Dual laser chipping method and device

The formation of micro-cracks in brittle materials through dual-laser combination technology solves the problems of high cost and low efficiency of wafer separation of third-generation semiconductor materials, achieves efficient and low-cost splitting process and low-roughness surface treatment, and meets the needs of high-end customers. Quality device production requirements.

CN114985990BActive Publication Date: 2024-10-22INST OF SEMICONDUCTORS - CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210826507.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-14
Publication Date
2024-10-22
Estimated Expiration
2042-07-14

AI Technical Summary

Technical Problem

The wafer separation technology of third-generation semiconductor materials has problems such as high cost, low efficiency and surface damage. The traditional diamond wire cutting process cannot meet the rapid development needs of high-quality devices.

Method used

Using a dual laser splitting method and device, through a combination of ultra-short pulse laser and short pulse or continuous laser, high peak power and thermal characteristics are used to form micro-cracks in brittle materials, achieving uniform expansion of the material and low-roughness surface treatment.

Benefits of technology

It improves the material splitting efficiency, reduces production costs, reduces subsequent grinding and polishing time, and improves processing efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114985990B_ABST
    Figure CN114985990B_ABST
Patent Text Reader

Abstract

The present invention discloses a dual laser splitting method and device, which is a method and device for splitting brittle materials, and utilizes the high peak power and "cold processing" characteristics of ultrashort pulse laser beams to absorb nonlinearly in the material, so that local positions of the material are exploded, forming microcracks to achieve material modification, and then utilizes the thermal characteristics of short pulse laser beams or continuous laser beams to achieve uniform expansion of cracks inside the material, and finally obtains a material surface with low surface roughness. Due to the low surface roughness of the material, the subsequent processing time can be greatly reduced during grinding and polishing, which has a qualitative improvement in processing efficiency and reduces production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of laser splitting technology, and in particular to a dual laser splitting device and a dual laser splitting method. Background Art

[0002] The third generation of semiconductor materials is represented by wide bandgap compound semiconductors such as silicon carbide, gallium nitride and diamond. Its crystal growth process is complex, its hardness is high, and its production cost is high, which leads to the high cost of third generation semiconductor wafers, becoming one of the bottleneck problems hindering the rapid development of third generation semiconductor devices. Taking silicon carbide as an example, the traditional wafer separation technology adopts diamond wire cutting process. The diamond wire has a slow scribing speed, high cutting cost, wide kerf width, serious cutting loss of about 50%, and deep damage layer on the surface of the cut piece, and there are different degrees of line marks. Eliminating all these defects requires expensive subsequent processes, such as grinding, mechanical polishing, chemical polishing, etc. The traditional cracking process is far from meeting the needs of the rapid development of high-quality third generation semiconductor devices. Compared with mechanical methods, laser processing has many advantages, such as no mechanical stress and no contact during the processing process, which can achieve high-quality and high-precision processing, and is suitable for processing hard and brittle materials. Therefore, more precise laser scribing equipment and processes are urgently needed to provide effective support for the third generation semiconductor industry.

[0003] Laser cold cracking technology uses a pulsed laser to pass through a series of optical systems to focus the laser on the interior of a brittle transparent material. Based on the multiphoton effect and avalanche ionization effect, a modified layer is formed inside the material. At the same time, the difference in thermal expansion coefficients between the brittle material and the polymer material adhered to the surface of the material is used to perform rapid cooling and other treatments to induce thermal stress, forming a crack layer inside the material, and finally obtaining an ultra-thin wafer. However, the split surface roughness obtained by the ultrafast laser cold cracking technology in related technologies is usually large, and the material and wafer need to be polished, ground and other processes subsequently, which reduces production efficiency and increases production costs. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, an embodiment of the present invention provides a dual laser cleavage method with high cleavage efficiency and low cost.

[0005] The embodiment of the present invention further provides a dual-laser chipping device with high chipping efficiency and low cost.

[0006] The dual laser splitting method of the embodiment of the present invention is a method for splitting a brittle material using a dual laser splitting device, wherein the dual laser splitting device includes a short pulse or continuous laser, an ultrashort pulse laser, a beam expander and a beam focuser, and the splitting method includes the following steps:

[0007] Setting the emission interval time of the ultrashort pulse laser and the short pulse or continuous laser, wherein the interval time is greater than or equal to 0s;

[0008] The ultrashort pulse laser emits an ultrashort pulse laser beam, and the ultrashort pulse laser beam passes through the beam expander and then is focused into the brittle material by the beam focuser;

[0009] Adjusting the depth of the focus of the laser beam in the brittle material, so that the ultrashort pulse laser beam forms cracks inside the brittle material through nonlinear absorption;

[0010] The short pulse or continuous laser emits a short pulse laser beam or a continuous laser beam after a preset interval time, and the short pulse laser beam or the continuous laser beam passes through the beam expander and is focused into the brittle material by the beam focuser;

[0011] Under the thermal characteristics of a short-pulse laser beam or a continuous laser beam, the crack spreads uniformly to the surroundings;

[0012] The position of the focus of the laser beam in the brittle material is adjusted in a certain path to etch the entire brittle material, so that the brittle material is split into a target wafer and remaining materials.

[0013] The dual laser cracking method provided by the embodiment of the present invention utilizes the high peak power and "cold processing" characteristics of the ultrashort pulse laser beam to absorb the nonlinear material, so that the local position of the material explodes, forming microcracks to achieve material modification, and then utilizes the thermal characteristics of the short pulse laser beam or the continuous laser beam to achieve uniform expansion of the cracks inside the material, and finally obtains a material surface with low surface roughness. Due to the low surface roughness of the material, the subsequent processing time can be greatly reduced during grinding and polishing, which has a qualitative improvement in processing efficiency and reduces production costs.

[0014] In some embodiments, the dual laser splitting device includes an X-axis moving axis, a Y-axis moving axis, and a Z-axis moving axis, wherein the X-axis moving axis is used to control the movement of the focus of the laser beam on the X-axis, the Y-axis moving axis is used to control the movement of the focus of the laser beam on the Y-axis, and the Z-axis moving axis is used to control the movement of the focus of the laser beam on the Z-axis, wherein the Z-axis is in a direction approaching or moving away from the brittle material, and the X-axis, the Y-axis, and the Z-axis are perpendicular to each other;

[0015] The step of adjusting the depth of the focus of the laser beam in the brittle material specifically includes adjusting the Z-axis moving axis so that the focus of the laser beam is located at a preset depth in the brittle material;

[0016] The step of adjusting the position of the focus of the laser beam in the brittle material along a certain path specifically includes adjusting the X-axis moving axis and the Y-axis moving axis to allow the focus of the laser beam to scan and etch the brittle material along a certain path.

[0017] In some embodiments, the brittle material is silicon carbide, gallium nitride, diamond, or a material composed of one or more elements of Group IV, Group III and Group V, Group II and Group VI.

[0018] In some embodiments, the pulse width of the short pulse or continuous laser is picoseconds, sub-picoseconds or femtoseconds, and the pulse width of the ultrashort pulse laser is picoseconds, sub-picoseconds or femtoseconds; and / or, the pulse forms of the short pulse or continuous laser and the ultrashort pulse laser are single pulse, double pulse or multiple pulses.

[0019] Another aspect of the present invention provides a dual laser splitting device, comprising: a short pulse or continuous laser, the short pulse or continuous laser is used to provide a short pulse laser beam or a continuous laser beam; an ultrashort pulse laser, the ultrashort pulse laser is used to provide an ultrashort pulse laser beam; a beam expander and a beam focuser, the beam expander is located on the output optical path of the short pulse or continuous laser and the ultrashort pulse laser and is used to expand the laser beam, the beam focuser is located on the output optical path of the optical beam expander and is used to focus the laser beam; an operating table, the operating table is used to place a brittle material, the beam focuser focuses the laser beam inside the brittle material; and a moving component, the moving component is used to control the movement of at least one of the operating table and the beam focuser to control the position of the focus of the laser beam inside the brittle material.

[0020] The dual laser splitting device provided by the embodiment of the present invention utilizes the high peak power and "cold processing" characteristics of the ultrashort pulse laser beam to absorb nonlinearly in the material, causing explosions at local locations of the material to form microcracks to achieve material modification, and then utilizes the thermal characteristics of the short pulse laser beam or continuous laser beam to achieve uniform expansion of cracks inside the material, ultimately obtaining a material surface with low surface roughness. Due to the low surface roughness of the material, the subsequent processing time can be greatly reduced during grinding and polishing, which has a qualitative improvement in processing efficiency and reduces production costs.

[0021] In some embodiments, the dual laser splitting device includes a signal generator, which is signal-connected to both the short pulse or continuous laser and the ultrashort pulse laser, and is used to control the interval time between the laser emission of the short pulse or continuous laser and the ultrashort pulse laser.

[0022] In some embodiments, the dual laser splitting device includes a first dichroic mirror, which is located in the output optical path of the short pulse or continuous laser and the ultrashort pulse laser, and is used to make the laser beam input into the beam expander in the same direction by reflection or transmission.

[0023] In some embodiments, the ultrashort pulse laser, the first dichroic mirror and the beam expander are located on the same straight line, and the first dichroic mirror is used to transmit the ultrashort pulse laser beam emitted by the ultrashort pulse laser; the short pulse or continuous laser is located on one side of the ultrashort pulse laser, and the dual laser splitting device also includes a reflector, which is located on the output optical path of the short pulse or continuous laser and is used to reflect the short pulse laser beam or the continuous laser beam onto the first dichroic mirror, and the first dichroic mirror is used to reflect the short pulse laser beam or the continuous laser beam.

[0024] In some embodiments, the dual laser splitting device further includes: an illumination light source, which is used to emit an illumination light beam to the beam focuser, and the beam focuser is also used to focus the illumination light beam in the brittle material so that the brittle material reflects the illumination light beam; an imaging system, which is located in the reflected light path of the illumination light beam and is used to monitor the focal position of the laser beam.

[0025] In some embodiments, the output optical path of the beam expander is perpendicular to the output optical path of the beam focuser, the output optical path of the beam focuser is perpendicular to the brittle material, the imaging system is located directly above the brittle material, and the dual laser splitting device further includes: a second dichroic mirror, the second dichroic mirror is located on the output optical path of the beam expander and below the imaging system, the second dichroic mirror is used to reflect the laser beam output by the beam expander to the beam focuser, and is also used to transmit the reflected light of the illumination beam; and a semi-transparent and semi-reflective mirror, the semi-transparent and semi-reflective mirror is located below the imaging system, and is used to reflect the illumination beam emitted by the illumination light source to the beam focuser, and is also used to transmit the reflected light of the illumination beam.

[0026] In some embodiments, the semi-transparent and semi-reflective mirror is located above the second dichroic mirror, so that the illumination light beam is reflected by the semi-transparent and semi-reflective mirror and then transmitted from the second dichroic mirror to the light beam focuser.

[0027] In some embodiments, the moving assembly includes an X-axis moving axis, a Y-axis moving axis, and a Z-axis moving axis, wherein the X-axis moving axis is used to control the movement of the focus of the laser beam on the X-axis, the Y-axis moving axis is used to control the movement of the focus of the laser beam on the Y-axis, and the Z-axis moving axis is used to control the movement of the focus of the laser beam on the Z-axis. The XY axis linkage determines the scanning mode, which is circular, elliptical, annular, rectangular, "bow" or Archimedean spiral.

[0028] In some embodiments, the X-axis moving axis and the Y-axis moving axis act on the operating table, the Z-axis moving axis acts on the beam focuser, the Z-axis is in a direction approaching or moving away from the brittle material, and the X-axis, the Y-axis and the Z-axis are perpendicular to each other. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Schematic diagram of the structure of a dual laser splitting device provided in an embodiment of the present invention.

[0030] Reference numerals:

[0031] Signal generator 1, short pulse or continuous laser 2, ultrashort pulse laser 3, reflector 4, first dichroic mirror 5, beam expander 6, laser beam 7, second dichroic mirror 8, beam focuser 9, brittle material 10, operating table 11, moving platform 12, controller 13, Z-axis moving axis 14, illumination light source 15, illumination beam 16, semi-transparent and semi-reflective mirror 17, imaging system 18. DETAILED DESCRIPTION

[0032] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0033] According to the following Figure 1 The dual laser splitting device provided in an embodiment of the present invention and the method for splitting a brittle material using the dual laser splitting device are described, wherein the dual laser splitting device includes a short pulse or continuous laser 2, an ultrashort pulse laser 3, a beam expander 6 and a beam focuser 9, an operating table 11 and a moving component.

[0034] The short pulse or continuous laser 2 is used to provide a short pulse laser beam or a continuous laser beam. The short pulse or continuous laser 2 can be a short pulse laser that emits a short pulse laser beam, or a continuous laser that emits a continuous laser beam. The ultrashort pulse laser 3 is used to provide an ultrashort pulse laser beam.

[0035] The beam expander 6 is located on the output optical path of the short pulse or continuous laser 2 and the ultrashort pulse laser 3 and is used to expand the laser beam, that is, the short pulse laser beam or the continuous laser beam emitted by the short pulse or continuous laser 2 is diffused through the beam expander 6, and the ultrashort pulse laser beam emitted by the ultrashort pulse laser 3 is diffused through the beam expander 6. The beam focuser 9 is located on the output optical path of the optical beam expander 6 and is used to focus the laser beam.

[0036] The operating table 11 is used to place the brittle material 10, and the beam focuser 9 focuses the laser beam inside the brittle material 10, that is, the beam focuser 9 focuses the short pulse laser beam or the continuous laser beam, the ultrashort pulse laser beam inside the brittle material 10 to split the brittle material 10 and obtain a wafer with a certain thickness.

[0037] The moving component is used to control the movement of at least one of the operating table 11 and the beam focuser 9 to control the position of the focus of the laser beam inside the brittle material 10. That is, by manipulating the moving component, the position of the focus of the laser beam inside the brittle material 10 can be adjusted, including adjusting the depth of the focus of the laser beam inside the brittle material 10, thereby controlling the thickness of the target wafer, and also including adjusting the position of the focus of the laser beam at the same depth in the brittle material 10, thereby performing a comprehensive scan and etching of the brittle material 10, so that the wafer is peeled off from the main body. The "depth of the focus of the laser beam in the brittle material 10" specifically refers to the distance between the focus of the laser beam and the upper surface of the brittle material 10 in the thickness direction of the brittle material 10.

[0038] Optionally, the pulse forms of the short pulse or continuous laser 2 and the ultrashort pulse laser 3 include single pulse, double pulse and multi-pulse, etc., and the pulse width includes continuous light, milliseconds, microseconds, nanoseconds, sub-nanoseconds, picoseconds, sub-picoseconds and femtoseconds, etc.

[0039] The function of the beam expander 6 is to expand the beam directly emitted by the laser, and it may optionally include a single lens, a single beam expander, a lens combination, a 4f system, etc.

[0040] The beam focuser 9 focuses the laser beam expanded by the beam expander 6, and may optionally include a single focusing lens, a focusing lens group, a micro-machining objective lens, and the like.

[0041] The brittle material 10 has relatively high hardness and brittleness, and may optionally include silicon carbide, gallium nitride, diamond, or a material composed of one or more elements of Group IV, Group III and Group V, Group II and Group VI.

[0042] Optionally, the operating table 11 is an adsorption table, which is used to adsorb the brittle material 10 on the vacuum adsorption table to ensure that the lower surface of the material does not warp during processing. In some embodiments, the brittle material 10 is located above the operating table 11, and the beam focuser 9 vertically injects the laser beam into the brittle material 10, that is, the incident direction of the laser beam is perpendicular to the plane where the brittle material 10 is located.

[0043] The dual laser chip splitting method provided by the embodiment of the present invention comprises the following steps:

[0044] Setting the emission interval time between the ultrashort pulse laser 3 and the short pulse or continuous laser 2, the interval time is greater than or equal to 0s, that is, the ultrashort pulse laser 3 and the short pulse or continuous laser 2 can emit laser beams at the same time or at an interval;

[0045] Placing a brittle material 10 on an operating table 11;

[0046] The ultrashort pulse laser 3 emits an ultrashort pulse laser beam, which passes through a beam expander 6 and is focused by a beam focuser 9, so that the spot diameter after focusing is less than 5 microns, preferably less than 4 microns, and more preferably less than 3 microns;

[0047] The depth of the focus of the laser beam in the brittle material 10 is adjusted by moving the component, and the depth is determined by the thickness of the target wafer. Optionally, the depth of the focus of the laser beam in the brittle material 10 is 250 microns or 175 microns;

[0048] The ultrashort pulse laser beam achieves material modification through nonlinear absorption, forming cracks inside the brittle material 10;

[0049] The short pulse or continuous laser 2 emits a short pulse laser beam or a continuous laser beam after a preset interval time, and the short pulse laser beam or the continuous laser beam passes through the beam expander 6 and is focused by the beam focuser 9;

[0050] Under the thermal characteristics of the short-pulse laser beam or the continuous laser beam, the cracks formed inside the brittle material 10 spread evenly to the surroundings, thereby reducing the externally applied stress during the splitting, and obtaining a material surface with a lower surface roughness after the splitting;

[0051] The focus of the laser beam is adjusted in a certain path by moving the component to etch the entire brittle material 10, that is, the brittle material 10 is scanned to split the brittle material into a target wafer and remaining material, and the target wafer is peeled off from the remaining material.

[0052] In some embodiments, the step of polishing the surface of the remaining material is also included to prepare for the next cycle of splitting operation.

[0053] The dual laser cracking method provided by the embodiment of the present invention utilizes the high peak power and "cold processing" characteristics of the ultrashort pulse laser beam to absorb the nonlinear material, so that the local position of the material explodes, forming microcracks to achieve material modification, and then utilizes the thermal characteristics of the short pulse laser beam or the continuous laser beam to achieve uniform expansion of the cracks inside the material, and finally obtains a material surface with low surface roughness. Due to the low surface roughness of the material, the subsequent processing time can be greatly reduced during grinding and polishing, which has a qualitative improvement in processing efficiency and reduces production costs.

[0054] In some embodiments, Figure 1 As shown, the dual laser splitting device includes a signal generator 1, which is signal-connected to both the short pulse or continuous laser 2 and the ultrashort pulse laser 3, and is used to control the interval time between the short pulse or continuous laser 2 and the ultrashort pulse laser 3 in emitting laser light. One port of the signal generator 1 can output two control signals at the same time, and the interval time between the ultrashort pulse laser 3 and the short pulse or continuous laser 2 can be set through the signal generator 1.

[0055] In some embodiments, the dual laser splitting device includes a first dichroic mirror 6, which is located on the output optical path of the short pulse or continuous laser 2 and the ultrashort pulse laser 3, and is used to make the laser beams input into the beam expander 6 along the same direction by reflection or transmission. That is, the short pulse or continuous laser beam emitted by the short pulse or continuous laser 2 is input into the beam expander 6 along the first direction after reflection or transmission by the first dichroic mirror 6, and the ultrashort pulse laser beam emitted by the ultrashort pulse laser 3 is input into the beam expander 6 along the first direction after reflection or transmission by the first dichroic mirror 6, so that both the short pulse or continuous laser beam and the ultrashort pulse laser beam can be expanded by the beam expander 6.

[0056] As an example, Figure 1 As shown, the ultrashort pulse laser 3, the first dichroic mirror 5 and the beam expander 6 are located on the same straight line. The first dichroic mirror 5 is used to transmit the ultrashort pulse laser beam emitted by the ultrashort pulse laser 3, that is, the ultrashort pulse laser beam emitted by the ultrashort pulse laser 3 is transmitted by the first dichroic mirror 6 and then input into the beam expander 6 along the first direction. The short pulse or continuous laser 2 is located on one side of the ultrashort pulse laser 3 ( Figure 1 The short pulse or continuous laser 2 emits a short pulse or continuous laser beam along a first direction. It can be understood that the short pulse or continuous laser beam emitted by the short pulse or continuous laser 2 is located above the ultrashort pulse laser beam emitted by the ultrashort pulse laser 3.

[0057] In order to make the short pulse or continuous laser beam reach the beam expander 6. Figure 1As shown, the dual laser splitting device further includes a reflector 4, which is located on the output optical path of the short pulse or continuous laser 2 and is used to reflect the short pulse laser beam or the continuous laser beam onto the first dichroic mirror 5, and the first dichroic mirror 5 is used to reflect the short pulse laser beam or the continuous laser beam. Figure 1 Taking the embodiment shown in the figure as an example, the reflector 4 is located directly above the first dichroic mirror 5. The short pulse or continuous laser beam emitted by the short pulse or continuous laser 2 is reflected by the reflector 4 and then emitted vertically downward to the first dichroic mirror 5. After being reflected by the first dichroic mirror 5, it is incident on the beam expander 6 along the first direction. The reflective surface of the reflector 4 is Figure 1 The 45° setting shown in the figure shows that the reflecting surface of the first dichroic mirror 5 is Figure 1 45° setting shown.

[0058] Of course, it is understandable that in other embodiments, the laser beam can be input into the beam expander 6 along the same direction by other means. Figure 1 The illustrated embodiments are merely examples and are not intended to limit the present invention.

[0059] Furthermore, in order to monitor the damage of the crack surface during the processing and determine the focus depth of the laser beam in the brittle material 10, in some embodiments, the dual laser cracking device further includes an illumination light source 15 and an imaging system 18. The illumination light source 15 is used to provide illumination so that the imaging system 18 can clearly reflect the focus position.

[0060] Specifically, the illumination light source 15 is used to emit an illumination light beam 16 to the beam focuser 9, and the beam focuser 9 is also used to focus the illumination light beam 16 in the brittle material 10 so that the brittle material 10 reflects the illumination light beam 16. The imaging system 18 is located in the reflected light path of the illumination light beam 16 and is used to monitor the focal position of the laser beam.

[0061] As an example, Figure 1 As shown, the output optical path of the beam expander 6 and the output optical path of the beam focuser 9 are perpendicular to each other, and the output optical path of the beam focuser 9 and the brittle material 10 are perpendicular to each other, that is, the output optical path of the beam expander 6 is along the horizontal direction, and the output optical path of the beam focuser 9 is along the vertical direction, and is vertically incident on the brittle material 10. The dual laser splitting device also includes a second dichroic mirror 8 located on the output optical path 7 of the beam expander 6. The second dichroic mirror 8 is used to reflect the horizontally extending laser beam output by the beam expander 6, so that the laser beam changes its path to be emitted downward in the vertical direction and is input into the beam focuser 9. The laser beam 9 is focused by the beam focuser 9 and input downward into the brittle material.

[0062] like Figure 1As shown, the imaging system 18 is located directly above the brittle material 10, and is used to receive the light reflected from the brittle material 10 (the reflected light of the laser and the illumination light). The second dichroic mirror 8 is located below the imaging system 18, and the second dichroic mirror 8 is also used to transmit the reflected light of the illumination light beam, that is, after the illumination light beam is reflected by the brittle material 10, it is emitted upward in the vertical direction, and is received by the imaging system 18 after passing through the second dichroic mirror 8.

[0063] The dual laser splitting device further includes a semi-transparent and semi-reflective mirror 17, which is located below the imaging system 18. The semi-transparent and semi-reflective mirror 17 is used to reflect the illumination beam 16 emitted by the illumination light source 15 to the beam focuser 9, and is also used to transmit the reflected light of the illumination beam. Figure 1 As shown, the illumination light source 15 emits an illumination light beam 16 toward the semi-transparent and semi-reflective mirror 17 in the horizontal direction. After being reflected by the semi-transparent and semi-reflective mirror 17, the illumination light beam 16 changes its path to be emitted vertically downward and is input into the beam focuser 9. After being focused by the beam focuser 9, it reaches the brittle material. The reflected light after being reflected by the brittle material 10 is transmitted vertically upward through the second dichroic mirror 8 and the semi-transparent and semi-reflective mirror 17 and is received by the imaging system 18.

[0064] exist Figure 1 In the illustrated embodiment, the semi-transparent and semi-reflective mirror 17 is located above the second dichroic mirror 8, so that the illumination light beam 16 is reflected by the semi-transparent and semi-reflective mirror 17 and then transmitted from the second dichroic mirror 8 to the input light beam focuser 9. The reflected light reflected by the brittle material 10 is vertically transmitted upward through the second dichroic mirror 8 and the semi-transparent and semi-reflective mirror 17 in sequence and then received by the imaging system 18.

[0065] In other embodiments, the semi-transparent mirror 17 can also be below the second dichroic mirror 8, and the illumination light beam 16 is directly input into the beam focuser 9 after being reflected by the semi-transparent mirror 17. The reflected light reflected by the brittle material 10 is vertically transmitted upward through the semi-transparent mirror 17 and the second dichroic mirror 8 in sequence and then received by the imaging system 18.

[0066] In some embodiments, the moving assembly includes an X-axis moving axis, a Y-axis moving axis, and a Z-axis moving axis. The X-axis moving axis is used to control the movement of the focus of the laser beam on the X-axis, the Y-axis moving axis is used to control the movement of the focus of the laser beam on the Y-axis, and the Z-axis moving axis is used to control the movement of the focus of the laser beam on the Z-axis.

[0067] As an example, the X-axis moving axis and the Y-axis moving axis act on the operating table 11, and the Z-axis moving axis acts on the beam focuser 9, and the Z-axis is a direction close to or away from the brittle material 10 ( Figure 1 The X-axis, the Y-axis and the Z-axis are perpendicular to each other, and the X-axis and the Y-axis are both in the horizontal direction, that is, they are parallel to the plane where the brittle material 10 is located.

[0068] use Figure 1In the method for splitting by the dual laser splitting device shown in , the step of adjusting the depth of the focus of the laser beam in the brittle material 10 by moving the assembly specifically includes adjusting the Z-axis moving shaft 14 so that the focus of the laser beam is located at a preset depth in the brittle material 10. The step of adjusting the position of the focus of the laser beam in the brittle material 10 along a certain path by moving the assembly specifically includes adjusting the X-axis moving shaft and the Y-axis moving shaft so that the focus of the laser beam scans and etches the brittle material 10 along a certain path.

[0069] Specifically, in Figure 1 In the embodiment shown, the moving assembly includes a moving platform 12, the operating table 11 is located on the moving platform 12, and the moving platform 12 includes the X-axis moving axis and the Y-axis moving axis. By manipulating the moving platform 12, the operating table 11 and the brittle material 10 adsorbed on the operating table 11 can be moved, so as to control the focus of the laser beam to move along the X-axis and the Y-axis. The moving platform 12 is mainly used to operate when scanning the brittle material 10, and is used to control the scanning direction and the scanning interval. The Z-axis moving axis 14 acts on the beam focuser 9 to make the beam focuser 9 rise or fall in the vertical direction to adjust the depth of the focus of the laser beam in the brittle material 10.

[0070] Furthermore, the dual laser splitting device includes a controller 13 , which is connected to each of the Z-axis moving shaft 14 and the moving platform 12 , and is used to control the operation of the Z-axis moving shaft 14 and the moving platform 12 .

[0071] During the laser scanning process, the laser scanning mode and scanning interval must be strictly controlled. The controller 13 mainly determines the scanning mode, and the scanning mode can be circular, elliptical, annular, rectangular, "bow" shape and Archimedean spiral.

[0072] The dual laser splitting method provided by the present invention is further described in detail below in conjunction with specific embodiments, taking the third generation brittle semiconductor silicon carbide material as an example.

[0073] Embodiment 1:

[0074] A "bow"-shaped scan is adopted, and short pulse laser or continuous laser is loaded simultaneously with the incident ultrashort pulse laser, that is, the interval emission time is adjusted to 0s through the signal generator 1.

[0075] 1. The silicon carbide wafer (brittle material 10) purchased on the market is 4H-SiC or 6H-SiC. The size of the silicon carbide wafer is 6 inches or 8 inches, and the thickness is 500μm or 350μm;

[0076] 2. If Figure 1As shown, the wavelength of the ultrashort pulse laser 3 is 1064nm or 1050nm or 808nm or 532nm, the repetition frequency is 10MHz or 1MHz or 500kHz, the power is 100W or 10W or 5W or 2.5W or 1W, the pulse is selected to be a single pulse, a double pulse or a multi-pulse, etc., the pulse width is selected to be picoseconds or sub-picoseconds or femtoseconds, and the diameter of the laser beam 7 passing through the beam expander 6 is limited by the beam focuser 9 to meet the clear aperture of the focusing system;

[0077] 3. After being reflected by the second dichroic mirror 8, the laser beam 7 enters the beam focuser 9 to focus the laser. After focusing, the laser is focused at a certain depth from the upper surface of the silicon carbide wafer. The thickness is determined according to the imaging system 18 and the Z-axis moving axis 14, and the depth is 250μm or 175μm;

[0078] 4. While the ultrashort pulse laser beam is being emitted, the short pulse or continuous laser 2 is made to emit a short pulse laser beam or a continuous laser beam, and the laser beam is simultaneously loaded inside the material. After the ultrashort pulse laser forms microcracks through nonlinear absorption, the thermal characteristics of the short pulse laser or the continuous laser are used to make the microcracks diffuse evenly around the laser etching line, and the moving platform 12 is adjusted to etch the entire material in a "bow" shape, and finally a surface with a lower surface roughness of the material is obtained after the material is separated;

[0079] 6. After the material is separated, the rough part of the material surface needs to be ground and polished. Due to the low surface roughness of the material, the grinding and polishing time can be greatly reduced or the grinding step can be directly omitted and polishing can be performed directly, thereby reducing the scattering of the laser and increasing the transmission. Prepare for the next splitting process.

[0080] Embodiment 2:

[0081] A "bow"-shaped scan is adopted, and a short pulse laser or a continuous laser is loaded after the ultrashort pulse laser, that is, the interval emission time is adjusted to be greater than 0s through the signal generator 1.

[0082] 1. The silicon carbide wafer (brittle material 10) purchased on the market is 4H-SiC or 6H-SiC. The size of the silicon carbide wafer is 6 inches or 8 inches, and the thickness is 500μm or 350μm;

[0083] 2. The wavelength of the ultrashort pulse laser 3 is 1064nm or 1050nm or 808nm or 532nm, the repetition frequency is 10MHz or 1MHz or 500kHz, the power is 100W or 10W or 5W or 2.5W or 1W, the pulse is selected to be a single pulse, a double pulse or a multi-pulse, etc., the pulse width is selected to be picosecond or sub-picosecond or femtosecond, and the diameter of the laser beam 7 passing through the beam expander 6 is limited by the beam focuser 9 to meet the aperture of the focusing system;

[0084] 3. After being reflected by the second dichroic mirror 8, the laser beam 7 enters the beam focuser 9 to focus the laser. After focusing, the laser is focused at a certain depth from the upper surface of the silicon carbide wafer. The thickness is determined according to the imaging system 18 and the Z-axis moving axis 14, and the depth is 250μm or 175μm;

[0085] 4. A short pulse laser beam or a continuous laser beam is emitted 1ns, 10ns, 100ns, 1ms, 10ms, 100ms, 1s, 10s, 100s after the ultrashort pulse laser beam is emitted, so that the ultrashort pulse laser beam and the short pulse or continuous laser beam are loaded inside the material with a difference of 1ns, 10ns, 100ns, 1ms, 10ms, 100ms, 1s, 10s, 100s, and the ultrashort pulse laser forms microcracks through nonlinear absorption, and the thermal characteristics of the short pulse laser or the continuous laser are used to make the microcracks diffuse evenly around the laser etching line, and the moving platform 12 is adjusted to etch the entire material in a "bow" shape, so that a surface with a lower surface roughness is finally obtained after the material is separated;

[0086] 6. After the material is separated, the rough part of the material surface needs to be ground and polished. Due to the low surface roughness of the material, the grinding and polishing time can be greatly reduced or the grinding step can be directly omitted and polishing can be performed directly, thereby reducing the scattering of the laser and increasing the transmission. Prepare for the next splitting process.

[0087] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0088] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0089] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0090] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0091] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0092] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.

Claims

1. A dual laser chipping method, characterized in that: A method for splitting a brittle material using a dual laser splitting device, wherein the dual laser splitting device comprises a short pulse or continuous laser, an ultrashort pulse laser, a beam expander and a beam focuser, and the splitting method comprises the following steps: Setting the emission interval time of the ultrashort pulse laser and the short pulse or continuous laser, wherein the interval time is greater than 0s; The ultrashort pulse laser emits an ultrashort pulse laser beam, and the ultrashort pulse laser beam passes through the beam expander and then is focused into the brittle material by the beam focuser; Adjusting the depth of the focus of the laser beam in the brittle material, so that the ultrashort pulse laser beam forms cracks inside the brittle material through nonlinear absorption; The short pulse or continuous laser emits a short pulse laser beam or a continuous laser beam after a preset interval time, and the short pulse laser beam or the continuous laser beam passes through the beam expander and is focused into the brittle material by the beam focuser; Under the thermal characteristics of a short-pulse laser beam or a continuous laser beam, the crack spreads uniformly to the surroundings; Adjusting the position of the focus of the laser beam in the brittle material in a certain path to etch the entire brittle material, so that the brittle material is split into a target wafer and remaining material; Wherein, the short pulse or continuous laser beam emitted by the short pulse or continuous laser is located above the ultrashort pulse laser beam emitted by the ultrashort pulse laser.

2. The dual laser cracking method according to claim 1, characterized in that: The dual laser splitting device includes an X-axis moving axis, a Y-axis moving axis and a Z-axis moving axis, wherein the X-axis moving axis is used to control the movement of the focus of the laser beam on the X-axis, the Y-axis moving axis is used to control the movement of the focus of the laser beam on the Y-axis, and the Z-axis moving axis is used to control the movement of the focus of the laser beam on the Z-axis, wherein the Z-axis is in a direction approaching or moving away from the brittle material, and the X-axis, the Y-axis and the Z-axis are perpendicular to each other; The step of adjusting the depth of the focus of the laser beam in the brittle material specifically includes adjusting the Z-axis moving axis so that the focus of the laser beam is located at a preset depth in the brittle material; The step of adjusting the position of the focus of the laser beam in the brittle material along a certain path specifically includes adjusting the X-axis moving axis and the Y-axis moving axis to allow the focus of the laser beam to scan and etch the brittle material along a certain path.

3. The dual laser cracking method according to claim 1, characterized in that: The brittle material is silicon carbide, gallium nitride, diamond, or a material composed of one or more elements of group IV, groups III and V, and groups II and VI.

4. The dual laser splitting method according to any one of claims 1 to 3, characterized in that: The pulse width of the short pulse or continuous laser is picosecond, sub-picosecond or femtosecond, and the pulse width of the ultrashort pulse laser is picosecond, sub-picosecond or femtosecond; And / or, the pulse form of the short pulse or continuous laser and the ultrashort pulse laser is single pulse, double pulse or multiple pulses.

Citation Information

Cited By

  • Method and device for laser peeling off wafer

    CN119794552B