Method for producing catalyst for producing methacrylic acid, method for producing methacrylic acid, method for producing methacrylic acid ester, and device for producing catalyst for producing methacrylic acid

By preparing and processing phosphorus-molybdenum-containing slurry, combined with specific mixing and drying procedures, the problem of catalyst particle size distribution instability in the prior art is solved, and the selectivity and performance of the methacrylic acid catalyst are improved.

CN114981008BActive Publication Date: 2024-10-11MITSUBISHI CHEM CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202180008493.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-08
Filing Date
2021-01-08
Publication Date
2024-10-11
Estimated Expiration
2041-01-08

AI Technical Summary

Technical Problem

It is difficult to stably produce a slurry with a desired particle size distribution with the existing technology, which leads to a decrease in the performance of the catalyst for methacrylic acid production. Moreover, when using equipment such as a linear mixer, the particles in the slurry are destroyed, affecting the selectivity of the catalyst. .

Method used

By preparing a slurry A1 containing a heteropoly acid or a salt thereof containing phosphorus and molybdenum, and mixing it with the liquid B containing a cationic raw material, the half-peak width and median particle size of the particle size distribution are controlled, using specific processes and equipment such as Turbine pump is used for processing to ensure that the particle size distribution of slurry C is within the range of 2≤Dc≤50μm and 0.6≤DA2/DA1<1.0.

Benefits of technology

It achieves the stable production of high-selectivity methacrylic acid catalysts, improves the performance and selectivity of the catalyst, avoids particle damage, and ensures the efficient use of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003737506480000221
    Figure BDA0003737506480000221
  • Figure HDA0003737506490000011
    Figure HDA0003737506490000011
Patent Text Reader

Abstract

The present invention provides a method for stably producing a catalyst capable of obtaining methacrylic acid with high selectivity. The method for producing a catalyst for producing methacrylic acid comprises the following steps: (i) preparing a slurry A1 containing a heteropolyacid or a salt thereof containing at least phosphorus and molybdenum, (ii) using the slurry A1, preparing a slurry A2 satisfying the following formulas (I) and (II), (iii) mixing the slurry A2 with a raw material liquid B containing a cationic raw material to prepare a slurry C, and (iv) drying the slurry C. A2 / α A1 ≤0.95(I);2≤D A2 ≤50(II)(in formula (I), α A1 The half-peak width [μm] of the particle size distribution of slurry A1, α A2 represents the half-peak width [μm] of the particle size distribution of slurry A2. A2 The median particle size (μm) of the particle size distribution of slurry A2 is shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a catalyst for producing methacrylic acid, a method for producing methacrylic acid, a method for producing methacrylic acid ester, and an apparatus for producing a catalyst for producing methacrylic acid. Background Art

[0002] As a catalyst for the manufacture of methacrylic acid (hereinafter, also referred to as "catalyst") used when methacrylic acid is manufactured by oxidizing methacrolein, a heteropolyacid catalyst containing molybdenum and phosphorus is known. As such a heteropolyacid catalyst, there are proton heteropoly acids whose counter cations are protons, and heteropolyacid salts formed by replacing a portion of the protons with cations other than protons (hereinafter, proton heteropoly acids are also referred to as "heteropoly acids", and proton heteropoly acids and / or heteropolyacid salts are also referred to as "heteropoly acids (salts)"). As heteropolyacid salts, alkali metal salts whose cations are alkali metals and ammonium salts whose cations are ammonium ions are known. It should be noted that proton heteropoly acids are water-soluble, but alkali metal salts of heteropoly acids are generally poorly soluble because the ionic radius of the cations is large (Non-Patent Document 1).

[0003] As a method for producing a heteropolyacid catalyst, the following method is known: a slurry is produced by mixing catalyst raw materials of each element at a specific ratio in a manner to obtain a desired catalyst composition, the slurry is mixed with a raw material containing a cation raw material, and then the slurry is produced by drying, etc. For example, in Patent Document 1, a method is described in which a liquid containing a heteropolyacid (salt) is obtained by mixing a catalyst raw material liquid A containing molybdenum, phosphorus and vanadium with a catalyst raw material liquid B containing a cation raw material, and then drying the liquid to obtain a catalyst.

[0004] In addition, Patent Document 2 proposes a method for producing a catalyst for methacrylic acid production by controlling the mixing state of a slurry using a linear mixer, a homomixer, a homogenizer, or the like.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2018 / 037998

[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 7-185354

[0009] Non-patent literature

[0010] Non-patent document 1: Masayuki Otake and Takeshi Onoda, The Society of Catalysts, “Catalysts”, vol. 18, No. 6 (1976), p. 169 Summary of the invention

[0011] According to the research of the present inventors, the particle size distribution when preparing the slurry has a great influence on the methacrylic acid selectivity of the obtained catalyst. However, it was found that it is difficult to stably prepare a slurry having a desired particle size distribution when only stirring and mixing is performed. In addition, when stirring and mixing is performed using a linear mixer, a homomixer, a homogenizer, etc. as described in Patent Document 2, the particles in the slurry are destroyed, and as a result, it was found that the performance of the obtained catalyst sometimes decreases.

[0012] Therefore, an object of the present invention is to provide a method for producing a catalyst for producing methacrylic acid, which can stably produce a catalyst capable of obtaining methacrylic acid with a high selectivity, and a method for producing methacrylic acid and a method for producing methacrylic acid ester using the catalyst. Another object of the present invention is to provide an apparatus for producing a catalyst for producing methacrylic acid, which can stably produce a catalyst capable of obtaining methacrylic acid with a high selectivity.

[0013] The present inventors have conducted intensive studies in view of the above problems and, as a result, have found that the above problems can be solved by using a catalyst produced by a specific production method as a catalyst for producing methacrylic acid, thereby completing the present invention.

[0014] That is, the present invention includes the following aspects [1] to

[22] .

[0015] [1]: A method for producing a catalyst for producing methacrylic acid, which is a method for producing a catalyst for use in producing methacrylic acid by oxidizing methacrolein, comprising the following steps:

[0016] (i) a step of preparing a slurry A1 containing a heteropolyacid or a salt thereof containing at least phosphorus and molybdenum,

[0017] (ii) a step of using the slurry A1 to prepare a slurry A2 satisfying the following formulas (I) and (II),

[0018] (iii) a step of mixing the slurry A2 with a raw material liquid B containing a cationic raw material to prepare a slurry C, and

[0019] (iv) a step of drying the slurry C;

[0020] α A2 / α A1 ≤0.95 (I)

[0021] 2≤D A2 ≤50 (II)

[0022] (In formula (I), α A1 The half-peak width [μm] of the particle size distribution of the slurry A1 is represented by α A2represents the half-peak width [μm] of the particle size distribution of the slurry A2. A2 represents the median particle size [μm] of the particle size distribution of the slurry A2.

[0023] [2]: The method for producing a catalyst for producing methacrylic acid according to [1], which satisfies the following formula (III).

[0024] 2≤D c ≤50 (III)

[0025] (In formula (III), D c represents the median particle size [μm] of the particle size distribution of the slurry C.

[0026] [3]: The method for producing a catalyst for producing methacrylic acid according to [1] or [2], which satisfies the following formula (IV).

[0027] 0.6≤D A2 / D A1 <1.0 (IV)

[0028] (In formula (IV), D A1 The median particle size [μm], D A2 represents the median particle size [μm] of the particle size distribution of the slurry A2.

[0029] [4]: The method for producing a catalyst for methacrylic acid production according to any one of [1] to [3], wherein in the step (ii), the slurry A2 is prepared by supplying the slurry A1 to a pump.

[0030] [5]: The method for producing a catalyst for producing methacrylic acid according to [4], wherein the volume of the slurry A1 prepared in the step (i) is V A1 , the total volume of the slurry A1 supplied to the pump is V POMP When the mixing of the raw material liquid B is started in the step (iii), V POMP / V A1 It is 0.1 or more.

[0031] [6]: The method for producing a catalyst for producing methacrylic acid according to [4] or [5], wherein in the step (iii), V at the time of starting mixing of the raw material liquid B is POMP / V A1 It is 1.0~10.0.

[0032] [7]: The method for producing a catalyst for producing methacrylic acid according to any one of [4] to [6], wherein in the step (iii), V at the time of starting mixing of the raw material liquid B is POMP / V A1 Greater than 1.0.

[0033] [8]: The method for producing a catalyst for methacrylic acid production according to any one of [4] to [7], wherein a supply rate of the slurry A1 to the pump is 1 L / min or more.

[0034] [9]: The method for producing a catalyst for producing methacrylic acid according to any one of [4] to [8], wherein the pump is a turbine pump or a reciprocating pump.

[0035]

[10] : The method for producing a catalyst for producing methacrylic acid according to any one of [4] to [9], wherein when the tank for preparing the slurry A1 in the step (i) is tank 1, and the tank for mixing the slurry A2 and the raw material liquid B in the step (iii) is tank 2, the tank 1 and the tank 2 are different tanks.

[0036]

[11] : The method for producing a catalyst for producing methacrylic acid according to

[10] , wherein the tank 1 and the tank 2 are connected by a pipe.

[0037]

[12] : The method for producing a catalyst for methacrylic acid production according to

[11] , wherein the pump is provided in the pipe.

[0038]

[13] : The method for producing a catalyst for producing methacrylic acid according to any one of [1] to

[12] , wherein the cation raw material is at least one selected from a compound containing an alkali metal and a compound containing an ammonium ion.

[0039]

[14] : The method for producing a catalyst for methacrylic acid production according to any one of [1] to

[13] , wherein the viscosity of the slurry A1 at 30°C is 1 to 200 cP.

[0040]

[15] : The method for producing a catalyst for methacrylic acid production according to any one of [1] to

[14] , wherein the solid content concentration of the slurry A1 is 5 to 60% by mass.

[0041]

[16] : The method for producing a catalyst for producing methacrylic acid according to any one of [1] to

[15] , wherein the catalyst has a composition represented by the following formula (V).

[0042] P a Mo b V c Cud X e Y f Z g (NH4) h O i (V)

[0043] (In the formula, P, Mo, V, Cu, NH4 and O represent phosphorus, molybdenum, vanadium, copper, ammonium and oxygen, respectively. X represents at least one element selected from silicon, titanium, germanium, arsenic, antimony and bismuth. Y represents at least one element selected from niobium, tantalum, tungsten, cerium, zirconium, silver, iron, zinc, chromium, magnesium, cobalt, manganese, barium and lanthanum. Z represents at least one element selected from lithium, sodium, potassium, rubidium and cesium. a~i represent the molar ratio of each component, and when b=12, a=0.5~3, c=0.01~3, d=0.01~2, e=0.1~3, f=0~3, g=0.01~3, h=0~20 are satisfied, and i is the molar ratio of oxygen required to satisfy the valence of the above-mentioned components.)

[0044]

[17] : A method for producing methacrylic acid, comprising oxidizing methacrolein in the presence of a catalyst produced by the method according to any one of [1] to

[16] .

[0045]

[18] : A method for producing a methacrylic acid ester, comprising esterifying methacrylic acid produced by the method described in

[17] .

[0046]

[19] : A device for producing a catalyst for producing methacrylic acid, which is a device for producing a catalyst used when producing methacrylic acid by oxidizing methacrolein, comprising:

[0047] a tank for preparing a slurry A1 containing at least phosphorus and molybdenum, and

[0048] The mechanism of preparing slurry A2 satisfying the following formulae (I) and (II) using the above slurry A1.

[0049] α A2 / α A1 ≤0.95 (I)

[0050] 2≤D A2 ≤50 (II)

[0051] (In formula (I), α A1 The half-peak width [μm] of the particle size distribution of the slurry A1 is represented by α A2 represents the half-peak width [μm] of the particle size distribution of the slurry A2. A2 represents the median particle size [μm] of the particle size distribution of the slurry A2.

[0052]

[20] : The methacrylic acid production apparatus according to

[19] , comprising a tank 1 for preparing the slurry A1 and a tank 2 for mixing the slurry A1 with a raw material liquid B containing a cationic raw material.

[0053]

[21] : The device for producing a catalyst for producing methacrylic acid according to

[20] , wherein the tank 1 and the tank 2 are connected by a pipe.

[0054]

[22] : The device for producing a catalyst for producing methacrylic acid according to

[21] , wherein a pump is provided in the pipe.

[0055] According to the present invention, there are provided a method for producing a catalyst for producing methacrylic acid, which can stably produce a catalyst capable of obtaining methacrylic acid with a high selectivity, and a method for producing methacrylic acid and a methacrylic acid ester using the catalyst. In addition, there is provided an apparatus for producing a catalyst for producing methacrylic acid, which can stably produce a catalyst capable of obtaining methacrylic acid with a high selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 It is a schematic diagram of a production apparatus according to one embodiment of the present invention. DETAILED DESCRIPTION

[0057] Hereinafter, an embodiment of the present invention will be described in detail. However, the description of the constituent elements described below is an example of the embodiment of the present invention, and the present invention is not limited to these contents.

[0058] [Methacrylic acid production catalyst]

[0059] The catalyst produced by the production method of the present invention is used when methacrylic acid is produced by oxidizing methacrolein. From the viewpoint of improving the selectivity when producing methacrylic acid, the catalyst preferably has a composition represented by the following formula (V). It should be noted that in the present invention, when the catalyst is formed using a carrier, the catalyst refers to a catalyst containing the carrier, and the following formula (V) is a composition taking the carrier into consideration.

[0060] P a Mo b V c Cu d X e Y f Z g (NH4) h O i (V)

[0061] (In the formula, P, Mo, V, Cu, NH4 and O represent phosphorus, molybdenum, vanadium, copper, ammonium and oxygen, respectively. X represents at least one element selected from silicon, titanium, germanium, arsenic, antimony and bismuth. Y represents at least one element selected from niobium, tantalum, tungsten, cerium, zirconium, silver, iron, zinc, chromium, magnesium, cobalt, manganese, barium and lanthanum. Z represents at least one element selected from lithium, sodium, potassium, rubidium and cesium. a~i represent the molar ratio of each component, and when b=12, a=0.5~3, c=0.01~3, d=0.01~2, e=0.1~3, f=0~3, g=0.01~3, h=0~20 are satisfied, and i is the molar ratio of oxygen required to satisfy the valence of the above-mentioned components.)

[0062] The molar ratio of each element is a value calculated by analyzing the components obtained by dissolving the catalyst in aqueous ammonia using ICP emission spectrometry. The molar ratio of ammonium is a value calculated by analyzing the catalyst using the Kjeldahl method.

[0063] [Method for producing catalyst for methacrylic acid production]

[0064] The present invention is a method for producing a catalyst used when producing methacrylic acid by oxidizing methacrolein, and is characterized by comprising the following steps (i) to (iv).

[0065] (i) A step of preparing a slurry A1 containing a heteropolyacid or a salt thereof containing at least phosphorus and molybdenum.

[0066] (ii) A step of preparing slurry A2 satisfying the following formulae (I) and (II) using the slurry A1.

[0067] (iii) A step of preparing slurry C by mixing the slurry A2 and a raw material solution B containing a cationic raw material.

[0068] (iv) A step of drying the slurry C.

[0069] α A2 / α A1 ≤0.95 (I)

[0070] 2≤D A2 ≤50 (II)

[0071] (In formula (I), α A1 The half-peak width [μm] of the particle size distribution of the slurry A1 is represented by α A2 represents the half-peak width [μm] of the particle size distribution of the slurry A2. A2 represents the median particle size [μm] of the particle size distribution of the slurry A2.

[0072] Hereinafter, each step will be described in detail.

[0073] (Process (i))

[0074] In the step (i), a slurry A1 containing a heteropoly acid (salt) containing at least phosphorus and molybdenum is prepared.

[0075] Slurry A1 contains at least these elements, so that a catalyst having a higher methacrylic acid selectivity can be produced.

[0076] The slurry A1 may contain other elements. For example, it may contain V (vanadium) and Cu (copper) in the above formula (V), and may also contain X element and Y element.

[0077] In addition, elements other than phosphorus and molybdenum in formula (V) may be added in the steps after step (i).

[0078] The slurry A1 can be prepared by dissolving or suspending a raw material compound of a catalyst component containing at least phosphorus and molybdenum in a solvent.

[0079] <Raw material compound of catalyst component>

[0080] The raw material compounds of the catalyst components are not particularly limited, and nitrates, carbonates, acetates, ammonium salts, oxides, halides, oxyacids, oxyacid salts, etc. of the constituent elements of the catalyst may be used alone or in combination of two or more.

[0081] Examples of the raw material compound of molybdenum include molybdenum oxide such as molybdenum trioxide, ammonium molybdate such as ammonium paramolybdate and ammonium dimolybdate, and molybdenum chloride.

[0082] Examples of the raw material compound of phosphorus include phosphoric acid, phosphorus pentoxide, and ammonium phosphate.

[0083] When producing a catalyst containing vanadium in addition to phosphorus and molybdenum, examples of the raw material compound of vanadium include ammonium metavanadate, vanadium pentoxide, vanadium chloride, vanadium oxalate and the like.

[0084] When producing a catalyst containing copper in addition to phosphorus and molybdenum, examples of the raw material compound of copper include copper sulfate, copper nitrate, copper oxide, copper carbonate, copper acetate, copper chloride and the like.

[0085] As the raw material compound of the catalyst component, each element constituting the catalyst component may be used alone or in combination of two or more.

[0086] The concentration of the raw material compound of the catalyst component in the slurry A1 is not particularly limited, but is preferably within a range of 5% by mass to 90% by mass.

[0087] <Solvent>

[0088] As the above-mentioned solvent, for example, water, ethanol, acetone, etc. can be mentioned. These can be used alone or in combination of two or more. Among these, water is preferably used from an industrial point of view.

[0089] <Formation of heteropolyacid (salt)>

[0090] Slurry A1 is preferably prepared by adding a raw material compound of a catalyst component to a solvent using a preparation container, and heating and stirring. The heating temperature can usually be carried out in the range of 30 to 150°C, but is preferably carried out in the range of 60 to 150°C. By making the heating temperature above 60°C, the generation rate of the heteropoly acid (salt) can be fully accelerated, and by making the heating temperature below 150°C, the evaporation of the solvent can be suppressed. The lower limit of the heating temperature is more preferably above 80°C, and more preferably above 90°C. In addition, the upper limit of the heating temperature is more preferably below 130°C, and more preferably below 110°C. In addition, depending on the vapor pressure of the solvent used, it can be concentrated or refluxed during heating, or operated in a closed container and heat-treated under pressurized conditions.

[0091] The heating rate is not particularly limited, but is preferably 0.8 to 15°C / min. By setting the heating rate to 0.8°C / min or more, the time required for step (i) can be shortened. In addition, by setting the heating rate to 15°C / min or less, a conventional heating device can be used for heating.

[0092] The stirring power is preferably 0.01 kW / m 3 The above is carried out, and more preferably 0.05 kW / m 3 The above is carried out. By making the stirring power 0.01 kW / m 3 The above results in that the temperature, composition and local temperature variations of the slurry A1 are reduced, and a structure suitable for a catalyst for producing methacrylic acid can be stably formed. In addition, from the viewpoint of the production cost of the catalyst, it is preferred to stir at a normal stirring power of 3.5 kW / m 3 The following is carried out.

[0093] <Particle size distribution of slurry A1>

[0094] The median particle size distribution of slurry A1 (D A1 ) is not particularly limited, but is preferably 2 to 50 μm. This makes it easy to prepare slurry A2 having a predetermined particle size distribution in the step (ii) described later. A1 The lower limit of D is more preferably 2.5 μm or more. A1 The upper limit is more preferably 25 μm or less, and further preferably 10 μm or less. In this specification, the median diameter refers to a particle diameter corresponding to a cumulative 50 volume % in a volume-based particle size distribution measured by a laser diffraction particle size distribution measurement method.

[0095] The half-peak width (α A1 ) is not particularly limited, but is preferably 3 to 10 μm, and the lower limit is more preferably 5 μm or more. In particular, when it is 5 μm or more, the effect of the present invention can be effectively obtained. It should be noted that in this specification, the half-peak width refers to the peak width at 1 / 2 the height of the peak with the largest particle size in the volume-based particle size distribution measured by the laser diffraction particle size distribution measurement method. It should be noted that the peak represents a maximum frequency of 0.5% or more.

[0096] <Physical properties of slurry A1>

[0097] The pH of slurry A1 is not particularly limited, but is preferably 0.1 to 4, with a lower limit of more preferably 0.5 or more, and an upper limit of more preferably 3 or less. By making the pH of slurry A1 to be 0.1 or more, the step of mixing raw material liquid B in the step (iii) described later can be stably performed. In addition, by making the pH of slurry A1 to be 4 or less, the formation reaction of heteropolyacid (salt) suitable for methacrylic acid production is stabilized. As a method for making the pH of slurry A1 to be 0.1 to 4, for example, molybdenum trioxide is used as a molybdenum raw material, or a method of appropriately selecting a raw material compound, adjusting the content of nitrate ions and oxalate ions, etc. can be cited.

[0098] The viscosity of slurry A1 is not particularly limited, and is preferably 1 to 200 cP at 30°C. By making the viscosity of slurry A1 at 30°C to be 1 cP or more, the step (ii) described later can be carried out stably, and by making it 200 cP or less, the mixing with the raw material liquid B in the step (iii) described later becomes good. The lower limit of the viscosity of slurry A1 at 30°C is more preferably 5 cP or more, and further preferably 10 cP or more. In addition, the upper limit is more preferably 150 cP or less, and further preferably 100 cP or less. The viscosity of slurry A1 can be measured by a method using a B-type viscometer described later.

[0099] The specific gravity of the slurry A1 is not particularly limited, but is preferably 1.05 to 1.25 kg / L from the viewpoint of stably performing the step (ii) described later.

[0100] The solid content concentration of slurry A1 (the mass ratio of the solid content to the whole slurry A1) is not particularly limited, but is preferably 5 to 60% by mass. Thus, in the step (iii) described later, slurry C can be stably prepared. The lower limit of the solid content concentration of slurry A1 is more preferably 10% by mass or more, and more preferably 15% by mass or more. In addition, the upper limit is more preferably 55% by mass or less, and more preferably 50% by mass or less.

[0101] <Volume of slurry A1>

[0102] In view of industrial production, from the viewpoint of production cost, the volume of slurry A1 and raw material liquid B is preferably 0.2 m 3 More preferably 0.8m 3 More than 1.5 m 3 It should be noted that the upper limit of the volume is not particularly limited, for example, it can be 5m 3 the following.

[0103] (Step (ii))

[0104] In step (ii), slurry A2 satisfying the following formulae (I) and (II) is prepared using slurry A1 obtained in step (i). Slurry A2 contains the heteropolyacid (salt) produced in step (i).

[0105] α A2 / α A1 ≤0.95 (I)

[0106] 2≤D A2 ≤50 (II)

[0107] In formula (I), α A1 The half-peak width [μm] of the particle size distribution of slurry A1, α A2 The half-peak width [μm] of the particle size distribution of slurry A2 is shown. A2 / α A1 is the ratio of the half-peak width of the particle size distribution of slurry A1 and slurry A2, α A2 / α A1 When it is less than 1, it means that the agglomerated particles in slurry A1 are dispersed, and slurry A2 containing more uniform particles can be prepared. A2 The median particle size [μm] of the particle size distribution of slurry A2 is shown.

[0108] By preparing slurry A2 satisfying the above formulas (I) and (II), a catalyst with high selectivity for methacrylic acid can be obtained. This is considered to be because by preparing the catalyst using slurry A2 in which the agglomerated particles in slurry A1 are dispersed (deagglomerated) and have a predetermined median particle size, a heteropolyacid salt suitable for methacrylic acid production can be produced in the later-described step (iii). Slurry A2 satisfies α A2 / α A1 ≤0.95, preferably satisfying α A2 / α A1 ≤0.9. A2 / α A1 The lower limit of is not particularly limited, but is 0.7 or more (α A2 / α A1 ≧0.7) can achieve sufficient effect. A2It is preferably 9 μm or less, more preferably 8 μm or less, and further preferably 7 μm or less.

[0109] D A2 The lower limit of D is 2 μm or more, preferably 2.5 μm or more. A2 The upper limit of the particle size is 50 μm or less, preferably 25 μm or less, and more preferably 10 μm or less.

[0110] In addition, slurry A2 preferably satisfies the following formula (IV).

[0111] 0.6≤D A2 / D A1 <1.0 (IV)

[0112] In formula (IV), D A1 The median particle size [μm], D A2 The median particle size [μm] of the particle size distribution of the slurry A2 is shown in D A2 / D A1 is the ratio of the median particle size of the particle size distribution of slurry A1 and slurry A2, D A2 / D A1 When D is less than 1, it means that the aggregated particles in slurry A1 are dispersed (deagglomerated), and the median particle size of slurry A2 is reduced. On the other hand, the particles in slurry A1 are destroyed, and D A2 / D A1 When D is less than 0.6, the selectivity of methacrylic acid of the obtained catalyst decreases. Slurry A2 more preferably satisfies 0.7≤D A2 / D A1 <1.0.

[0113] The slurry A2 satisfying the above formulas (I) and (II) can be prepared using a catalyst manufacturing device, which includes: a tank for preparing the slurry A1, and a mechanism for preparing the slurry A2 satisfying the above formulas (I) and (II) using the slurry A1. The mechanism for preparing the slurry A2 satisfying the above formulas (I) and (II) is not particularly limited, and examples thereof include a method of supplying the slurry A1 to a pump and preparing the slurry using shear force; a method of preparing the slurry by irradiating the slurry A1 with ultrasonic waves to directly vibrate the particles; or a method of separating the agglomerated particles in the slurry A1 using a sieve (filtration), gravity, inertia, centrifugal force, etc.

[0114] Hereinafter, a method for preparing slurry A2 by supplying slurry A1 to a pump will be described with reference to the drawings and by showing an embodiment.

[0115] <Methacrylic acid production catalyst production device>

[0116] The method of supplying slurry A1 to a pump to prepare slurry A2 is not particularly limited, for example, Figure 1 The production process is carried out using the production apparatus shown (hereinafter, also simply referred to as "the present production apparatus").

[0117] Figure 1 The manufacturing apparatus shown has a tank 1 and a tank 2, and the tank 1 and the tank 2 are connected by a pipe 32 equipped with a pump 31. The tank 1 is provided with a stirrer 11, a take-out port 12, and a liquid return port 13. The tank 2 is provided with a stirrer 21, a supply port 22, a take-out port 23, and a liquid supply port 24.

[0118] The piping 32 is connected to the tank 1 via the outlet 12 and the liquid return port 13 of the tank 1, and is connected to the tank 1 via the liquid supply port 24 of the tank 2. In addition, the piping 32 includes a piping portion 32a connected to the liquid return port 13 of the tank 1, and a piping portion 32b connected to the liquid supply port 24 of the tank 2, and a two-way valve 33 is provided at a branch portion between the piping portion 32a and the piping portion 32b. By using the two-way valve 33, it is possible to switch the method of sending the slurry A1 sent from the pump 31 to either the liquid return port 13 or the liquid supply port 24. In addition, by installing a pressure gauge 34 between the pump 31 and the two-way valve 33, the discharge pressure of the pump 31 can be measured. It should be noted that Figure 1 The manufacturing apparatus shown is an example and may have other configurations.

[0119] The volumes of tank 1 and tank 2 are not particularly limited and can be appropriately selected according to the volume of slurry A1. The materials of tank 1 and tank 2 are also not particularly limited and tanks made of stainless steel or tanks with glass coating inside can be used.

[0120] The form of the pump 31 is not particularly limited, and a generally used turbine pump, positive displacement pump, etc. can be used. Examples of the turbine pump include a centrifugal pump, a propeller pump (axial flow pump, diagonal flow pump), and a viscous pump. In addition, examples of the positive displacement pump include a reciprocating pump and a rotary pump. Among these, a turbine pump or a reciprocating pump is preferably used, and a turbine pump is more preferably used.

[0121] The inner diameter of the pipe 32 (including the pipe parts 32a and 32b) is not particularly limited. In view of industrial production and the processing volume, it is preferably 5 to 500 mm. The lower limit of the inner diameter of the pipe 32 is more preferably 7 mm or more, and more preferably 10 mm or more. In addition, the upper limit is more preferably 200 mm or less, and more preferably 100 mm or less.

[0122] <Preparation of Slurry A2 by Supplying Slurry A1 to a Pump>

[0123] The slurry A2 satisfying the above formulae (I) and (II) can be prepared as follows using the above-mentioned present production apparatus.

[0124] First, slurry A1 is prepared in tank 1. At this time, tank 1 may be used as a preparation container in step (i), or slurry A1 prepared in step (i) may be supplied to tank 1. At this time, slurry A1 may be stirred by stirrer 11.

[0125] Thereafter, slurry A1 is taken out from the outlet 12, supplied to the pump 31 via the pipe 32, and supplied to the tank 2 from the liquid supply port 24 via the pipe portion 32b. At this time, the pump 31 applies shear force to the slurry A1, and the agglomerated particles in the slurry A1 are dispersed, and the slurry A2 containing more uniform particles can be prepared.

[0126] It should be noted that the slurry A1 can also be sent and circulated by returning to the tank 1 from the return port 13 via the piping portion 32a. The sending of the slurry A1 to the tank 2 and the sending of the slurry A1 to the tank 1 can be performed in combination. That is, after the slurry A1 is supplied to the pump 31, it can be sent to the tank 1 and returned, and after at least a part of it is circulated, the pump 31 is used again to send the slurry A1 from the tank 1 to the tank 2. It should be noted that "circulation" here means that the slurry A1 taken out from the tank 1 and supplied to the pump 31 is returned to the tank 1 again, and circulation is a type of sending.

[0127] It should be noted that the delivery of slurry A1 taken out from the outlet 12 of tank 1 to the liquid return port 13 side of tank 1 and the delivery to the liquid supply port 24 side of tank 2 can be controlled by switching the liquid delivery pipeline (piping parts 32a, 32b) of slurry A1 using a two-way valve 33.

[0128] The slurry A1 may be fed into the tank 1 and / or the tank 2 while being stirred by the stirrers 11 and 21 .

[0129] The supply rate of slurry A1 to pump 31 is not particularly limited, and is preferably 1 L / min or more. This can generate a shear force for dispersing the agglomerated particles in slurry A1, and can efficiently prepare slurry A2. In addition, the supply rate of slurry A1 to pump 31 is preferably 400 L / min or less. Thus, it is possible to suppress the destruction of particles in slurry A1 by excessive shear force. The lower limit of the supply rate of slurry A1 to pump 31 is more preferably 10 L / min or more, further preferably 100 L / min or more, and particularly preferably 150 L / min or more. In addition, the upper limit is more preferably 300 L / min or less, and further preferably 250 L / min or less.

[0130] The volume of the slurry A1 prepared in the above step (i) is defined as V. A1 , the total volume of slurry A1 supplied to the pump 31 is V POMP When V POMP / V A1When the ratio of the slurry A1 to the raw material B in the step (iii) described later is 0.1 or more, the mixing of the raw material liquid B is started. Thus, the heteropolyacid salt suitable for the production of methacrylic acid can be stably produced in the step (iii). It should be noted that as long as at least a part of the slurry A1 is supplied to the pump 31 and the prepared slurry A2 is present in the tank 2, the mixing of the raw material liquid B can be started in the tank 2 while the remaining slurry A1 is supplied to the pump 31. POMP / V A1 The lower limit of V is more preferably 0.5 or more, further preferably 1.0 or more, particularly preferably greater than 1.0, and most preferably 2.0 or more. POMP / V A1 V is greater than 1.0, which means that after the slurry A1 is supplied to the pump 31, it is sent to the tank 1 and returned, and after at least a part of it is circulated, the slurry A1 is sent from the tank 1 to the tank 2 again by the pump 31 (as a result, the slurry including the slurry sent again by the circulation is mixed with the raw material liquid B). On the other hand, in order to prevent the particles in the slurry A1 from contacting each other and being destroyed, V POMP / V A1 The upper limit of is preferably 10.0 or less, more preferably 5.0 or less, and further preferably 4.0 or less.

[0131] It should be noted that V POMP / V A1 It is preferable to adjust the speed appropriately according to the supply speed of the slurry A1 to the pump 31. When the liquid feeding speed of the slurry A1 is high, the shear force is high, and the aggregated particles in the slurry A1 are easily dispersed. POMP / V A1 Even when the particle size is small, slurry A2 can be easily prepared.

[0132] The temperature during the liquid feeding of the slurry A1 is not particularly limited, but is preferably a temperature that does not cause the solvent to vaporize and generate cavitation in the pump. In order to stabilize the properties of the slurry A1, it is preferably 30 to 150° C. The lower limit of the temperature during the liquid feeding of the slurry A1 is more preferably 40° C. or higher, and further preferably 50° C. or higher. In addition, the upper limit is more preferably 120° C. or lower, and further preferably 100° C. or lower.

[0133] The discharge pressure of the pump 31 for supplying the slurry A1 is not particularly limited, but is preferably 1 to 1000 kPa in order to stabilize the properties of the slurry A1. The lower limit of the discharge pressure of the pump 31 is more preferably 10 kPa or more, and further preferably 100 kPa or more, and the upper limit is more preferably 800 kPa or less, and further preferably 600 kPa or less.

[0134] (Process (iii))

[0135] In the step (iii), the slurry A2 obtained in the step (ii) is mixed with a raw material solution B containing a cationic raw material to prepare a slurry C.

[0136] By mixing slurry A2 and raw material solution B, the counter cations of the heteropoly acid (salt) contained in slurry A2 are replaced by the cations contained in raw material solution B, thereby obtaining slurry C containing the heteropoly acid salt.

[0137] A catalyst having high selectivity in methacrylic acid production can be obtained by mixing slurry A2 satisfying the above formulae (I) and (II) with raw material liquid B to produce slurry C. The mechanism is not clear, but is believed to be based on the following reasons.

[0138] As described above, slurry A1 contains a heteropoly acid (salt) containing at least phosphorus and molybdenum, and the particles in slurry A1 containing the heteropoly acid (salt) are usually present in a coagulated state. When raw material liquid B is mixed into slurry A1 in this state to produce slurry C, it is difficult to uniformly form a heteropoly acid salt because raw material liquid B cannot evenly reach the inside of the coagulated particles in slurry A1. However, in the above-mentioned step (ii), slurry A2 can be prepared in which the coagulated particles in slurry A1 are dispersed (de-coagulated) and contain more uniform particles. By mixing the slurry A2 with raw material liquid B, a heteropoly acid salt can be uniformly formed. This uniform heteropoly acid salt is suitable as a catalyst for the manufacture of methacrylic acid, and as a result, it is believed that a catalyst with a high selectivity for methacrylic acid can be obtained.

[0139] It should be noted that, when a treatment is performed to disperse the particles formed after mixing slurry A1 with raw material liquid B, or when a treatment is performed to disperse only the particles in raw material liquid B, it is difficult to obtain a catalyst having a high selectivity for methacrylic acid as described above. Thus, it is extremely important to first disperse the agglomerated particles in slurry A1 to prepare slurry A2, and then mix slurry A2 with raw material liquid B. However, a treatment to disperse the particles in raw material liquid B may be performed as necessary.

[0140] <Preparation of raw material solution B>

[0141] The raw material solution B contains a cation raw material. The raw material solution B can be prepared by dissolving or suspending the cation raw material in a solvent.

[0142] Here, "cation raw material" means at least one selected from compounds containing alkali metals, compounds containing alkaline earth metals, compounds containing transition metals, compounds containing base metals, and compounds containing nitrogen (compounds containing ammonia, ammonium ions or alkylammonium ions, or nitrogen-containing heterocyclic compounds). As alkali metals, lithium, sodium, potassium, rubidium, and cesium can be mentioned. As alkaline earth metals, magnesium, calcium, strontium, and barium can be mentioned. As compounds containing alkali metals, compounds containing alkaline earth metals, compounds containing transition metals, and compounds containing base metals, nitrates, carbonates, bicarbonates, acetates, sulfates, ammonium salts, oxides, hydroxides, halides, oxygen-containing acids, and oxygen-containing acid salts of alkali metals, alkaline earth metals, transition metals, or base metals can be mentioned. As compounds containing ammonium ions, ammonium bicarbonate, ammonium carbonate, ammonium nitrate, ammonium phosphate, ammonium vanadate, and the like can be mentioned. Examples of compounds containing alkylammonium ions include halides or hydroxides of tetramethylammonium, tetraethylammonium, tetra-n-propylammonium, tetra-n-butylammonium, triethylmethylammonium, and the like. Examples of nitrogen-containing heterocyclic compounds include pyridine, piperidine, piperazine, pyrimidine, quinoline, isoquinoline, and alkyl derivatives thereof. One or more of these may be used. Among these, as a cationic raw material, from the viewpoint of obtaining a catalyst for the production of methacrylic acid with a higher selectivity for methacrylic acid, it is preferred that at least one selected from a compound containing an alkali metal and a compound containing an ammonium ion be used, and more preferably a compound containing an alkali metal and a compound containing an ammonium ion be used.

[0143] Examples of the solvent include water, ethanol, and acetone. These may be used alone or in combination of two or more. Among these, water is preferably used.

[0144] When a plurality of substances are used as the cation raw materials, a plurality of preparation containers may be used to dissolve or suspend the respective cation raw materials in a solvent, thereby preparing a plurality of raw material liquids B such as raw material liquids B1, B2, etc.

[0145] The concentration of the cationic raw material in the raw material solution B is not particularly limited, but is preferably within a range of 5 to 90% by mass.

[0146] When the raw material liquid B contains particles based on the above raw materials, the median particle size of the particle size distribution of the raw material liquid B is not particularly limited, and is preferably 5 μm or less. Thus, the slurry C satisfying formula (III) described later can be easily prepared. The upper limit of the median particle size of the particle size distribution of the raw material liquid B is more preferably 3 μm or less, and further preferably 1 μm or less. The raw material liquid B is preferably a solution state in which all the above raw materials are dissolved. When it contains particles based on the above raw materials, the upper limit of the median particle size is preferably small as described above, but from the viewpoint of being able to be used as a core for the generation of particles of the reactant, there may be particles with a median particle size of 0.01 μm or more, and there may be particles with a median particle size of 0.05 μm or more, and there may be particles with a median particle size of 0.1 μm or more.

[0147] <Mixing of slurry A2 and raw material liquid B>

[0148] In mixing slurry A2 and raw material liquid B, slurry A2 and raw material liquid B may be added to one of the two liquids and mixed to prepare slurry C. That is, raw material liquid B may be added to slurry A2 and mixed, or slurry A2 may be added to raw material liquid B and mixed.

[0149] It should be noted that when multiple raw material liquids B1, B2, etc. are prepared using multiple preparation containers, the raw material liquids B1, B2, etc. can be added to the slurry A2 in different orders, or they can be added simultaneously. In addition, the slurry A2 can be added to any raw material liquid B, and the obtained liquid can be mixed with other raw material liquids B, or the slurry A2 can be divided into multiple portions and added to each raw material liquid B, and the obtained liquids can be mixed.

[0150] In the above mixing, it is preferred to add the raw material liquid B to the slurry A2 for mixing. Specifically, it is preferred to add the raw material liquid B to the tank containing the slurry A2 for mixing. Figure 1 In the manufacturing apparatus shown, slurry A1 in tank 1 can be supplied to pump 31 to prepare slurry A2, and raw material liquid B is added from supply port 22 to slurry A2 transferred to tank 2 for mixing. It is presumed that by mixing raw material liquid B containing a cationic raw material as an additive liquid, particles more effective in improving the selectivity of methacrylic acid can be easily generated.

[0151] The temperature at which slurry A2 is mixed with raw material liquid B is not particularly limited, but is preferably 30 to 150° C. By making the temperature above 30° C., a heteropolyacid salt can be stably generated. In addition, by making the temperature below 150° C., evaporation of the solvent can be avoided, and a heteropolyacid salt can be generated in a stable environment. The lower limit of the temperature is preferably above 40° C., and the upper limit is more preferably below 100° C.

[0152] The slurry A2 and the raw material liquid B may be stirred when mixed. Examples of the stirring device include known stirring devices such as a rotary blade stirrer, a rotary stirring device, a vibrator-type linear motion stirrer, an oscillator that oscillates together with a container, and a vibration stirrer using ultrasonic waves or the like.

[0153] <Slurry C>

[0154] It is preferred that the slurry C obtained by mixing the slurry A2 and the raw material liquid B satisfies the following formula (III).

[0155] 2≤D C ≤50 (III)

[0156] In formula (III), D C The median diameter [μm] of the particle size distribution of the slurry C is shown.

[0157] When the slurry C satisfies the formula (III), pores suitable for methacrylic acid production can be formed.

[0158] The median particle size D of the particle size distribution of slurry C C The lower limit of D is preferably 2.5 μm or more, and more preferably 3 μm or more. C The upper limit of is preferably 50 μm or less, more preferably 25 μm or less, and further preferably 10 μm or less.

[0159] In addition, the half-peak width α of the particle size distribution of slurry C is C It is preferably 10 μm or less, more preferably 9 μm or less, further preferably 8 μm or less, and particularly preferably 7.5 μm or less.

[0160] Slurry C contains the metals and the like listed above for slurry A1 and raw material liquid B, but from the viewpoint of improving the selectivity in the production of methacrylic acid, the dried component preferably has a composition represented by the above formula (V). The raw material compound of the element may be added to slurry A1 and raw material liquid B so as to have the composition represented by the above formula (V), or the raw material compound of the element may be added after mixing slurry A2 and raw material liquid B.

[0161] The slurry C contains a heteropolyacid salt, and the heteropolyacid salt preferably has a Keggin structure. Since the slurry C contains a heteropolyacid salt having a Keggin structure, the generated particles are less likely to change and can exist stably, so a catalyst with high selectivity for methacrylic acid can be obtained.

[0162] As a method for obtaining the slurry C containing the heteropolyacid salt having a Keggin type structure, for example, in the above-mentioned step (i), the pH of the slurry A1 is adjusted to a low level in advance, so that the pH of the slurry C is 4 or less, preferably 3 or less. The pH of the slurry C can be set in the range of 0.1 to 4, with the lower limit preferably being 0.5 or more, more preferably 1 or more, and the upper limit preferably being 3 or less.

[0163] It should be noted that the slurry C contains a heteropolyacid salt having a Keggin-type structure, which can be confirmed by measuring the material obtained by drying the slurry C with an infrared absorption spectrum. When the slurry contains a heteropolyacid salt having a Keggin-type structure, the infrared absorption spectrum obtained is 1060, 960, 870, 780 cm -1 There are characteristic peaks nearby.

[0164] (Process (iv))

[0165] In the step (iv), the slurry C obtained in the above step (iii) is dried to obtain a dried product.

[0166] Examples of the drying method include known methods such as drum drying, airflow drying, evaporation to dryness, and spray drying. Among these, spray drying is preferably used because a granular dried product can be obtained and the dried product has a uniform spherical shape.

[0167] The drying temperature varies depending on the drying method, but can generally be 100 to 500° C., with the lower limit being preferably 140° C. or higher and the upper limit being preferably 400° C. or lower.

[0168] Drying is preferably performed so that the moisture content of the obtained dried product becomes 4.5 mass % or less, and more preferably 0.1 to 4.5 mass %.

[0169] These conditions are not particularly limited and can be appropriately selected according to the shape and size of the desired dried product.

[0170] The dried product obtained in step (iv) exhibits catalytic performance and can be used as a catalyst for producing methacrylic acid, but is preferably further subjected to shaping and calcination as described below in order to improve the performance as a catalyst. In the present invention, the materials including these shaped and calcined materials are collectively referred to as catalysts.

[0171] (Molding process)

[0172] In the molding step, the dried product obtained in the above step (iv) is molded as necessary to obtain a molded body. The molding may be performed after the calcination step described later.

[0173] The molding method is not particularly limited, and known dry and wet molding methods can be used, for example, tablet molding, pressure molding, extrusion molding, granulation molding, etc. can be mentioned. The shape of the molded product is not particularly limited, for example, cylindrical, annular, spherical and other shapes can be mentioned. In addition, during molding, it is preferred not to add a carrier to the dried product, and only the dried product is molded, but known additives such as graphite and talc can be added as needed. It should be noted that when a carrier is used, the carrier is not particularly limited, and preferably silica is mentioned.

[0174] (Calcination process)

[0175] From the viewpoint of the selectivity of methacrylic acid, it is preferred that the dried product obtained in the step (iv) and the molded body obtained in the molding step be calcined.

[0176] The calcination can be carried out under the circulation of at least one of an oxygen-containing gas such as air and an inert gas, preferably under the circulation of an oxygen-containing gas such as air. Here, the inert gas refers to a gas that does not reduce the activity of the catalyst, and nitrogen, carbon dioxide, helium, argon, etc. can be mentioned. They can be used alone or in combination of two or more.

[0177] The shape of the calcination container is not particularly limited, and a box-shaped container, a tubular container, etc. can be used. In addition, the filling and calcination can be performed in multiple containers. Among them, it is preferred to use a container with a cross-sectional area of ​​1 to 100 cm 2 Tubular container.

[0178] The calcination temperature (maximum temperature during calcination) is preferably 200 to 700°C, with the lower limit being more preferably 320°C or higher, and the upper limit being more preferably 450°C or lower.

[0179] The catalyst for producing methacrylic acid can be produced as described above.

[0180] [Method for producing methacrylic acid]

[0181] In the method for producing methacrylic acid according to the present invention, methacrylic acid is produced by oxidizing methacrolein in the presence of the catalyst for producing methacrylic acid produced by the above method. According to this method, methacrylic acid can be produced with a high selectivity.

[0182] Specifically, methacrylic acid can be produced by contacting a raw material gas containing methacrolein and oxygen with the above-mentioned catalyst for producing methacrylic acid. This reaction can usually be carried out using a fixed bed. The catalyst layer may be one layer or two or more layers. The catalyst for producing methacrylic acid may be a catalyst mixed with other additives.

[0183] The concentration of methacrolein in the raw material gas is not particularly limited, but is preferably 1 to 20% by volume, with a lower limit of more preferably 3% by volume or more, and an upper limit of more preferably 10% by volume or less. Components other than methacrolein contained in the raw material gas are not particularly limited, and examples thereof include water, oxygen, and nitrogen. It should be noted that methacrolein may contain a small amount of impurities such as lower saturated aldehydes that have no substantial effect on the reaction.

[0184] The concentration of oxygen in the raw material gas is preferably 0.4 to 4 mol relative to 1 mol of methacrolein, with a lower limit of more preferably 0.5 mol or more and an upper limit of more preferably 3 mol or less. It should be noted that, as an oxygen source, air is preferred from the viewpoint of economic efficiency. If necessary, a gas enriched in oxygen by adding pure oxygen to air may be used.

[0185] The raw material gas may be a gas obtained by diluting methacrolein and oxygen (or an oxygen source) with an inert gas such as nitrogen or carbon dioxide. In addition, water vapor may be added to the raw material gas. By reacting in the presence of water vapor, methacrylic acid can be obtained with a higher selectivity. The concentration of water vapor in the raw material gas is preferably 0.1 to 50% by volume, the lower limit is more preferably 1% by volume or more, and the upper limit is more preferably 40% by volume or less.

[0186] The contact time between the raw material gas and the catalyst for producing methacrylic acid is preferably 0.1 to 30 seconds, with the lower limit being more preferably 1 second or more, and the upper limit being more preferably 10 seconds or less.

[0187] The reaction pressure is preferably 0.1 to 1 MPa(G) or less, wherein (G) means gauge pressure.

[0188] The reaction temperature is not particularly limited, but is preferably 200 to 450°C, with a lower limit of more preferably 250°C or higher and an upper limit of more preferably 400°C or lower.

[0189] [Method for producing methacrylate]

[0190] The method for producing methacrylic acid ester according to the present invention comprises a step of esterifying methacrylic acid produced by the above method. According to this method, methacrylic acid ester can be obtained using methacrylic acid obtained by oxidation of methacrolein.

[0191] The alcohol to be reacted with methacrylic acid is not particularly limited, and examples thereof include methanol, ethanol, isopropanol, n-butanol, isobutanol, etc. Examples of the methacrylic acid ester to be obtained include methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, etc.

[0192] The esterification reaction can be carried out in the presence of an acidic catalyst such as a sulfonic acid type cation exchange resin, etc. The reaction temperature is preferably 50 to 200°C.

[0193] Example

[0194] Hereinafter, the present invention will be described in detail by way of Examples and Comparative Examples, but the present invention is not limited to these Examples. "Parts" in Examples and Comparative Examples represent parts by mass.

[0195] <Measurement of slurry particle size distribution>

[0196] The particle size distribution of the slurry was measured by laser diffraction particle size distribution measurement using a particle size distribution measuring device (trade name: SALD-7000) manufactured by Shimadzu Corporation. In the obtained volume-based particle size distribution, the peak width at 1 / 2 of the peak with the largest particle size was taken as the half-peak width, and the particle size corresponding to the cumulative 50% by volume was taken as the median particle size.

[0197] <Viscosity measurement>

[0198] The viscosity of the slurry was measured at 30° C. using a B-type viscometer (trade name: LVDV-II) manufactured by Brookfield Co., Ltd. A No. 2 spindle was used, and the measurement was performed at 30 rpm.

[0199] <Specific gravity of slurry>

[0200] The specific gravity of the slurry is calculated from the weight of the slurry filled in a 100 ml measuring cylinder with a capacity of 100 ml.

[0201] <Solid content of slurry>

[0202] The solid content of the slurry was measured by heating at 120° C. for 30 minutes using a moisture meter manufactured by Shimadzu Corporation (trade name: MOC-120H).

[0203] <Analysis of raw material gas and products>

[0204] The raw material gas and the product were analyzed by gas chromatography (apparatus: GC-2014 manufactured by Shimadzu Corporation, column: DB-FFAP manufactured by J&W, 30 m×0.32 mm, film thickness 1.0 μm).

[0205] Based on the analysis results of gas chromatography, the methacrolein conversion rate and the methacrylic acid selectivity were calculated from the following formula.

[0206] Methacrolein conversion rate (%) = ((AB) / A) × 100

[0207] Methacrylic acid selectivity (%) = (D / C) × 100

[0208] (In the formula, A is the number of carbon atoms of methacrolein in the raw material gas, B is the number of carbon atoms of methacrolein in the reaction gas after the raw material gas passes through the catalyst reaction, C is the number of carbon atoms based on the entire reaction product, and D is the number of carbon atoms of methacrylic acid generated in the reaction gas after the raw material gas passes through the catalyst reaction.)

[0209] (Production Example 1)

[0210] exist Figure 1 In the manufacturing apparatus shown, 400 parts of pure water are added to tank 1, and 100 parts of molybdenum trioxide, 7.0 parts of ammonium metavanadate, 8.0 parts of 85% phosphoric acid aqueous solution and 5.6 parts of copper (II) nitrate trihydrate are further added. The mixture is heated to 95° C. while being stirred by a stirrer 11, and then stirred for 3 hours while the liquid temperature is maintained at 95° C., thereby obtaining slurry A1 containing a heteropoly acid.

[0211] The obtained slurry A1 is: half peak width α A1 =7.2μm, median particle size D A1 =3.2μm, viscosity 15cP, specific gravity 1.16kg / L, solid content concentration 20.2% by mass.

[0212] (Example 1)

[0213] For slurry A1 obtained in Production Example 1, a volume V A1 , supplied to a centrifugal pump 31 of a turbine type, and delivered under the conditions shown in Table 1. It should be noted that the discharge pressure of the pump 31 is measured by a pressure gauge 34. Initially, the liquid is delivered in a state where the valve 33 is switched to the pipeline (piping portion 32a) on the tank 1 side in such a manner that the slurry A1 circulates from the outlet 12 of the tank 1 to the return liquid port 13 at the top of the tank 1. Next, the valve 33 is switched to the pipeline (piping portion 32b) on the tank 2 side, and all the slurry A1 is delivered from the liquid delivery supply port 24 to the tank 2, thereby preparing slurry A2. The total volume of the slurry A1 supplied to the pump 31 is set to V POMP V POMP / V A1 The values ​​are shown in Table 1.

[0214] The particle size distribution of the obtained slurry A2 and the ratio of the half-peak width of the particle size distribution of slurry A1 to slurry A2 are calculated as follows: A2 / α A1 Shown in Table 1.

[0215] Next, slurry A2 was mixed with a raw material liquid containing a cationic raw material as follows to prepare slurry C. First, slurry A2 in tank 2 was maintained at 95° C., and 8.5 parts of cesium bicarbonate dissolved in 20 parts of pure water was added from supply port 22 while stirring using a rotary blade stirrer 21, and stirred for 15 minutes. Thereafter, 15.0 parts of ammonium carbonate dissolved in 40 parts of pure water was added from supply port 22 and stirred for 15 minutes to prepare slurry C containing a heteropolyacid salt having a Keggin-type structure.

[0216] Table 1 shows the pH, half peak width, and median particle size of the obtained slurry C.

[0217] Next, the obtained slurry C was dried by spray drying to obtain a dried product. Next, the obtained dried product was press-formed and then crushed to obtain a molded body. The obtained molded body was filled into a cylindrical quartz glass calcining container with an inner diameter of 3 cm, and the temperature was raised at 10°C / h under air circulation, and calcined at 380°C for 15 hours to obtain a catalyst. It should be noted that the composition of the obtained catalyst excluding oxygen is Mo 12 P 1.2 V 1.0 Cu 0.4 Cs 0.8 .

[0218] The obtained catalyst was filled in a reaction tube, and a raw material gas of 5% by volume of methacrolein, 10% by volume of oxygen, 30% by volume of water vapor, and 55% by volume of nitrogen was flowed at a reaction temperature of 285° C. The contact time between the raw material gas and the catalyst was adjusted so that the methacrolein conversion rate became 40%, and the reaction was carried out.

[0219] The obtained product was captured and analyzed by gas chromatography to calculate the selectivity of methacrylic acid. The obtained results are shown in Table 1.

[0220] (Example 2)

[0221] The catalyst for producing methacrylic acid was produced in the same manner as in Example 1 except that the slurry A1 obtained in Production Example 1 was fed to the pump 31 under the conditions shown in Table 1, and the catalyst was used for reaction to calculate the methacrylic acid selectivity. The obtained results are shown in Table 1.

[0222] (Comparative Example 1)

[0223] Without supplying the slurry A1 obtained in Production Example 1 to the pump 31, 8.5 parts of cesium hydrogen carbonate dissolved in 20 parts of pure water were added to the slurry A1, and stirred for 15 minutes, and then 15.0 parts of ammonium carbonate dissolved in 40 parts of pure water were added, and stirred for 15 minutes to obtain slurry C. The catalyst was prepared by the same method as in Example 1 using the slurry C, and the reaction was carried out using the catalyst to calculate the methacrylic acid selectivity. The obtained results are shown in Table 1.

[0224] (Example 3)

[0225] The catalyst for producing methacrylic acid was produced in the same manner as in Example 1 except that the slurry A1 obtained in Production Example 1 was fed to the pump 31 under the conditions shown in Table 1, and the catalyst was used for reaction to calculate the methacrylic acid selectivity. The obtained results are shown in Table 1.

[0226] (Example 4)

[0227] The catalyst for producing methacrylic acid was produced in the same manner as in Example 1 except that the slurry A1 obtained in Production Example 1 was fed to the pump 31 under the conditions shown in Table 1, and the catalyst was used for reaction to calculate the methacrylic acid selectivity. The obtained results are shown in Table 1.

[0228] (Comparative Example 2)

[0229] The slurry A1 obtained in Production Example 1 was not supplied to the pump 31, and the slurry A1 was stirred at a high speed at 30°C using a homogenizer. Thereafter, 8.5 parts of cesium hydrogen carbonate dissolved in 20 parts of pure water was added, and stirred for 15 minutes, and then 15.0 parts of ammonium carbonate dissolved in 40 parts of pure water was added, and stirred for 15 minutes to prepare slurry C. Using this slurry C, a catalyst was prepared by the same method as in Example 1, and the catalyst was reacted using the catalyst to calculate the selectivity of methacrylic acid. The obtained results are shown in Table 1.

[0230] [Table 1]

[0231]

[0232] As shown in Table 1, in Examples 1 to 4 in which slurry A2 satisfying a predetermined particle size distribution was prepared, it was confirmed that a catalyst having a high selectivity for methacrylic acid was obtained. From these results, it is understood that by preparing slurry A2 satisfying a predetermined particle size distribution, a heteropolyacid salt can be uniformly formed in the preparation of slurry C, and a desired catalyst for methacrylic acid production can be produced.

[0233] In addition, as shown in Examples 1 to 4, when slurry A2 is prepared by supplying slurry A1 to a pump, V is adjusted according to the supply speed of slurry A1 to the pump. POMP / V A , which can produce a catalyst with high selectivity for methacrylic acid.

[0234] On the other hand, in Comparative Example 1 in which the step of producing slurry A2 having a predetermined particle size distribution was not performed, the methacrylic acid selectivity of the obtained catalyst was low.

[0235] Furthermore, when shearing force was applied to slurry A1 using a homogenizer as in Comparative Example 2, particles in slurry A1 were broken, and as a result, slurry A2 satisfying a predetermined median particle size could not be prepared, and the obtained catalyst had a low selectivity for methacrylic acid.

[0236] Industrial Applicability

[0237] According to the present invention, a catalyst capable of achieving a high methacrylic acid selectivity in the production of methacrylic acid can be provided, and thus the present invention is industrially useful.

[0238] Explanation of symbols

[0239] 1 slot

[0240] 11. Blender

[0241] 12 Take the exit

[0242] 13 Liquid return port

[0243] 2 slots

[0244] 21. Blender

[0245] 22 Supply port

[0246] 23 Take the exit

[0247] 24 Liquid supply port

[0248] 31 Pump

[0249] 32 piping

[0250] 32a, 32b Piping section

[0251] 33 Two-way valve

[0252] 34 Pressure gauge

Claims

1. A method for producing a catalyst for producing methacrylic acid, which is a method for producing a catalyst used when producing methacrylic acid by oxidizing methacrolein, comprising the following steps: (i) a step of preparing a slurry A1 containing a heteropoly acid or a salt thereof, wherein the heteropoly acid or a salt thereof contains at least phosphorus, molybdenum, vanadium and copper, (ii) a step of using the slurry A1 to prepare a slurry A2 satisfying the following formulas (I) and (II), (iii) a step of mixing the slurry A2 with a raw material solution B containing a cationic raw material to prepare a slurry C, and (iv) a step of drying the slurry C, α A2 / α A1 ≤0.95(I) 2≤D A2 ≤50(II) In formula (I), α A1 represents the half-peak width of the particle size distribution of the slurry A1, α A2 represents the half-peak width of the particle size distribution of the slurry A2. In addition, in formula (II), D A2 represents the median particle size of the particle size distribution of the slurry A2, wherein, The unit of half peak width and median particle size is μm. In the step (ii), the slurry A2 is prepared by supplying the slurry A1 to a pump. The volume of the slurry A1 prepared in the step (i) is defined as V. A1 , the total volume of the slurry A1 supplied to the pump is V POMP When the step (iii) is started, V POMP / V A1 is 0.1 or more, The cation raw material is at least one selected from a compound containing an alkali metal and a compound containing an ammonium ion.

2. The method for producing a catalyst for producing methacrylic acid according to claim 1, wherein Satisfies the following formula (III), 2≤D C ≤50(III) In formula (III), D C It represents the median particle size of the particle size distribution of the slurry C, and the unit of the median particle size is μm.

3. The method for producing a catalyst for producing methacrylic acid according to claim 1 or 2, wherein: Satisfies the following formula (IV), 0.6≤D A2 / D A1 <1.0(IV) In formula (IV), D A1 represents the median particle size of the particle size distribution of the slurry A1, D A2 It represents the median particle size of the particle size distribution of the slurry A2, and the unit of the median particle size is μm.

4. The method for producing a catalyst for producing methacrylic acid according to claim 1 or 2, wherein: In the step (iii), V at the time of starting to mix the raw material solution B is POMP / V A1 It is 1.0~10.

0.

5. The method for producing a catalyst for producing methacrylic acid according to claim 1 or 2, wherein: In the step (iii), V at the time of starting to mix the raw material solution B is POMP / V A1 Greater than 1.

0.

6. The method for producing a catalyst for producing methacrylic acid according to claim 1 or 2, wherein: The supply rate of the slurry A1 to the pump is 1 L / min or more.

7. The method for producing a catalyst for producing methacrylic acid according to claim 1 or 2, wherein: The pump is a turbine pump or a reciprocating pump.

8. The method for producing a catalyst for producing methacrylic acid according to claim 1 or 2, wherein When the tank for preparing the slurry A1 in the step (i) is referred to as tank 1, and the tank for mixing the slurry A2 and the raw material liquid B in the step (iii) is referred to as tank 2, the tank 1 and the tank 2 are different tanks.

9. The method for producing a catalyst for producing methacrylic acid according to claim 8, wherein The tank 1 and the tank 2 are connected by pipes.

10. The method for producing a catalyst for producing methacrylic acid according to claim 9, wherein The pump is provided in the pipe.

11. The method for producing a catalyst for producing methacrylic acid according to claim 1 or 2, wherein: The viscosity of the slurry A1 at 30° C. is 1 to 200 cP.

12. The method for producing a catalyst for producing methacrylic acid according to claim 1 or 2, wherein: The solid content concentration of the slurry A1 is 5 to 60% by mass.

13. The method for producing a catalyst for producing methacrylic acid according to claim 1 or 2, wherein: The catalyst has a composition represented by the following formula (V): P a With b V c Cu d X e Y f Z g (NH4) h OF i (V) In the formula, P, Mo, V, Cu, NH4 and O represent phosphorus, molybdenum, vanadium, copper, ammonium and oxygen respectively, X represents at least one element selected from silicon, titanium, germanium, arsenic, antimony and bismuth, Y represents at least one element selected from niobium, tantalum, tungsten, cerium, zirconium, silver, iron, zinc, chromium, magnesium, cobalt, manganese, barium and lanthanum, Z represents at least one element selected from lithium, sodium, potassium, rubidium and cesium, a~i represents the molar ratio of each component, when b=12, a=0.5~3, c=0.01~3, d=0.01~2, e=0.1~3, f=0~3, g=0.01~3, h=0~20, and i is the molar ratio of oxygen required to satisfy the valence number of each component. 14 . A method for producing methacrylic acid, comprising oxidizing methacrolein in the presence of a catalyst produced by the method according to claim 1 .

15. A method for producing a methacrylic acid ester, comprising esterifying methacrylic acid produced by the method according to claim 14.

16. A manufacturing device for a catalyst for producing methacrylic acid, the manufacturing device being used in the method for producing a catalyst for producing methacrylic acid according to claim 1, and being a manufacturing device for a catalyst used when methacrylic acid is produced by oxidizing methacrolein, comprising: A tank 1 is prepared containing a slurry A1 at least comprising phosphorus, molybdenum, vanadium and copper, A mechanism for preparing slurry A2 satisfying the following formulae (I) and (II) using the slurry A1, and Tank 2 for mixing the slurry A2 with a raw material liquid B containing a cationic raw material, α A2 / α A1 ≤0.95(I) 2≤D A2 ≤50(II) In formula (I), α A1 represents the half-peak width of the particle size distribution of the slurry A1, α A2 represents the half-peak width of the particle size distribution of the slurry A2. In addition, in formula (II), D A2 represents the median particle size of the particle size distribution of the slurry A2, wherein, The unit of half peak width and median particle size is μm. The cation raw material is at least one selected from a compound containing an alkali metal and a compound containing an ammonium ion.

17. The production apparatus for a catalyst for producing methacrylic acid according to claim 16, wherein The tank 1 and the tank 2 are connected by pipes.

18. The production apparatus for a catalyst for producing methacrylic acid according to claim 17, wherein The pipe is provided with a pump.

Citation Information

Patent Citations

  • Production of catalyst for production of methacrylic acid

    JP1995185354A

  • Method for producing catalyst for methacrylic acid production, method for producing methacrylic acid and method for producing methacrylic acid ester

    WO2018037998A1

  • Method for producing methacrylic acid production catalyst, method for producing methacrylic acid, and method for producing methacrylic acid ester

    CN109311005A

  • Method for producing catalyst for methacrylic acid production, method for producing methacrylic acid and method for producing methacrylic acid ester

    CN109641202A

  • Layered lithium nickel composite oxide powder and process for producing the same

    CN1698223A