A method for preparing a high-throughput solid diffusion couple
Through the vacuum hot pressing method and mold design, the problem of multi-component diffusion couple preparation and tight interface integration is solved, and fast and energy-saving diffusion coupling preparation is achieved. It is suitable for multi-component diffusion couples and mass production, and improves experimental efficiency and analytical applicability. .
Patent Information
- Application Number
- CN202210538325.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-05-18
AI Technical Summary
Existing diffusion couple preparation methods are difficult to achieve continuous preparation of multi-element diffusion couples and tight interface bonding, and it is not easy to achieve batch production and simultaneous preparation of different types of diffusion couples, which affects subsequent phase diagram, diffusion thermodynamics and kinetic studies.
The diffusion couple is prepared using the vacuum hot pressing method. Through the design of the vacuum hot pressing mold and component materials, the plastic deformation combination of the component metals is achieved, and the heat and pressure holding time is reduced. It is suitable for the preparation of binary, ternary, and quaternary diffusion couples. , and realize batch and diffusion couple sample preparation of different materials through mold design.
The diffusion couple interface is tightly coupled, the preparation time and energy consumption are reduced, a more suitable sample is provided for thermodynamic and kinetic analysis, and the experimental efficiency and continuity of the diffusion couple sample are improved.
Smart Images

Figure CN114964990B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material science, and in particular to a method for preparing a high-throughput solid diffusion couple. Background Art
[0002] The diffusion couple method is the most efficient and reliable method for the current determination of alloy systems, especially for the determination of solid-state relationships. A single-section diffusion couple can be used to efficiently determine the relationship between the entire composition range of the system. At the same time, the diffusion coefficient of the system can be obtained by measuring the composition-distance curve of the diffusion couple. The diffusion couple method also has the characteristics of simple experimental process, high accuracy, low consumption of raw materials, and is suitable for systems with slow phase change rates. Its outstanding advantage is that it avoids the "supercooling effect" caused by the alloy method when measuring phase diagrams, which is very important for the study of solid-state phase equilibrium. Therefore, the diffusion couple method is a high-throughput method for studying phase equilibrium and diffusion coefficients.
[0003] Generally, according to the state of the diffusion couple components, the methods for preparing diffusion couples can be divided into solid / solid diffusion method, solid / liquid diffusion method and solid / gas diffusion method. According to the number of components contained in the diffusion couple, the methods for preparing diffusion couples can be divided into binary diffusion couples, ternary diffusion couples, quaternary and higher diffusion couples. For the preparation of binary diffusion couples, there are generally "bundling method", "rivet method", "rolling method", "solid-liquid dipping method" and the like. For the preparation of ternary diffusion couples, the common methods are "pin" shaped combination method, "rivet method" and "fire layer method". For the preparation of diffusion couples with four or more components, it is usually a combination of the above methods. For the above preparation methods, the difficulty is that the preparation is very difficult, and success or failure often depends on experience. Therefore, incomplete diffusion caused by loose contact and bonding between interfaces is a common problem. In addition, the above methods are not easy to achieve the problem of simultaneous batch production and preparation of different types of diffusion couples.
[0004] In view of this, the present invention provides a new method for preparing a diffusion couple to solve the above technical problems. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing a high-throughput solid diffusion couple, which can continuously prepare multi-component diffusion couples with tight interface bonding, and the prepared diffusion couples are more conducive to the subsequent research on phase diagrams, diffusion thermodynamics and kinetics.
[0006] In order to solve the above problems, the technical solution of the present invention is as follows:
[0007] A method for preparing a high-throughput solid diffusion couple comprises the following steps:
[0008] Step S1, providing a vacuum hot pressing mold, wherein the vacuum hot pressing mold comprises a female mold, a plurality of receiving grooves provided in the female mold, a lower mold fixed to the bottom of the receiving groove, an upper mold embedded in the receiving groove and slidable along the axis of the receiving groove, a limiting ring sleeved on the outside of the female mold, and a cover plate covering the limiting ring and fitting with the upper mold during operation;
[0009] Step S2, preparing a binary diffusion couple, specifically comprises the following steps:
[0010] Step S21, cutting the raw material components A and B to be used for preparing diffusion couples into the same size by using a tangent line, and the cross-sectional shape and size of the components A and B correspond to the end surface shape and size of the upper mold and the lower mold in the vacuum hot pressing mold, and the sum of the thickness of the components A and B is equivalent to their width;
[0011] Step S22, polishing the component A and component B prepared in step S21 with 600, 1000, 1500, and 2000 grit sandpapers, and then polishing with 0.3 μm diamond polishing liquid on a polishing cloth, and placing in alcohol for ultrasonic treatment for 10-20 minutes;
[0012] Step S23, placing the components A and B prepared in step S22 in the receiving grooves of the vacuum hot pressing mold in sequence, and assembling the mold, the upper mold and the lower mold to fix the components A and B;
[0013] Step S24, placing the mold assembled in step S23 on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the mold fits the pressing head;
[0014] Step S25, performing vacuum hot pressing at the plastic deformation temperature of the two components, and controlling the heat preservation time to be 50-60 minutes, the pressure holding time to be 4-6 minutes, and removing the mold after cooling, and taking out the diffusion couple sample;
[0015] Step S26, the diffusion couple sample prepared in step S25 is polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes, and then dried in a vacuum drying oven, the sample is taken out and packaged into a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes and then vacuum dried to obtain a binary diffusion couple AB that can be directly used for phase diagram determination and diffusion experiments.
[0016] Furthermore, a method for preparing a ternary diffusion couple is also provided, which specifically comprises the following steps:
[0017] Step S31, performing side line cutting on the binary diffusion couple sample prepared in step S2, so that the shape and size after cutting correspond to the end face shape and size of the upper mold and the lower mold in the vacuum hot pressing mold, and satisfying that component A and component B occupy one half of the volume of the original diffusion couple sample;
[0018] Step S32, the binary diffusion couple AB and component C obtained by cutting in step S31 are polished with 600, 1000, 1500, and 2000 mesh sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes; wherein the size of component C is the same as the size of the binary diffusion couple AB after cutting;
[0019] Step S33, assembling the binary diffusion couple AB and component C prepared in step S32 into a vacuum hot pressing mold;
[0020] Step S34, placing the mold assembled in step S23 on a pressing platform of a vacuum hot pressing furnace, so that the cover plate of the mold fits the pressing head;
[0021] Step S35, performing vacuum hot pressing at the plastic deformation temperature of the diffusion couple AB and the component C, and controlling the heat preservation time to be 50-60 minutes, the pressure holding time to be 4-6 minutes, and removing the mold after cooling to remove the diffusion couple sample;
[0022] Step S36, the diffusion couple sample prepared in step S35 is polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes, and then dried in a vacuum drying oven, the sample is taken out and packaged into a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes and then vacuum dried to obtain a ternary diffusion couple that can be directly used for phase diagram determination and diffusion experiments.
[0023] Furthermore, a method for preparing a quaternary diffusion couple is also provided, which specifically comprises the following steps:
[0024] Step S41, preparing binary diffusion couple AB and binary diffusion couple CD according to the preparation method of binary diffusion couple, and performing side line cutting on the diffusion couple samples, so that the shape and size after cutting correspond to the end face shape and size of the upper mold and the lower mold in the vacuum hot pressing mold, and satisfying that the two components each occupy one half of the volume of the original diffusion couple sample;
[0025] Step S42, the diffusion couple AB and the diffusion couple CD obtained by cutting in step S41 are polished with 600, 1000, 1500, and 2000 grit sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes;
[0026] Step S43, assembling the diffusion couple AB and the diffusion couple CD prepared in step S42 into a vacuum hot pressing mold;
[0027] Step S44, placing the mold assembled in step S43 on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the mold fits the pressing head;
[0028] Step S45, performing vacuum hot pressing at the plastic deformation temperature of the diffusion couple AB and the diffusion couple CD, and controlling the heat preservation time to be 50-60 minutes, the pressure holding time to be 4-6 minutes, and removing the mold after cooling to remove the diffusion couple sample;
[0029] Step S46, the diffusion couple sample prepared in step S45 is polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes, and then dried in a vacuum drying oven, the sample is taken out and packaged into a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing treatment, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes and then vacuum dried to obtain a quaternary diffusion couple that can be directly used for phase diagram determination and diffusion experiments.
[0030] Furthermore, the dimensions of component A and component B are 10 mm*7 mm*3.5 mm respectively.
[0031] Furthermore, in step S31, the size of the cut binary diffusion couple AB is 10 mm*7 mm*3.5 mm.
[0032] Furthermore, in the vacuum hot pressing mold, there are at least three groups of upper molds and lower molds.
[0033] Compared with the prior art, the method for preparing a high-throughput solid diffusion couple provided by the present invention has the following beneficial effects:
[0034] 1. The preparation method of the high-throughput solid diffusion couple provided by the present invention adopts the vacuum hot pressing method to prepare the diffusion couple, and the hot pressing temperature is the plastic deformation temperature of the component materials, so that the bonding is achieved through the plastic deformation of the component metals, and the diffusion couple interface is well bonded; and the bonding is achieved through plastic deformation, and the heat preservation and pressure holding time during the vacuum hot pressing process can be greatly reduced, so as to facilitate the rapid preparation of diffusion couple samples and save energy consumption; moreover, the heat preservation and pressure holding time is greatly reduced, and the prepared diffusion couple samples are more conducive to subsequent thermodynamic analysis and testing, because if the heat preservation and pressure holding time is too long, atomic diffusion occurs in the diffusion couple sample, which will affect the subsequent phase diagram, diffusion thermodynamics and kinetics research and analysis results.
[0035] Second, the method for preparing a high-throughput solid diffusion couple provided by the present invention is to design the size of the vacuum hot pressing mold and the component materials so that the sum of the thickness of component A and component B is equivalent to their width, and to achieve continuous processing of ternary diffusion couples, quaternary diffusion couples, and higher diffusion couples through subsequent sample cutting and component assembly. The method has continuity. In addition, the same process is used to complete the preparation of multi-component diffusion couples, and the method is simple and easy to operate.
[0036] 3. The method for preparing high-throughput solid diffusion couples provided by the present invention comprises a vacuum hot pressing mold including multiple sets of upper molds and lower molds, which can realize batch preparation of diffusion couple samples and simultaneously prepare diffusion couple samples of different materials, thereby effectively improving experimental efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0038] Figure 1 It is a structural schematic diagram of the vacuum hot pressing mold in the present invention;
[0039] Figure 2 for Figure 1 A schematic structural diagram of the vacuum hot pressing mold from another angle shown;
[0040] Figure 3 This is a schematic diagram of the AB component mold assembly;
[0041] Figure 4 This is a schematic diagram of the AB-C component mold assembly.
[0042] Figure 5 This is a schematic diagram of the AB-CD component mold assembly.
[0043] Figure 6This is the SEM scanning image of the diffusion interface of Co-AlCo diffusion couple. The dotted line in the figure represents the position of the line scan.
[0044] Figure 7 for Figure 6 Line scan diagram of the solid line position;
[0045] Figure 8 for Figure 6 The magnified phase composition diagram of the solid line in the middle;
[0046] Fig. 9 This is a SEM scan of the diffusion interface of the Fe-Mn-Zn ternary diffusion couple. DETAILED DESCRIPTION
[0047] In order to enable those skilled in the art to better understand the technical solutions in the embodiments of the present invention and to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are further described below.
[0048] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0049] Please refer to Figure 1 and Figure 2 ,in Figure 1 It is a structural schematic diagram of the vacuum hot pressing mold in the present invention; Figure 2 for Figure 1 A schematic structural diagram of the vacuum hot pressing mold from another angle is shown. Figure 1 The light-colored lines in the figure are dotted lines, which are invisible parts in the attached figure. In order to more intuitively show the structure of the mold, the invisible parts are presented with dotted lines. The vacuum hot pressing mold 100 used in the present invention includes a female mold 1, a plurality of receiving grooves 2 provided in the female mold 1, a lower mold 3 fixed to the bottom of the receiving groove, an upper mold 4 embedded in the receiving groove 2 and slidable along the axis of the receiving groove, a limiting ring 5 sleeved on the outside of the female mold 1, and a cover plate 6 covering the limiting ring and fitting with the upper mold during operation.
[0050] Among them, the upper mold 4 and the lower mold 3 are used to fix the fixed component materials used for preparing the diffusion couple; the function of the limit ring 5 is to regulate the deformation of the diffusion couple, and its working principle is as follows: after the mold is assembled, when the cover plate is in full contact with the upper mold, there will be a certain distance between the cover plate and the limit ring. During vacuum hot pressing preparation, the pressure head pushes the cover plate to move downward. When it moves to the height of the limit ring, since the cover plate and the limit ring are in contact, the area of the limit ring is large, and the limit ring uses H13 mold steel, which is difficult to deform, so it will limit the pressure head and the cover plate from continuing to move downward, thereby achieving control of the thickness of the diffusion couple sample.
[0051] In order to improve the preparation efficiency of diffusion couples, preferably, multiple sets of upper molds and lower molds can be set. The vacuum hot pressing mold includes multiple sets of upper molds and lower molds, which can realize batch preparation of diffusion couple samples and simultaneous preparation of diffusion couple samples of different materials. In this embodiment, there are at least three sets of upper molds and lower molds.
[0052] The preparation method of the high-throughput solid diffusion couple provided by the present invention is described in detail below in conjunction with the structure of the vacuum hot pressing mold.
[0053] Example 1
[0054] A method for preparing a binary diffusion couple comprises the following steps:
[0055] Step S1, providing a vacuum hot pressing mold, the vacuum hot pressing mold 100 includes a female mold 1, a plurality of receiving grooves 2 provided in the female mold, a lower mold 3 fixed to the bottom of the receiving groove, an upper mold 4 embedded in the receiving groove and slidable along the axis of the receiving groove, a limiting ring 5 sleeved on the outside of the female mold, and a cover plate 6 covering the limiting ring and fitting the upper mold during operation;
[0056] Step S2, preparing a binary diffusion couple, specifically comprises the following steps:
[0057] Step S21, cutting the raw material components A and B to be used for preparing diffusion couples into the same size by using a tangent line, and the cross-sectional shape and size of the components A and B correspond to the end surface shape and size of the upper mold and the lower mold in the vacuum hot pressing mold, and the sum of the thickness of the components A and B is equivalent to their width;
[0058] Step S22, polishing the component A and component B prepared in step S21 with 600, 1000, 1500, and 2000 grit sandpapers, and then polishing with 0.3 μm diamond polishing liquid on a polishing cloth, and placing in alcohol for ultrasonic treatment for 10-20 minutes;
[0059] Step S23, placing the components A and B prepared in step S22 in the receiving groove of the vacuum hot pressing mold in sequence, and assembling the mold, the upper mold and the lower mold to fix the components A and B; wherein the assembly diagram of the components A and B is as shown in Figure 3As shown;
[0060] Step S24, placing the mold assembled in step S23 on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the mold fits the pressing head;
[0061] Step S25, performing vacuum hot pressing at the plastic deformation temperature of the two components, and controlling the heat preservation time to be 50-60 minutes, the pressure holding time to be 4-6 minutes, and removing the mold after cooling, and taking out the diffusion couple sample;
[0062] Step S26, the diffusion couple sample prepared in step S25 is polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes, and then dried in a vacuum drying oven, the sample is taken out and packaged into a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes and then vacuum dried to obtain a binary diffusion couple AB that can be directly used for phase diagram determination and diffusion experiments.
[0063] Example 2
[0064] A method for preparing a ternary diffusion couple comprises the following steps:
[0065] Step S31, performing side line cutting on the binary diffusion couple sample prepared in Example 1, wherein the shape and size after cutting correspond to the end face shape and size of the upper mold and the lower mold in the vacuum hot pressing mold, and the components A and B occupy half of the volume of the original diffusion couple sample;
[0066] Step S32, the binary diffusion couple AB and component C obtained by cutting in step S31 are polished with 600, 1000, 1500, and 2000 mesh sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes; wherein the size of component C is the same as the size of the binary diffusion couple AB after cutting;
[0067] Step S33, assembling the binary diffusion couple AB and component C prepared in step S32 into a vacuum hot pressing mold; wherein the assembly diagram of the binary diffusion couple AB and component C is as shown in Figure 4 As shown;
[0068] Step S34, placing the mold assembled in step S23 on a pressing platform of a vacuum hot pressing furnace, so that the cover plate of the mold fits the pressing head;
[0069] Step S35, performing vacuum hot pressing at the plastic deformation temperature of the diffusion couple AB and the component C, and controlling the heat preservation time to be 50-60 minutes, the pressure holding time to be 4-6 minutes, and removing the mold after cooling to remove the diffusion couple sample;
[0070] Step S36, the diffusion couple sample prepared in step S35 is polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes, and then dried in a vacuum drying oven, the sample is taken out and packaged into a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes and then vacuum dried to obtain a ternary diffusion couple that can be directly used for phase diagram determination and diffusion experiments.
[0071] Example 3
[0072] A method for preparing a quaternary diffusion couple comprises the following steps:
[0073] Step S41, preparing binary diffusion couple AB and binary diffusion couple CD according to the preparation method of Example 1, and performing side line cutting on the diffusion couple samples, so that the shapes and sizes after cutting correspond to the end faces of the upper mold and the lower mold in the vacuum hot pressing mold, and satisfying that the two components each occupy one half of the volume of the original diffusion couple sample;
[0074] Step S42, the diffusion couple AB and the diffusion couple CD obtained by cutting in step S41 are polished with 600, 1000, 1500, and 2000 grit sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes;
[0075] Step S43, assembling the diffusion couple AB and the diffusion couple CD prepared in step S42 into a vacuum hot pressing mold; wherein the assembly schematic diagram of the diffusion couple AB and the diffusion couple CD is as shown in Figure 5 As shown;
[0076] Step S44, placing the mold assembled in step S43 on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the mold fits the pressing head;
[0077] Step S45, performing vacuum hot pressing at the plastic deformation temperature of the diffusion couple AB and the diffusion couple CD, and controlling the heat preservation time to be 50-60 minutes, the pressure holding time to be 4-6 minutes, and removing the mold after cooling to remove the diffusion couple sample;
[0078] Step S46, the diffusion couple sample prepared in step S45 is polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes, and then dried in a vacuum drying oven, the sample is taken out and packaged into a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing treatment, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes and then vacuum dried to obtain a quaternary diffusion couple that can be directly used for phase diagram determination and diffusion experiments.
[0079] The method for preparing the diffusion couple provided by the present invention is described below by using specific metal raw materials.
[0080] Example 4
[0081] A method for preparing a Co-AlCo diffusion couple comprises the following steps:
[0082] (1) Cutting the raw materials (pure Co, 10 at% Al-Co alloy) to be used for preparing diffusion couples into shapes of the same size (7*10*3.5 mm) by wire cutting;
[0083] (2) The pure Co and 10 at% Al-Co obtained by cutting in step (1) were polished with 600, 1000, 1500, and 2000 grit sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10 minutes;
[0084] (3) The pure Co and 10 at% Al-Co prepared in step (2) are placed in a vacuum hot pressing mold in sequence, and the assembly method is as follows: Figure 3 As shown, use the lower die with a cover of 6.5 mm and assemble the mold;
[0085] (4) placing the mold assembled in step (3) on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the assembled mold fits the pressing head;
[0086] (5) performing vacuum hot pressing on the assembled mold in step (4), with the hot pressing temperature being 500° C., the pressure being 4T, and the pressure being maintained for 4 minutes; after cooling, removing the mold and demolding, and taking out the diffusion couple sample;
[0087] (6) The diffusion couple sample prepared in step (5) is polished with 600, 1000, 1500, and 2000 mesh sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10 minutes, and then dried in a vacuum drying oven for 30 minutes, and the sample is taken out and packaged in a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing, and the annealing process is 900°C for 120 hours, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10 minutes and then vacuum dried, and can be directly used for phase diagram determination and diffusion experiment.
[0088] Please refer to Figure 6 , Figure 7 and Figure 8 ,in Figure 6 This is the SEM scanning image of the diffusion interface of Co-AlCo diffusion couple. The dotted line in the figure represents the position of the line scan. Figure 7 for Figure 6 Line scan diagram of the solid line position; Figure 8 for Figure 6 The magnified phase composition diagram of the solid line in the middle. Figure 6 , Figure 7 and Figure 8 It can be seen that the Co-AlCo diffusion couple has a good bonding interface and good diffusion occurs at the hot pressing temperature.
[0089] EPMA was used to detect Figure 8 The composition of the marked points 1-6 is measured in Table 1:
[0090] Table 1: Ratio of ingredients at each test point
[0091]
[0092]
[0093] It can be seen from the above table that a stable phase is formed at the bonding interface of the diffusion couple, indicating that the interface bonding is good.
[0094] Example 5
[0095] A method for preparing a Dy-BFe diffusion couple comprises the following steps:
[0096] (1) Cutting the raw materials (pure Dy, 5at% B-Fe alloy) to prepare diffusion couples into shapes of the same size (7*10*3.5 mm) by wire cutting;
[0097] (2) The pure Dy and 5 at% B-Fe alloy obtained by cutting in step (1) were polished with 600, 1000, 1500, and 2000 grit sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10 minutes;
[0098] (3) The pure Dy and 5at% B-Fe alloy prepared in step (2) are placed in a vacuum hot pressing mold in sequence, and the assembly method is as follows: Figure 3 As shown, use the lower die with a cover of 6.5 mm and assemble the mold;
[0099] (4) placing the mold assembled in step (3) on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the assembled mold fits the pressing head;
[0100] (5) performing vacuum hot pressing on the assembled mold in step (4), with the hot pressing temperature being 500° C., the pressure being 4T, and the pressure being maintained for 4 minutes; after cooling, removing the mold and demolding, and taking out the diffusion couple sample;
[0101] (6) The diffusion couple sample prepared in step (5) is polished with 600, 1000, 1500, and 2000 mesh sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10 minutes, and then dried in a vacuum drying oven for 30 minutes. The sample is taken out and packaged in a quartz tube in a vacuum environment; the sample is then placed in a diffusion furnace for annealing, and the annealing process is 1100°C for 300 hours. The sample is then quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10 minutes and then vacuum dried. It can then be directly used for phase diagram determination and diffusion experiments.
[0102] Example 6
[0103] A method for preparing a Fe-Mn-Zn ternary diffusion couple comprises the following steps:
[0104] (1) The raw materials (pure Fe, 64wt% Mn-Fe alloy) to be used for preparing diffusion couples are cut into shapes of the same size (7*10*3.5) by wire cutting;
[0105] (2) The pure Fe and 64 wt% Mn-Fe alloy obtained by cutting in step (1) were polished using 600, 1000, 1500, and 2000 grit sandpapers, and then polished on a polishing cloth with 0.3 μm diamond polishing liquid, and placed in alcohol for ultrasonic treatment for 10 minutes;
[0106] (3) The pure Fe and 64wt% Mn-Fe alloy prepared in step (2) are placed in a vacuum hot pressing mold in sequence, and the assembly method is as follows: Figure 3 As shown, use the lower die with a cover of 6.5 mm and assemble the mold;
[0107] (4) placing the mold assembled in step (3) on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the assembled mold fits the pressing head;
[0108] (5) performing vacuum hot pressing on the assembled mold in step (4), with the hot pressing temperature being 600° C., the pressure being 5T, and the pressure being maintained for 4 minutes; after cooling, removing the mold and demolding, and taking out the diffusion couple sample;
[0109] (6) The diffusion couple sample prepared in step (5) was polished with 600, 1000, 1500, and 2000 grit sandpaper, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10 minutes, and then dried in a vacuum drying oven for 30 minutes, and the sample was taken out and packaged in a quartz tube in a vacuum environment. The sample was then placed in a diffusion furnace for annealing, and then the sample was quenched and taken out;
[0110] (7) The diffusion couple sample prepared in step (6) is cut by wire cutting, with the cutting line parallel to the side with a side length of 10 mm and 3.5 mm away from the side, into a sample with a size of 10*7*3.5 mm, wherein the two components of the diffusion couple sample, pure Fe and 64 wt% Mn-Fe, each account for half;
[0111] (8) Cut the raw material (pure Zn) to be used for preparing diffusion couples into the same size (7*10*3.5) by wire cutting;
[0112] (9) The Fe / 64wt% Mn-Fe and pure Zn obtained by cutting in step (7) and step (8) were polished using 600, 1000, 1500, and 2000 grit sandpapers, and then polished on a polishing cloth with 0.3 μm diamond polishing liquid, and placed in alcohol for ultrasonic treatment for 10 minutes;
[0113] (10) The Fe / 64wt% Mn-Fe and pure Zn prepared in step (9) are placed in a vacuum hot pressing mold in sequence, and the assembly method is as follows: Figure 4 As shown, use the lower die with a cover of 6.5 mm and assemble the mold;
[0114] (11) placing the mold assembled in step (10) on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the assembled mold fits the pressing head;
[0115] (12) performing vacuum hot pressing on the assembled mold in step (11), with the hot pressing temperature being 600° C., the pressure being 4T, and the pressure being maintained for 2 minutes; after cooling, removing the mold and demolding, and taking out the diffusion couple sample;
[0116] (13) The diffusion couple sample prepared in step (12) is polished with 600, 1000, 1500, and 2000 mesh sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10 minutes, and then dried in a vacuum drying oven for 30 minutes. The sample is taken out and packaged in a quartz tube in a vacuum environment; the sample is then placed in a diffusion furnace for annealing. The annealing process is 300°C for 100 hours, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10 minutes and then vacuum dried. It can then be directly used for phase diagram determination and diffusion experiments.
[0117] Please refer to Fig. 9 , is the SEM scanning image of the diffusion interface of the Fe-Mn-Zn ternary diffusion couple. Fig. 9 It can be seen that the two adjacent interfaces in the ternary diffusion couple are well bonded, and there is an obvious diffusion area between the components, which provides a reliable diffusion couple sample for the subsequent research and analysis results of phase diagrams, diffusion thermodynamics and kinetics.
[0118] It should be noted that, according to the above-mentioned assembly method of metal materials in the preparation of diffusion couples and the preparation process of diffusion couples, the preparation method of the diffusion couple of the present invention can also be used for the preparation of higher-order diffusion couples.
[0119] Compared with the prior art, the method for preparing a high-throughput solid diffusion couple provided by the present invention has the following beneficial effects:
[0120] 1. The preparation method of the high-throughput solid diffusion couple provided by the present invention adopts the vacuum hot pressing method to prepare the diffusion couple, and the hot pressing temperature is the plastic deformation temperature of the component materials, so that the bonding is achieved through the plastic deformation of the component metals, and the diffusion couple interface is well bonded; and the bonding is achieved through plastic deformation, and the heat preservation and pressure holding time during the vacuum hot pressing process can be greatly reduced, so as to facilitate the rapid preparation of diffusion couple samples and save energy consumption; moreover, the heat preservation and pressure holding time is greatly reduced, and the prepared diffusion couple samples are more conducive to subsequent thermodynamic analysis and testing, because if the heat preservation and pressure holding time is too long, the diffusion couple sample has already diffused, thus affecting the subsequent phase diagram, diffusion thermodynamics and kinetics research and analysis results.
[0121] Second, the method for preparing a high-throughput solid diffusion couple provided by the present invention is to design the size of the vacuum hot pressing mold and the component materials so that the sum of the thickness of component A and component B is equivalent to their width, and to achieve continuous processing of ternary diffusion couples, quaternary diffusion couples, and higher diffusion couples through subsequent sample cutting and component assembly. The method has continuity. In addition, the same process is used to complete the preparation of multi-component diffusion couples, and the method is simple and easy to operate.
[0122] 3. The method for preparing high-throughput solid diffusion couples provided by the present invention comprises a vacuum hot pressing mold including multiple sets of upper molds and lower molds, which can realize batch preparation of diffusion couple samples and simultaneously prepare diffusion couple samples of different materials, thereby effectively improving experimental efficiency.
[0123] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations made to these embodiments without departing from the principles and spirit of the present invention are still within the protection scope of the present invention.
Claims
1. A method for preparing a high-throughput solid diffusion couple, It is characterized in that The steps include: Step S1, providing a vacuum hot pressing mold, wherein the vacuum hot pressing mold comprises a female mold, a plurality of receiving grooves provided in the female mold, a lower mold fixed to the bottom of the receiving groove, an upper mold embedded in the receiving groove and slidable along the axis of the receiving groove, a limiting ring sleeved on the outside of the female mold, and a cover plate covering the limiting ring and fitting with the upper mold during operation; Step S2, preparing a binary diffusion couple, specifically comprises the following steps: Step S21, cutting the raw material components A and B to be used for preparing diffusion couples into the same size by wire cutting, and the cross-sectional shape and size of the components A and B correspond to the end surface shape and size of the upper mold and the lower mold in the vacuum hot pressing mold, and the sum of the thickness of the components A and B is equivalent to their width; Step S22, polishing the component A and component B prepared in step S21 with 600, 1000, 1500, and 2000 grit sandpapers, and then polishing with 0.3 μm diamond polishing liquid on a polishing cloth, and placing in alcohol for ultrasonic treatment for 10-20 minutes; Step S23, placing the components A and B prepared in step S22 in the receiving grooves of the vacuum hot pressing mold in sequence, and assembling the mold, the upper mold and the lower mold to fix the components A and B; Step S24, placing the mold assembled in step S23 on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the mold fits the pressing head; Step S25, performing vacuum hot pressing at the plastic deformation temperature of the two components, and controlling the heat preservation time to be 50-60 minutes, the pressure holding time to be 4-6 minutes, and removing the mold after cooling, and taking out the diffusion couple sample; Step S26, the diffusion couple sample prepared in step S25 is polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes, and then dried in a vacuum drying oven, the sample is taken out and packaged into a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes and then vacuum dried to obtain a binary diffusion couple AB that can be directly used for phase diagram determination and diffusion experiments.
2. The method for preparing a high-throughput solid diffusion couple according to claim 1, It is characterized in that Also included is a method for preparing a ternary diffusion couple, which specifically includes the following steps: Step S31, performing side line cutting on the binary diffusion couple sample prepared in step S2, so that the shape and size after cutting correspond to the end face shape and size of the upper mold and the lower mold in the vacuum hot pressing mold, and satisfying that component A and component B occupy one half of the volume of the original diffusion couple sample; Step S32, the binary diffusion couple AB and component C obtained by cutting in step S31 are polished with 600, 1000, 1500, and 2000 mesh sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes; wherein the size of component C is the same as the size of the binary diffusion couple AB after cutting; Step S33, assembling the binary diffusion couple AB and component C prepared in step S32 into a vacuum hot pressing mold; Step S34, placing the mold assembled in step S23 on a pressing platform of a vacuum hot pressing furnace, so that the cover plate of the mold fits the pressing head; Step S35, performing vacuum hot pressing at the plastic deformation temperature of the diffusion couple AB and the component C, and controlling the heat preservation time to be 50-60 minutes, the pressure holding time to be 4-6 minutes, and removing the mold after cooling to remove the diffusion couple sample; Step S36, the diffusion couple sample prepared in step S35 is polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes, and then dried in a vacuum drying oven, the sample is taken out and packaged into a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes and then vacuum dried to obtain a ternary diffusion couple that can be directly used for phase diagram determination and diffusion experiments.
3. The method for preparing a high-throughput solid diffusion couple according to claim 1, It is characterized in that Also included is a method for preparing a quaternary diffusion couple, which specifically includes the following steps: Step S41, preparing binary diffusion couple AB and binary diffusion couple CD according to the preparation method of claim 1, and performing side line cutting on the diffusion couple sample, so that the shape and size after cutting correspond to the end face shape and size of the upper mold and the lower mold in the vacuum hot pressing mold, and satisfying that the two components each occupy one half of the volume of the original diffusion couple sample; Step S42, the diffusion couple AB and the diffusion couple CD obtained by cutting in step S41 are polished with 600, 1000, 1500, and 2000 grit sandpapers, and then polished with 0.3 μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes; Step S43, assembling the diffusion couple AB and the diffusion couple CD prepared in step S42 into a vacuum hot pressing mold; Step S44, placing the mold assembled in step S43 on a pressing platform of a vacuum hot pressing furnace so that the cover plate of the mold fits the pressing head; Step S45, performing vacuum hot pressing at the plastic deformation temperature of the diffusion couple AB and the diffusion couple CD, and controlling the heat preservation time to be 50-60 minutes, the pressure holding time to be 4-6 minutes, and removing the mold after cooling to remove the diffusion couple sample; Step S46, the diffusion couple sample prepared in step S45 is polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes, and then dried in a vacuum drying oven, the sample is taken out and packaged into a quartz tube in a vacuum environment; then the sample is placed in a diffusion furnace for annealing treatment, and then the sample is quenched and taken out, and polished with 600, 1000, 1500, and 2000 mesh sandpapers in sequence, and then polished with 0.3μm diamond polishing liquid on a polishing cloth, and placed in alcohol for ultrasonic treatment for 10-20 minutes and then vacuum dried to obtain a quaternary diffusion couple that can be directly used for phase diagram determination and diffusion experiments.
4. The method for preparing a high-throughput solid diffusion couple according to claim 1, It is characterized in that The dimensions of component A and component B are 10 mm*7 mm*3.5 mm respectively.
5. The method for preparing a high-throughput solid diffusion couple according to claim 2, It is characterized in that In step S31, the size of the cut binary diffusion couple AB is 10 mm*7 mm*3.5 mm.
6. The method for preparing a high-throughput solid diffusion couple according to claim 1, It is characterized in that In the vacuum hot pressing mold, there are at least three groups of upper molds and lower molds.
Citation Information
Patent Citations
Vanadium slag / calcium oxide diffusion couple and preparation method thereof
CN110146357A
High-coercivity neodymium iron boron magnet and preparation method therefor
WO2019169875A1
Cited By
Sintering-free ceramic powder-metal diffusion couple preparation method
CN122167180A