferrooxidans to convert Fe in lithium iron phosphate into 2+ Oxidized to Fe 3 + .

[0019] 3. The present invention adopts a method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder using Thiobacillus ferrooxidans. The leaching rates of Li and Fe are 97.5% and 3%, respectively. This method realizes efficient and selective extraction of lithium, and is simple to operate, low in cost, low in energy consumption, and avoids secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The present invention is a process flow chart for selectively leaching and recovering lithium from waste lithium-ion battery black powder. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0022] Figure 1 The process flow chart of selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder provided by the present invention is as follows:

[0023] The waste lithium ion battery black powder involved in the present invention is specifically a black powder produced by using waste lithium ion batteries containing lithium iron phosphate in the positive electrode active material as raw materials, and the black powder mainly includes lithium iron phosphate and negative electrode carbon powder.

[0024] (1) Discharge, disassemble, crush and sort the waste lithium-ion batteries to obtain battery black powder mixed with positive and negative electrode active materials, and determine the metal and carbon content (wt.%) in the black powder.

[0025] (2) Preliminary culture of Thiobacillus ferrooxidans

[0026] Will A. ferrooxidans Inoculate into improved 9K medium (without FeSO 4 7H 2 O) was placed in a superimposed shaker, and black powder of waste lithium iron phosphate power batteries was added and cultured for 1 to 3 days to allow the bacteria to enter the logarithmic phase with good bacterial activity and stress resistance, thereby improving A. ferrooxidans Tolerance to lithium.

[0027] (3) Thiobacillus ferrooxidans selectively leaches lithium from battery black powder

[0028] The cells that have been cultured to the logarithmic phase A. ferrooxidans The bacterial suspension was inoculated into the modified 9K medium (without FeSO 4 7H 2 O) in a conical flask, and at the same time, discharge, disassemble, crush and sort the waste lithium iron phosphate power battery to obtain battery black powder mixed with positive and negative electrode materials; put the mixed conical flask into a superimposed shaking table, filter and wash after leaching for 7 days to obtain leachate and leach residue respectively. Use NaOH solution to adjust the pH of the leachate until the addition of NaOH no longer produces Fe(OH) 3 After precipitation, continue filtering and washing, separate the filtrate and the residue by vacuum filtration, wash the residue with ultrapure water, add the washing liquid to the filtrate, and measure the content of metal ions in the filtrate by ICP-OES. Calculate the leaching rate of Li and Fe.

[0029] (4) Lithium carbonate recovery

[0030] The lithium-containing filtrate and washing liquid obtained after leaching are collected, saturated sodium carbonate solution is added to precipitate lithium carbonate, filtered, washed, and dried to obtain crude lithium carbonate.

[0031] Example 1

[0032] A method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder has the following specific steps:

[0033] (1) Determination of metal and carbon content in samples

[0034] Take about 0.1g of dry sample and place it in a digestion tank, then add 6mL of concentrated hydrochloric acid, 2mL of concentrated nitric acid and 2mL of deionized water, and then place the digestion tank in a microwave digestion instrument. After digestion, the volume is fixed to 100mL and the solution is diluted 10 times and 100 times respectively. Then, the ICP-OES (ICAP700) of ThermoFisher Scientific was used to quantitatively determine the content of metal components, and the CHN-8000B carbon, hydrogen and nitrogen element analyzer of Huanuo Electronic Technology Co., Ltd. was used to measure the carbon content in the sample. The results are shown in Table 1.

[0035] Table 1 Main components of black powder from waste lithium-ion batteries

[0036]

[0037] (2) Preliminary culture of Thiobacillus ferrooxidans

[0038] Add 200 ml of improved 9K medium (without FeSO 4 7H 2 O) Add the conical flask and place it in the LYZ-D2403-D superimposed shaker of Shanghai Longyue Company. A. ferrooxidans The inoculation amount was 20%, and the waste lithium iron phosphate power battery black powder was added. The pH value of the reaction system was maintained between 1.50 and 2. The culture temperature was 30°C and the stirrer speed was 120 rpm. The culture was carried out for 3 days to make the bacteria enter the logarithmic phase with good bacterial activity and stress resistance, and improve A. ferrooxidans Tolerance to lithium. The components of the 9K medium used in the initial culture included (NH 4 ) 2 SO 4 3g / L, MgSO 4 7H 2 O 0.50g / L, KCl0.10g / L, Ca(NO 3 ) 2 0.01g / L, K 2 HPO 4 0.50g / L; prepared with deionized water and 5mol / L H 2 SO 4 Adjust the pH value of the culture medium to 1.50~2.

[0039] (3) Thiobacillus ferrooxidans selectively leaches lithium from battery black powder

[0040] The cells that have been cultured to the logarithmic phase A. ferrooxidans The bacterial solution was inoculated into the modified 9K medium (without FeSO) at an inoculum volume of 20%. 4 7H 2O) in conical flasks, each containing 50 ml of specially prepared improved 9K medium (without FeSO 4 7H 2 O), and at the same time, the waste lithium iron phosphate power battery was discharged, disassembled, crushed, and sorted to obtain battery black powder mixed with positive and negative electrode materials. 1.5g of battery black powder was weighed, and the solid-liquid mass ratio was 30g / L. H 2 SO 4 The pH value of the reaction system was maintained between 1.50 and 2. The mixed conical flask was placed in a LYZ-D2403-D superimposed shaker of Shanghai Longyue Company, the culture temperature was 30°C, the stirrer speed was 120 rpm, the leaching time was 7 days, and the leaching solution and leaching residue were obtained by filtration and washing. The pH of the leaching solution was adjusted with a 10 mol / L NaOH solution. When the pH was adjusted to 4.5, the addition of NaOH no longer produced Fe(OH) 3 After precipitation, continue filtering and washing, separate the filtrate and the residue by vacuum filtration, wash the residue with ultrapure water, add the washing liquid to the filtrate, and measure the content of metal ions in the filtrate by ICP-OES. Calculate the leaching rates of Li and Fe. The C in the black powder does not dissolve and remains in the leaching residue, so the leaching effect of C in the black powder is not considered in subsequent experiments. The leaching rates of Li and Fe are calculated to be 97.5% and 3%, respectively.

[0041]

[0042] Where: LE M : Leaching rate of metal M

[0043] C L : Concentration of metal in leachate (measured by ICP)

[0044] V L : Volume of leachate

[0045] m Z : Mass of filter residue (weighed after drying at 80°C for 24 hours)

[0046] W: mass fraction of metal in the filter residue

[0047] C Z : Metal concentration in digestion solution (measured by ICP)

[0048] m: the weight of the filter residue

[0049] The calculated leaching rates of Li and Fe are 97.5% and 3% respectively, which means that the selective leaching and efficient recovery of lithium in the black powder of waste lithium iron phosphate power batteries are achieved.

[0050] Example 2

[0051] The method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder of this embodiment is the same as that of embodiment 1 except that: in step (3), A. ferrooxidans The inoculation amount of the bacterial solution was 10%, the solid-liquid mass ratio was 40g / L, the culture temperature was 33°C, and the stirrer speed was 100rpm. The calculated leaching rates of Li and Fe were 92.13% and 3.09%, respectively, which achieved the selective leaching and efficient recovery of lithium in the black powder of waste lithium iron phosphate power batteries.

[0052] Example 3

[0053] The method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder of this embodiment is the same as that of embodiment 1 except that: in step (3), A. ferrooxidans The inoculation amount of the bacterial solution was 15%, the solid-liquid mass ratio was 20g / L, the culture temperature was 35°C, and the stirrer speed was 150rpm. The calculated leaching rates of Li and Fe were 91.62% and 2.97% respectively, which achieved the selective leaching and efficient recovery of lithium in the black powder of waste lithium iron phosphate power batteries.

[0054] Table 2 Li and Fe element leaching rates under different embodiments

[0055]

[0056] Comparative Example 1

[0057] The method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder in this comparative example is the same as that in Example 1, except that the preliminary cultivation step of Thiobacillus ferrooxidans in step (2) is omitted, and the A. ferrooxidans The bacterial liquid was inoculated into a conical flask containing improved 9K medium and mixed with black powder for culture and leaching. The leaching rates of Li and Fe were calculated to be 68.15% and 3.13%, respectively. At this time, efficient leaching of lithium could not be achieved, so the early cultivation step of Thiobacillus ferrooxidans made it possible to achieve efficient leaching of lithium in the future.

[0058] Comparative Example 2

[0059] The method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder in this comparative example is the same as that in Example 1, except that: in step (3), a 5 mol / L H 2 SO 4 The pH value of the reaction system was maintained at 1.50. Step 2 was omitted and the A. ferrooxidansThe bacterial solution was inoculated into a conical flask containing improved 9K medium and mixed with black powder for culturing and leaching. The pH was not adjusted during the process. The leaching rates of Li and Fe were calculated to be 14.79% and 3.07%, respectively. At this time, efficient leaching of lithium could not be achieved, so H2O with a concentration of 5 mol / L was used. 2 SO 4 Maintaining the pH value of the reaction system at 1.50~2 makes it possible to achieve efficient lithium leaching in the subsequent step.

[0060] Comparative Example 3

[0061] The method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder in this comparative example is the same as that in Example 1, except that: the improved 9K culture medium (without FeSO 4 7H 2 O) was replaced with traditional 9K medium, which contains (NH 4 ) 2 SO 4 3g / L, MgSO 4 7H 2 O 0.50g / L, KCl0.10g / L, Ca(NO 3 ) 2 0.01g / L, K 2 HPO 4 0.50g / L, FeSO 4 44.2 g / L; the calculated leaching rates of Li and Fe were 46.52% and 3.01% respectively. At this time, efficient leaching of lithium could not be achieved, so the improved 9K medium (without FeSO 4 7H 2 O) step is the key to the present invention.

[0062] Comparative Example 4

[0063] The method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder in this comparative example is the same as that in Example 1, except that: in step (2) (3) A. ferrooxidans The bacterial solution step was omitted, and the battery black powder was directly mixed with the improved 9K culture medium (without FeSO 4 7H 2 O) mixing and leaching. The calculated leaching rates of Li and Fe are 30.06% and 2.83% respectively. At this time, efficient leaching of lithium cannot be achieved, so A. ferrooxidans The key to the present invention is that the bacteria can achieve selective leaching and efficient recovery of lithium.

[0064] Table 3 Li and Fe element leaching rates under different embodiments

[0065]

[0066] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for selectively leaching and recovering lithium from waste lithium iron phosphate power battery black powder using Thiobacillus ferrooxidans, characterized in that: Lithium iron phosphate battery black powder and Thiobacillus ferrooxidans that have been cultured to the logarithmic phase ( A.ferrooxidans ) was added to a conical flask containing an improved 9K medium without FeSO4·7H2O for leaching reaction. After the reaction, solid-liquid separation was performed to obtain a leachate and a filter residue. NaOH solution was then dropped into the leachate to adjust the pH so that Fe 3+ Fe(OH)3 precipitate is generated, and after filtering the precipitate, saturated Na2CO3 solution is added to the filtrate to precipitate Li2CO3, thereby realizing the recovery of lithium in the black powder of lithium-ion batteries; The lithium iron phosphate battery black powder is obtained by discharging, disassembling, crushing and sorting waste lithium iron phosphate power batteries to obtain battery black powder mixed with positive and negative electrode materials; the content of iron in the lithium iron phosphate battery black powder is not less than 20wt%; The method for culturing Thiobacillus ferrooxidans to the logarithmic phase is as follows: The improved 9K medium without FeSO4·7H2O was added into a conical flask and placed in a shaking table, Thiobacillus ferrooxidans was inoculated at an inoculation rate of 20 vol%, and waste lithium iron phosphate power battery black powder was added at a solid-liquid mass ratio of 30 g / L, the pH of the reaction system was maintained between 1.5 and 2, and the culture temperature was 30°C to 35°C and the stirrer speed was 100 to 150 rpm. The culture was carried out for 1 to 3 days to allow the bacteria to enter a logarithmic phase with good bacterial activity and stress resistance, thereby improving the tolerance of Thiobacillus ferrooxidans to lithium; The conditions for the leaching reaction of lithium iron phosphate battery black powder by Thiobacillus ferrooxidans liquid are as follows: The bacterial liquid that has been cultured to the logarithmic phase is inoculated into an improved 9K medium without FeSO4·7H2O at an inoculation amount of 10vol% to 20vol%; waste lithium iron phosphate power battery black powder is added, and the solid-liquid mass ratio is 20g / L to 40g / L; the pH value of the reaction system is maintained between 1.5 and 2, the culture temperature is 30℃ to 35℃, the stirrer speed is 100 to 150rpm, the leaching time is 5-8 days, and the leaching solution and leaching residue are obtained by filtering and washing respectively; The improved 9K medium without FeSO4·7H2O includes (NH4)2SO4 3g / L, MgSO4·7H2O 0.50g / L, KCl 0.10g / L, Ca(NO3)20.01g / L and K2HPO4 0.50g / L; it is prepared with deionized water, and the pH value of the medium is maintained between 1.5 and 2 with H2SO4 at a concentration of 5mol / L; The concentration of NaOH solution is 5 ~ 10 mol / L, and the pH value of the leaching solution is adjusted to 4.5 by NaOH solution; The time for adding saturated sodium carbonate solution for precipitation is 60 to 180 minutes.