Glass substrate, display device, and method for manufacturing glass substrate

By etching the glass of a specific composition, a glass substrate with specific surface characteristics and optical characteristics is prepared, which solves the problem of reduced flash and cleaning properties of the glass substrate, and achieves good visual effects and anti-glare performance in high-definition display devices.

CN115003639BActive Publication Date: 2024-11-05AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180011201.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-30
Filing Date
2021-01-22
Publication Date
2024-11-05
Estimated Expiration
2041-01-22

AI Technical Summary

Technical Problem

Existing glass substrates are prone to flash problems after anti-glare treatment, and their cleaning properties are reduced. Especially in high-definition display devices, the flash problems are more prominent, affecting visual recognition.

Method used

By etching the glass of a specific composition, a glass substrate with specific surface characteristics and optical properties is prepared, including the reference mole percentage of oxides of SiO2, Al2O3, B2O3, Y2O3, MgO, CaO, Li2O, Na2O, K2O, TiO2 and ZrO2, which is a glass substrate with specific surface characteristics and optical properties. In a glass substrate within a specific range, the number of etching surface protrusions is more than 400 and less than 2,000, the average interval of concave and convex is less than 30 μm, and the arithmetic average inclination angle RΔa is more than 1.50°. The etching is determined by analysis by laser microscope and image processing software. Face characteristics.

Benefits of technology

Effectively suppress flash, improve cleaning performance, enhance visual recognition, and maintain good anti-glare effect in the display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0003909847890000251
    Figure GDA0003909847890000251
  • Figure HDA0003765067820000011
    Figure HDA0003765067820000011
  • Figure HDA0003765067820000021
    Figure HDA0003765067820000021
Patent Text Reader

Abstract

An embodiment of the present invention relates to a glass substrate having a specific basic composition and at least one main surface comprising an etched surface having a number of protrusions of greater than 400 and less than 2000, wherein the number of protrusions is obtained by measuring an area of ​​285.12 μm×213.77 μm using a laser microscope to obtain XYZ data of the surface shape, and performing shape analysis on the XYZ data using image processing software SPIP manufactured by Image Metrolоgy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a glass substrate which suppresses flare and has excellent cleanability and is used for a display device or the like, a display device having the glass substrate, and a method for manufacturing the glass substrate. Background Art

[0002] In recent years, a cover plate made of glass is disposed on the display surface side of a display device such as an LCD (liquid crystal display) device in order to protect the display device.

[0003] However, when such a glass plate is provided on a display device, when visually recognizing the display screen of the display device through the glass plate, objects placed around the display screen may be reflected on the glass plate. When such reflection occurs on the glass plate, it is difficult for the viewer of the display screen to visually recognize the display screen, and an unpleasant impression is left.

[0004] In order to suppress such reflection, for example, an attempt has been made to perform an anti-glare treatment on the surface of the glass plate to form a concave-convex shape. In the anti-glare treatment, for example, methods such as etching the surface of the glass plate (for example, refer to Patent Document 1)) and forming a film having a concave-convex shape on the surface of the glass plate (for example, refer to Patent Document 2)) can be cited.

[0005] On the other hand, in such a display device, there are many opportunities for a human finger or the like to touch the surface of the glass substrate constituting the cover plate, and when a human finger or the like touches the surface of the glass substrate, grease or the like is easily attached to the surface of the glass substrate. Furthermore, when grease or the like is attached, visual recognition is affected, and therefore, a glass substrate having an anti-fouling treatment applied to the surface of the glass substrate having been subjected to an anti-glare treatment has been used in the past.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: International Publication No. 2014 / 119453

[0009] Patent Document 2: U.S. Patent No. 8003194 Summary of the invention

[0010] Problems to be solved by the invention

[0011] Anti-glare treatment can suppress the above-mentioned reflection, reduce reflection, and obtain anti-fouling effect, but on the other hand, it may cause the disadvantages of flashing or reduced washing resistance. When flashing occurs on the glass substrate, it is difficult for the viewer of the display to visually recognize the display, and it will leave an unpleasant impression.

[0012] When the roughness of the surface of the glass substrate treated with anti-glare is larger than the pitch between pixels of the display device, or when the size and depth of the surface concave-convex of the glass substrate are uneven, the flash becomes significant. As the display device becomes higher definition, the pixel size and the pixel pitch become smaller. Therefore, it can be predicted that the flash problem of the glass substrate will become more and more significant in the future. In addition, as mentioned above, grease and the like are easily attached to the surface of the glass substrate in the display device, but due to the anti-glare treatment, there is a problem that the cleanability of grease and the like is easily reduced.

[0013] Therefore, an object of the present invention is to provide a glass substrate including an etched surface which suppresses flare and has excellent cleaning properties.

[0014] Means used to solve problems

[0015] In view of the above problems, the present inventors have found that by etching glass having a specific composition, a glass substrate including an etched surface with suppressed flare and excellent cleanability can be obtained, thereby completing the present invention.

[0016] That is, the gist of the present invention is as follows.

[0017] 1. A glass substrate, wherein the glass substrate contains, in terms of molar percentage based on oxides:

[0018] SiO2: 50%~75%,

[0019] Al2O3: 0.1%~25%,

[0020] B2O3: 0~10%,

[0021] Y2O3: 0~5%,

[0022] MgO: 0-20%,

[0023] CaO: 0-15%,

[0024] Li2O: 0~15%

[0025] Na2O: 1% to 25%,

[0026] K2O: 0.1%~20%,

[0027] TiO2: 0-1%, and

[0028] ZrO2: 0~2%,

[0029] As a basic component, and

[0030] At least one main surface of the glass substrate includes an etched surface having a number of protrusions of 400 or more and 2000 or less as determined by the following method,

[0031] Method: A laser microscope was used to measure an area of ​​285.12 μm × 213.77 μm to obtain XYZ data of the surface shape. In the shape analysis of the XYZ data using the image processing software SPIP manufactured by Image Metrology, after the entire surface was smoothed, the number of protrusions was determined when the particle detection was set to a threshold level of 50.0000 nm.

[0032] 2. The glass substrate according to item 1 above, wherein the value of the average interval RSm between the concavities and convexities of the etched surface is 30 μm or less.

[0033] 3. The glass substrate according to 1 or 2 above, wherein, under a condition where there is no cutoff value, the arithmetic mean inclination angle RΔa of the etched surface is 1.50° or more.

[0034] 4. The glass substrate according to any one of 1 to 3 above, wherein a haze ratio of transmitted light of the etched surface measured by a method in accordance with JIS K7136 (2000) is 0.2% to 75%.

[0035] 5. The glass substrate according to any one of 1 to 4 above, wherein the flash value S of the etched surface is quantified by the following method: a Below 8,

[0036] Method: A glass plate is arranged on the display surface side of a display device having a resolution of 264 ppi so that the etched surface is in contact with the display surface side of the display device. When a single green image composed of RGB (0, 255, 0) is displayed on the display device, an image analysis is performed using SMS-1000 manufactured by DM&S Co., Ltd., which is arranged above the glass plate, to obtain a sparkle value, and the sparkle value is set as the sparkle value S. a The distance d between the solid-state imaging element and the glass plate was set to 568 mm, and a 23FM50SP lens with a focal length of 50 mm was used under the condition of an aperture of 16 for the camera lens. The measurement was performed by the Difference Image Method (DIM), and 0 was entered in the Pixel Ratio value to obtain the flash value S a .

[0037] 6. The glass substrate according to any one of 1 to 5 above, wherein the total content of Na2O, K2O and Li2O in the basic composition is less than 30% in terms of molar percentage based on oxides.

[0038] 7. A display device comprising the glass substrate according to any one of 1 to 6 above.

[0039] 8. A method for manufacturing a glass substrate, comprising: a method for manufacturing a glass substrate having an etched surface on at least one main surface, the number of protrusions of which is 400 or more and 2000 or less as determined by the following method; wherein the method for manufacturing a glass substrate comprises a step of frosting the glass substrate;

[0040] The glass substrate contains, in terms of molar percentage based on oxides:

[0041] SiO2: 50%~75%,

[0042] Al2O3: 0.1%~25%,

[0043] B2O3: 0~10%,

[0044] Y2O3: 0~5%,

[0045] MgO: 0-20%,

[0046] CaO: 0-15%,

[0047] Li2O: 0~15%

[0048] Na2O: 1% to 25%,

[0049] K2O: 0.1%~20%,

[0050] TiO2: 0-1%, and

[0051] ZrO2: 0~2%,

[0052] Method: A laser microscope was used to measure an area of ​​285.12 μm × 213.77 μm to obtain XYZ data of the surface shape. In the shape analysis of the XYZ data using the image processing software SPIP manufactured by Image Metrology, after the entire surface was smoothed, the number of protrusions was determined when the particle detection was set to a threshold level of 50.0000 nm.

[0053] Effects of the Invention

[0054] The glass substrate according to the embodiment of the present invention can effectively suppress flare and exhibit excellent cleaning properties because the basic composition of glass is within a specific range and has surface properties within a specific range. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 To schematically represent the determination of the flash value Sa A diagram showing an example of a measuring device used when performing an experiment.

[0056] Figure 2 It is a diagram schematically showing an example of a measuring device used when measuring the reflection image diffusivity index value R. DETAILED DESCRIPTION

[0057] Hereinafter, a mode for carrying out the present invention will be described, but the present invention is not limited to the following embodiment, and various modifications and substitutions can be made to the following embodiment without departing from the scope of the present invention.

[0058] <Basic composition of glass>

[0059] The composition of the glass can also be simply determined by semi-quantitative analysis using fluorescent X-ray method, but more precisely, it can be measured by wet analysis such as ICP emission analysis. It should be noted that, unless otherwise specified, the content of each component is expressed as a molar percentage based on oxide.

[0060] The glass substrate according to the embodiment of the present invention is characterized in that the glass substrate contains, in terms of molar percentage based on oxides:

[0061] SiO2: 50%~75%,

[0062] Al2O3: 0.1%~25%,

[0063] B2O3: 0~10%,

[0064] Y2O3: 0~5%,

[0065] MgO: 0-20%,

[0066] CaO: 0-15%,

[0067] Li2O: 0~15%

[0068] Na2O: 1% to 25%,

[0069] K2O: 0.1%~20%,

[0070] TiO2: 0-1%, and

[0071] ZrO2: 0~2%

[0072] As the basic composition.

[0073] SiO2 is a component constituting the glass skeleton. In addition, SiO2 is a component that improves chemical durability and is a component that reduces the generation of cracks when damage (indentation) occurs on the glass surface.

[0074] The content of SiO2 in the glass substrate of the present embodiment is 50% or more, and preferably 54% or more, 58% or more, 60% or more, 63% or more, 66% or more, or 68% or more.

[0075] On the other hand, when the content of SiO2 is greater than 75%, the melting property is significantly reduced. Therefore, the content of SiO2 in the glass substrate of the present embodiment is 75% or less, preferably 74% or less, more preferably 73% or less, further preferably 72% or less, particularly preferably 71% or less, and most preferably 70% or less.

[0076] The glass substrate of this embodiment can increase the number of protrusions on the etched surface by containing Al2O3, thereby suppressing flash and improving cleaning properties. From the perspective of improving the characteristics of the etched surface such as the increase in the number of protrusions, the content of Al2O3 is 0.1% or more, preferably 0.3% or more, 0.5% or more, 0.7% or more, 0.8% or more, 0.9% or more, 1% or more, and 5% or more.

[0077] On the other hand, when the content of Al2O3 is greater than 25%, the acid resistance of the glass decreases or the devitrification temperature increases. In addition, the viscosity of the glass increases and the melting property decreases. Therefore, the content of Al2O3 in the glass substrate of the present embodiment is 25% or less, preferably 20% or less, more preferably 18% or less, further preferably 16% or less, and particularly preferably 14% or less.

[0078] Y2O3 is a component that improves the crushability of chemically strengthened glass, and may be contained. When Y2O3 is contained in the glass substrate of the present embodiment, the content of Y2O3 is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, particularly preferably 2% or more, and most preferably 2.5% or more.

[0079] When the content of Y2O3 exceeds 5%, the glass is easily devitrified during melting, and the quality may be reduced. Therefore, the content of Y2O3 in the glass substrate of this embodiment is 5% or less, preferably 4% or less, and more preferably 3% or less.

[0080] MgO is a component that increases the surface compressive stress of chemically strengthened glass during chemical strengthening, and is a component that improves crushability, and MgO may be contained. When MgO is contained in the glass substrate of this embodiment, the content of MgO is preferably 3% or more, and more preferably 4% or more, 5% or more, 6% or more, 7% or more, and 8% or more.

[0081] On the other hand, when the content of MgO is greater than 20%, the glass is easily devitrified during melting. Therefore, the content of MgO in the glass substrate of this embodiment is 20% or less, preferably 15% or less, and more preferably 14% or less, 13% or less, 12% or less, 11% or less, and 10% or less.

[0082] CaO is a component that improves the meltability of glass and improves the crushability of chemically strengthened glass during chemical strengthening, and CaO may be contained. When CaO is contained in the glass substrate of this embodiment, the content of CaO is preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, particularly preferably 3% or more, and most preferably 5% or more.

[0083] On the other hand, when the CaO content exceeds 15%, the ion exchange performance decreases, so the CaO content in the glass substrate of this embodiment is set to 15% or less. The CaO content is preferably 10% or less, more preferably 9% or less, and further preferably 8% or less.

[0084] Li2O is a component that forms surface compressive stress by ion exchange and is a component that improves the crushability of chemically strengthened glass. When a chemical strengthening treatment is performed to exchange Li ions on the glass surface with Na ions, the content of Li2O in the glass substrate of the present embodiment is preferably 3% or more, more preferably 4% or more, further preferably 5% or more, particularly preferably 6% or more, and typically 7% or more.

[0085] On the other hand, when the content of Li2O in the glass substrate of the present embodiment is greater than 15%, the acid resistance of the glass is significantly reduced. The content of Li2O is 15% or less, preferably 14% or less, more preferably 13% or less, further preferably 12% or less, and particularly preferably 11% or less.

[0086] On the other hand, when a chemical strengthening treatment is performed to exchange Na ions on the glass surface for K ions, when the content of Li2O in the glass substrate of the present embodiment is greater than 3%, the magnitude of the compressive stress is sometimes reduced. In this case, the content of Li2O is preferably 3% or less, more preferably 2% or less, further preferably 1% or less, particularly preferably 0.5% or less, and most preferably substantially free of Li2O.

[0087] In this specification, “substantially free of” means that it does not contain, or is not intentionally contained, other than inevitable impurities contained in raw materials, etc. Specifically, it means that the content in the glass composition is less than 0.1 mol%.

[0088] By including Na2O, the number of protrusions on the etched surface can be increased, thereby suppressing flash and improving cleaning properties. In addition, Na2O is a component that improves the solubility of glass and forms a surface compressive stress layer when ion exchange is performed.

[0089] From the viewpoint of improving the characteristics of the etched surface such as an increase in the number of protrusions, the content of Na2O in the glass substrate of the present embodiment is 1% or more, preferably 2% or more, and more preferably 3% or more.

[0090] On the other hand, when the content of Na2O in the glass substrate of the present embodiment is greater than 25%, the acid resistance of the glass is significantly reduced. From the viewpoint of acid resistance, the content of Na2O is 25% or less, preferably 20% or less, more preferably 18% or less, further preferably 16% or less, and particularly preferably 14% or less.

[0091] By including K2O, the number of protrusions on the etched surface can be increased, thereby suppressing flash and improving cleaning properties. In addition, by including K2O, the ion exchange performance can be improved.

[0092] From the viewpoint of improving the characteristics of the etched surface such as increasing the number of protrusions, the content of K2O in the glass substrate of this embodiment is 0.1% or more, preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, and particularly preferably 3% or more.

[0093] On the other hand, when the content of K2O is greater than 20%, the characteristics of the etched surface such as the reduction in the number of protrusions are reduced, so the content of K2O in the glass substrate of this embodiment is 20% or less. The content of K2O is preferably 15% or less, more preferably 12% or less, further preferably 10% or less, particularly preferably 8% or less, and most preferably 6% or less.

[0094] When the content of K2O is greater than the content of Na2O, the number of protrusions on the etched surface is insufficient, so the content of K2O in the glass substrate of this embodiment is preferably less than the content of Na2O. For example, the content of Na2O / the content of K2O is preferably 1.1 or more, more preferably 1.5 or more, further preferably 2 or more, particularly preferably 2.5 or more, and most preferably 3 or more.

[0095] The total content of Na2O, K2O and Li2O in the glass substrate of the present embodiment (Na2O+K2O+Li2O) is preferably 30% or less, more preferably 28% or less, further preferably 26% or less, and particularly preferably 25% or less. By making Na2O+K2O+Li2O 30% or less, the reduction of RSm can be suppressed and the cleaning property can be improved.

[0096] TiO 2 is a component that improves the crushability of chemically strengthened glass during chemical strengthening, and may be contained. When TiO 2 is contained in the glass substrate of this embodiment, the content of TiO 2 is preferably 0.1% or more, more preferably 0.15% or more, and further preferably 0.2% or more.

[0097] On the other hand, when the content of TiO2 is greater than 1%, devitrification is likely to occur during melting, and the quality of chemically strengthened glass may be reduced. The content of TiO2 in the glass substrate of this embodiment is 1% or less, preferably 0.8% or less, more preferably 0.5% or less, and further preferably 0.25% or less.

[0098] ZrO2 is a component that increases the surface compressive stress caused by ion exchange and has the effect of improving glass breakability, and ZrO2 may be contained. When ZrO2 is contained in the glass substrate of this embodiment, the content of ZrO2 is preferably 0.5% or more, and more preferably 1% or more.

[0099] On the other hand, when the content of ZrO2 is greater than 2%, devitrification is likely to occur during melting, and the quality may be reduced. The content of ZrO2 in the glass substrate of this embodiment is 2% or less, preferably 1.8% or less, more preferably 1.6% or less, further preferably 1.4% or less, and particularly preferably 1.2% or less.

[0100] B2O3 is a component that improves the chipping resistance of glass and improves its solubility. B2O3 is not essential. When B2O3 is contained in the glass substrate of the present embodiment, in order to improve the solubility, the content of B2O3 is preferably 0.5% or more, more preferably 1% or more, and further preferably 2% or more.

[0101] On the other hand, the content of B2O3 in the glass substrate of the present embodiment is 10% or less. By setting the content of B2O3 to 10% or less, it is possible to suppress the generation of ribs during melting, and the quality of the glass is not easily reduced. The content of B2O3 is preferably 5% or less, more preferably 4% or less, further preferably 3% or less, and particularly preferably 1% or less. In order to improve acid resistance, it is preferred not to contain B2O3.

[0102] P2O5 is a component that improves ion exchange performance and chipping resistance. The glass substrate of this embodiment may not contain P2O5. If P2O5 is contained, the content of P2O5 is preferably 0.5% or more, more preferably 1% or more, and further preferably 2% or more.

[0103] On the other hand, by making the content of P2O5 in the glass substrate of this embodiment 4% or less, the breakability and acid resistance of the chemically strengthened glass can be improved. Therefore, the content of P2O5 is preferably 4% or less, more preferably 3% or less, further preferably 2% or less, and particularly preferably 1% or less. In order to improve the acid resistance, it is preferred not to contain P2O5.

[0104] SrO is a component that improves the meltability of chemically strengthened glass and improves the crushability of chemically strengthened glass, and SrO may be contained. When SrO is contained in the glass substrate of the present embodiment, the content of SrO is preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, particularly preferably 3% or more, and most preferably 5% or more.

[0105] On the other hand, when the content of SrO in the glass substrate of the present embodiment is greater than 20%, the ion exchange performance is significantly reduced, so the content of SrO is preferably 20% or less. The content of SrO is more preferably 14% or less, and further preferably 10% or less, 8% or less, 6% or less, 3% or less, and 1% or less.

[0106] BaO is a component that improves the meltability of chemically strengthened glass and improves the crushability of chemically strengthened glass, and BaO may be contained. When BaO is contained in the glass substrate of the present embodiment, the content of BaO is preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, particularly preferably 3% or more, and most preferably 5% or more.

[0107] On the other hand, when the content of BaO is greater than 15%, the ion exchange performance is significantly reduced. The content of BaO in the glass substrate of this embodiment is preferably 15% or less, more preferably 10% or less, 8% or less, 6% or less, 3% or less, and 1% or less.

[0108] ZnO is a component that improves the solubility of glass, and ZnO may be contained. When ZnO is contained in the glass substrate of the present embodiment, the content of ZnO is preferably 0.25% or more, and more preferably 0.5% or more.

[0109] On the other hand, when the content of ZnO exceeds 10%, the weather resistance of the glass is significantly reduced. The content of ZnO in the glass substrate of this embodiment is preferably 10% or less, more preferably 7% or less, further preferably 5% or less, particularly preferably 2% or less, and most preferably 1% or less.

[0110] La2O3 and Nb2O5 are components for improving the breakability of glass, and La2O3 and Nb2O5 may be contained. In the glass substrate of this embodiment, when these components are contained, the content of each is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, particularly preferably 2% or more, and most preferably 2.5% or more.

[0111] On the other hand, when the contents of La2O3 and Nb2O5 are each greater than 8%, the glass is easily devitrified during melting, and the quality of the glass may be reduced. The contents of La2O3 and Nb2O5 in the glass substrate of the present embodiment are each preferably 8% or less, more preferably 6% or less, further preferably 5% or less, particularly preferably 4% or less, and most preferably 3% or less.

[0112] In the glass substrate of this embodiment, in order to improve the breakability of the glass, a small amount of Ta2O5 and Gd2O3 may be contained, but since the refractive index and reflectivity become higher, the content of Ta2O5 and Gd2O3 is preferably less than 1%, more preferably less than 0.5%, and further preferably does not contain Ta2O5 and Gd2O3.

[0113] In addition, when the glass is colored for use, a coloring component may be added within a range that does not hinder the realization of the desired chemical strengthening characteristics. As the coloring component, for example, Co3O4, MnO2, Fe2O3, NiO, CuO, Cr2O3, V2O5, Bi2O3, SeO2, TiO2, CeO2, Er2O3, and Nd2O3 can be listed as appropriate coloring components.

[0114] In the glass substrate of the present embodiment, the content of the coloring components is preferably within a range of 7% or less in total, based on the molar percentage of the oxide. When the total content is greater than 7%, the glass is prone to devitrification, which is not preferred. The content is preferably 5% or less, more preferably 3% or less, and further preferably 1% or less. In the case where the visible light transmittance of the glass is given priority, it is preferred that these components are substantially not contained.

[0115] The glass substrate of this embodiment may contain SO3, chloride, fluoride, etc. as a clarifier when the glass is melted. Preferably, As2O3 is not contained. When Sb2O3 is contained, the content of Sb2O3 is preferably 0.3% or less, more preferably 0.1% or less, and most preferably, no Sb2O3 is contained.

[0116] Furthermore, the glass substrate of the present embodiment can be provided with antibacterial properties by having silver ions on the surface.

[0117] As a basic composition of the glass substrate of this embodiment, the following glass composition can be mentioned, for example.

[0118] The glass composition contains 55% to 72% SiO2, 0.1% to 18% Al2O3, 0 to 4% B2O3, 0 to 1% Y2O3, 2% to 12% MgO, 0 to 10% CaO, 0 to 11% Li2O, 3% to 20% Na2O, 0.1% to 10% K2O, 0 to 0.2% TiO2 and 0 to 1.5% ZrO2.

[0119] At least one major surface of the glass substrate of this embodiment includes an etched surface. In the present invention, "etched surface" refers to a surface having a specific surface texture / roughness obtained by removing a certain amount of glass material by chemical means (i.e., acid etching). The etched surface of the glass substrate is characterized by its surface properties and optical properties.

[0120] <Surface characteristics>

[0121] Hereinafter, the surface characteristics of the etched surface in the glass substrate of this embodiment will be described.

[0122] (Shape Count)

[0123] The number of protrusions on the etched surface of the glass substrate of this embodiment is 400 or more as determined by the following method. Method: XYZ data of the surface shape is obtained by measuring an area of ​​285.12 μm×213.77 μm using a laser microscope. In the shape analysis of the above XYZ data using the image processing software SPIP manufactured by Image Metrology, after the entire surface is leveled, the number of protrusions is determined when the particle detection is set to a threshold level of 50.0000 nm.

[0124] The number of the protrusions is preferably 500 or more, more preferably 600 or more, further preferably 700 or more, and particularly preferably 800 or more. In addition, the number of the protrusions is 2000 or less, preferably 1600 or less, more preferably 1400 or less, and further preferably 1200 or less.

[0125] When the number of protrusions is 400 or more, glare can be suppressed and visibility can be improved. When the number of protrusions is 2000 or less, a decrease in RSm described below can be suppressed and cleaning properties can be improved.

[0126] (RSm)

[0127] The average interval (RSm) of the concavoconvexities on the etched surface of the glass substrate of this embodiment is preferably 30 μm or less, more preferably 28 μm or less, further preferably 26 μm or less, and particularly preferably 25 μm or less. When RSm is 30 μm or less, the sparkle value S described later can be reduced. a This suppresses flash.

[0128] The lower limit of RSm is preferably 5 μm or more, more preferably 8 μm or more, further preferably 12 μm or more, and particularly preferably 15 μm or more. When RSm is 5 μm or more, the cleaning property can be improved.

[0129] The mean concave-convex spacing (RSm) generally refers to the average value of the concave-convex period in the roughness curve formed on the cross section of the object to be measured. It should be noted that the mean concave-convex spacing (RSm) can be calculated according to the calculation formula of JIS-B0601 (2013).

[0130] (RΔa)

[0131] Under the condition of no cutoff value, the arithmetic mean inclination angle (RΔa) of the etched surface of the glass substrate of the present embodiment is preferably 1.50° or more, more preferably 1.60° or more, further preferably 1.70° or more, and particularly preferably 1.80° or more. When RΔa is 1.50° or more, glare can be suppressed and visual recognition can be improved.

[0132] In the glass substrate of the present embodiment, RΔa is preferably 15° or less, more preferably 12° or less, and further preferably 10° or less. When RΔa is 15° or less, the cleaning property can be improved.

[0133] The arithmetic mean inclination angle (RΔa) refers to the value obtained by dividing the profile curve horizontally at a certain interval ΔX, finding the absolute value of the slope (angle) of the line segment connecting the start and end points of the profile curve in each interval, and averaging the value. RΔa is measured and calculated using a laser microscope. The measurement position is set to a plurality of positions, at least 10 positions, preferably 12 positions or more.

[0134] As the measurement operation procedure, select line roughness analysis and analyze at any position. Data analysis can be performed on the measured data in the horizontal or vertical direction. In the data analysis, set the cutoff value λs, the phase compensation type high pass filter λc, and the phase compensation type low pass filter λf to none.

[0135] (Ra)

[0136] The arithmetic mean roughness (Ra) of the etched surface of the glass substrate of the present embodiment is preferably 0.02 μm or more, more preferably 0.04 μm or more, and further preferably 0.06 μm or more.

[0137] Moreover, in the glass substrate of this embodiment, Ra is preferably 0.50 μm or less, more preferably 0.40 μm or less, and further preferably 0.30 μm or less.

[0138] In the glass substrate of the present embodiment, when Ra is 0.02 μm or more, the sparkle value can be reduced, and when Ra is 0.50 μm or less, the cleaning property can be improved.

[0139] Ra can be calculated using a calculation formula based on JIS-B0601 (2013).

[0140] (Rz)

[0141] The maximum height (Rz) of the surface roughness of the etched surface of the glass substrate of the present embodiment is preferably 0.10 μm or more, more preferably 0.20 μm or more, and further preferably 0.30 μm or more.

[0142] Moreover, in the glass substrate of this embodiment, Rz is preferably 2.50 μm or less, more preferably 2.40 μm or less, and further preferably 2.30 μm or less.

[0143] When Rz is 0.10 μm or more, the sparkle value can be reduced. When Rz is 2.50 μm or less, the cleaning property can be improved. Rz can be calculated using a calculation formula based on JIS-B0601 (2013).

[0144] <Optical properties>

[0145] (Haze rate)

[0146] The haze ratio of the transmitted light in the visible light region of the etched surface of the glass substrate of the present embodiment measured according to JIS K 7136 (2000) is preferably 0.2% or more, more preferably 0.5% or more, and further preferably 1% or more. In addition, the haze ratio is preferably 75% or less, more preferably 70% or less, and further preferably 65% ​​or less. When the haze ratio is within the above range, the reflection of light can be effectively suppressed.

[0147] (Flash value S a )

[0148] In this application specification, the flash value S measured according to the following operation steps is used as a flash index. a . Flash value S a It refers to the degree to which the unevenness of bright spots generated by the interference of scattered light when the light (image) from the display screen passes through the glass plate is detected, and the flash value S is confirmed. a It shows a good correlation with the judgment result of the flicker obtained by the viewer's visual observation. a The flash of the large glass plate is obvious. On the contrary, the flash value S a Small glass sheets have a tendency for the flash to be suppressed.

[0149] The sparkle value S of the etched surface of the glass substrate of the present embodiment measured by the following method is a It is preferably 8 or less, more preferably 7 or less, further preferably 6 or less, and particularly preferably 5 or less.

[0150] Reference Figure 1 , for the flash value S a The determination method of the flash value S is described below. a When first, a display device 54 [iPad (registered trademark)-Air2; resolution 264ppi] is prepared. The display device may have a cover plate provided on the display surface side for the purpose of preventing damage, etc.

[0151] Next, the sample to be measured, that is, the glass substrate 50, is arranged on the display surface side of the display device. It should be noted that, when the first principal surface 52, which is one principal surface of the glass substrate 50, includes an etched surface, the glass substrate 50 is arranged on the display surface side of the display device in such a manner that the first principal surface 52 becomes the opposite side (surface brightness measuring instrument 75 side) of the display device 54. That is, the second principal surface 53, which is the other principal surface, is arranged on the display device 54.

[0152] Next, while the display device is turned on and an image is displayed, an analysis device (SMS-1000; manufactured by Display-Messtechnik & Systeme [DM&S]) is used to analyze the degree of sparkle on the glass substrate 50. Thus, the sparkle value S expressed in the form of a sparkle value is obtained. a .

[0153] It should be noted that, during the measurement, it is preferred to display a single green image composed of RGB (0, 255, 0) on the entire display screen of the display device 54. This is to minimize the influence of differences in observation methods caused by differences in display colors. The distance d between the front end of the device's camera lens and the transparent substrate with an anti-glare function is set to 568 mm. The Pixel Ratio value (a value indicating how many times the pitch of one pixel of the display device is equivalent to the pitch of the pixels of the camera) measured at this time is 2.45. As the camera lens, a 23FM50SP lens with a focal length of 50 mm is used under the condition of an aperture of 16. The evaluation area ROI is set to 200×200. The measurement is performed by the difference method (DIM), and 0 is entered in the PixelRatio value to obtain the flash value S a It should be noted that the same measurement can be performed in the single image method (SIM), but the flash value S obtained in this case is a The absolute values ​​of are different, so they need to be distinguished.

[0154] The flash value Sa It shows a good correlation with the judgment result of the flicker obtained by the viewer. a The flash of the large transparent substrate is significant, on the contrary, the flash S a Small transparent substrates have a tendency for the flash to be suppressed.

[0155] (G60)

[0156] The etched surface of the glass substrate of the present embodiment preferably has a specular gloss GS (60°) (hereinafter referred to as G60) of 60 degrees specular gloss specified in JIS Z 8741 (1997) of 10 or more, more preferably 15 or more, and further preferably 20 or more. In addition, G60 is preferably 140 or less, more preferably 135 or less, and further preferably 130 or less. In addition, G60 is preferably 10 or more and 140 or less, more preferably 15 or more and 135 or less, and further preferably 20 or more and 130 or less. When G60 is within the above range, the reflection of light is suppressed.

[0157] (Reflection image diffusion index value R)

[0158] In this application specification, as an index of anti-glare performance, a reflection image diffusiveness index value R measured according to the following operating steps is used. Reflection image diffusivity refers to the extent to which the reflected image of an object (such as lighting) placed around the glass plate is consistent with the original object, and it is confirmed that the reflection image diffusivity shows a good correlation with the anti-glare judgment result obtained by the viewer's visual observation. For example, a glass plate showing a small reflection image diffusiveness index value R (close to 0) has poor anti-glare performance, while a glass plate showing a large reflection image diffusiveness index value R (the closer to 1, the larger) has good anti-glare performance.

[0159] The reflected image diffusion index value R of the etched surface of the glass substrate of the present embodiment is preferably 0.01 or more, more preferably 0.05 or more, and further preferably 0.1 or more. When the reflected image diffusion index value R is within the above range, sufficient anti-glare properties can be obtained.

[0160] Reference Figure 2 , a method for measuring the reflected image diffusion index value R of the glass substrate 50 is described. Figure 2 Schematically shows an example of a measuring device used when measuring the reflected image diffusivity index value R.

[0161] like Figure 2As shown, the measuring device 70 has a linear light source device 71 and a surface brightness measuring instrument 75. The measuring device 70 is provided with a sample to be measured, that is, a glass substrate 50 with an anti-glare function (a transparent substrate (or a transparent substrate with an anti-glare function that has been subjected to an anti-glare treatment) 50). The linear light source device 71 includes a light source 711 and a black plate 712. The light source 711 is provided in a slit-shaped opening of the black plate 712. The glass substrate 50 has a first main surface 52 and a second main surface 53 including an etched surface. The linear light source device 71 is directed toward the glass substrate 50, and Figure 2 The surface brightness measuring instrument 75 is arranged in a direction perpendicular to the paper surface. The surface brightness measuring instrument 75 is arranged in a vertical plane passing through the center of the width direction of the linear light source device 71. The focus of the surface brightness measuring instrument 75 is consistent with the image of the linear light source device 71 reflected by the glass substrate 50. That is, the surface on which the image is focused is aligned with the black plate 712. Here, when focusing on the light rays with equal incident angle θi and reflection angle θr (hereinafter referred to as the first incident light 731 and the first reflected light 732) among the light rays incident from the linear light source device 71 and reflected by the glass substrate 50 and incident on the surface brightness measuring instrument 75, θi=θr=5.7°.

[0162] It should be noted that the glass substrate 50 is arranged so that the first principal surface 52 is located on the side of the linear light source device 71 and the surface brightness meter 75. A black plate is arranged on the second principal surface 53 side of the glass substrate 50. Therefore, the light detected by the surface brightness meter 75 is reflected light reflected by the glass substrate 50.

[0163] Next, the measurement method is described. For example, when focusing on the light rays 733 and 734 whose difference between the incident angle θi and the reflection angle θr is θr-θi=0.5°, the light ray 734 represents the component scattered on the glass substrate 50 in the direction deviating from the regular reflection by 0.5°. The light from this direction is observed in the surface brightness measuring instrument 75 as an image of the part where the black plate 712 and the imaginary incident light 733-2 (the light incident at an angle equal to the angle of reflection of the light ray 734) intersect. That is, when the surface brightness is obtained using the surface brightness measuring instrument 75, an image is obtained in which the light scattered on the first main surface 52 of the glass substrate 50 extends to the left and right of the bright line corresponding to the regular reflection of the linear light source device 71 as the center. The brightness cross-sectional profile in the direction perpendicular to the bright line is extracted. It should be noted that in order to improve the measurement accuracy, data can also be accumulated in the direction parallel to the bright line.

[0164] First, the brightness of the first reflected light 732 that is regularly reflected among the light incident on the first main surface 52 of the glass substrate 50 is set to R1. The incident angle θi of the first incident light 731 is 5.7°, and the reflection angle θr of the first reflected light 732 is 5.7°. The angle changed by the reflection of the light by the glass substrate 50 (transparent base 50) is recorded as θr-θi, and θr-θi is 0°. Since there is an error in the implementation, θr-θi is within the range of 0°±0.1°.

[0165] Next, the brightness of light 733 and 734 with a difference of θr-θi=0.5° between the incident angle θi and the reflection angle θr is set to R2. This light represents a component scattered in a direction deviating 0.5° from the regular reflection on the glass substrate 50 (transparent base 50). Since it actually includes an error, θr-θi=0.5°±0.1°.

[0166] Similarly, the brightness of light 735 and 736 at θr-θi=-0.5° is defined as R3. This light represents a component scattered in a direction deviating from regular reflection by -0.5° on the glass substrate 50 (transparent base 50). Since it actually includes an error, θr-θi=-0.5°±0.1°.

[0167] The reflected image diffusion index value R of the glass substrate 50 is calculated by the following formula (I) using the obtained brightness R1, R2, and R3.

[0168] Reflection image diffusion index value R = (R2 + R3) / (2 × R1) Formula (I)

[0169] It is confirmed that the reflected image diffusion index value R shows a good correlation with the anti-glare judgment result obtained by the viewer's visual observation. For example, the glass substrate 50 showing a small reflected image diffusion index value R (close to 0) has poor anti-glare properties, and conversely, the glass substrate 50 showing a large reflected image diffusion index value R (the closer to 1, the larger) has good anti-glare properties.

[0170] It should be noted that such measurement can be implemented, for example, by using the device SMS-1000 manufactured by DM&S. When using this device, a C1614A lens with a focal length of 16 mm is used under the condition of an aperture of 5.6. In addition, the distance from the first main surface 52 of the transparent base 50 constituting the glass substrate 50 to the camera lens is about 300 mm, and the imaging scale is set within the range of 0.0276 to 0.0278. The slit-shaped opening formed by the black plate 712 of the linear light source device 71 is 101 mm×1 mm.

[0171] <Manufacturing method>

[0172] The manufacturing method of the glass substrate of this embodiment includes a step of frosting the glass substrate of the basic composition to form an etched surface. The frosting can be performed by, for example, immersing the glass substrate as the object to be processed in a mixed solution of hydrofluoric acid and ammonium fluoride and performing a chemical surface treatment on the immersed surface.

[0173] As a surface treatment for the above purpose, for example, a method of frosting the first main surface of the glass substrate can be cited. The frosting treatment can be performed, for example, by immersing the first main surface of the glass substrate as the object to be treated in a mixed solution of hydrofluoric acid and ammonium fluoride, or a mixed solution of hydrofluoric acid and potassium fluoride, and performing a chemical surface treatment on the immersed surface. In particular, in the frosting treatment method using chemicals such as hydrofluoric acid to perform chemical surface treatment, microcracks are not easily generated in the treated surface, and the mechanical strength is not easily reduced, so it is preferred.

[0174] After the projections and depressions are made in this way, the glass surface is preferably chemically etched to adjust the surface shape. This can remove cracks caused by sandblasting or the like, and effectively suppress flashes.

[0175] As an etching method, for example, a method of immersing a glass plate as a treated object in a treatment solution containing hydrogen fluoride as a main component can be cited. As components other than hydrogen fluoride, for example, hydrochloric acid, nitric acid, citric acid and sulfuric acid can be cited, among which hydrochloric acid and sulfuric acid are particularly preferred. By containing these components, it is possible to suppress the alkali components contained in the glass from reacting with hydrogen fluoride to locally produce a precipitation reaction, and etching can be performed uniformly within the surface.

[0176] The glass plate is a glass plate formed by a float process, a down-draw process, or the like. In addition, the glass plate may be not only a flat glass plate but also a curved glass plate. There is no particular limitation on the thickness of the glass plate, and for example, a glass plate with a thickness of 10 mm or less may be used. Since the thinner the thickness, the lower the light absorption is suppressed, it is preferred for applications for the purpose of increasing the transmittance.

[0177] The glass substrate may be a strengthened glass plate. A strengthened glass plate is a glass plate that has been subjected to a strengthening treatment. The strength of the glass is improved by the strengthening treatment, for example, the thickness of the glass plate can be reduced while maintaining the strength. As a strengthening treatment, a treatment for forming a compressive stress layer on the surface of the glass plate is generally known. As a method for forming a compressive stress layer on the surface of the glass plate, for example, an air cooling strengthening method (physical strengthening method) and a chemical strengthening method can be cited.

[0178] The thickness of the glass plate subjected to chemical strengthening treatment is preferably 0.1 mm to 3.0 mm, and particularly preferably 0.3 mm to 1.5 mm. Physical strengthening treatment and chemical strengthening treatment of glass may be performed before or after forming an etched surface on the main surface of the glass plate.

[0179] [Example]

[0180] Specific examples are given below for illustration, but the present invention is not limited to these examples.

[0181] <Sample preparation>

[0182] [Examples 1 to 14]

[0183] The glass plate of the present embodiment was produced by the following operation procedure: As a glass substrate, an untempered glass plate (size: 300 mm×300 mm, thickness 1.0 mm) having a composition shown in Table 1 was used.

[0184] First, an acid-resistant protective film is attached to the main surface of the glass plate on the side where the etching surface is not formed. Then, a frosting process is performed according to the following operation steps to form an etching surface on the glass plate.

[0185] The glass plate was immersed in a hydrofluoric acid aqueous solution to remove dirt attached to the main surface of the glass plate on the side where the protective film was not attached, and the thickness of the glass plate was adjusted as a pretreatment. In addition, the glass plate was immersed in a mixed solution of hydrofluoric acid and ammonium fluoride to frost the main surface of the glass plate on the side where the protective film was not attached, and a plurality of fine recesses were formed on the main surface of the glass plate.

[0186] <Evaluation Method>

[0187] The properties of the glass plates produced in Examples 1 to 14 were evaluated by the following methods. The results are shown in Table 1. Examples 1 to 11 are Examples, and Examples 12 to 14 are Comparative Examples. In Table 1, "-" means that the value was not measured.

[0188] (Shape Count)

[0189] For the glass plate, the surface shape of the main surface with an etched surface was measured using a laser microscope (manufactured by Keyence Corporation, trade name VK-X250) for an area of ​​285.12 μm×213.77 μm observed with a 50x objective lens, thereby obtaining XYZ data. In the shape analysis of the XYZ data using the image processing software SPIP6.4.3 manufactured by Image Metrology, after the entire surface was leveled, the number of protrusions detected when the particle detection was set to a threshold level of 50.0000 nm was measured.

[0190] (RSm, RΔa, Ra, Rz)

[0191] For the glass plate, the surface shape of the main surface with the etched surface was analyzed using a laser microscope (manufactured by Keyence Corporation, trade name VK-X250) using a 50x objective lens. RSm, RΔa, Ra, and Rz were obtained by analysis using a multi-file analysis application manufactured by Keyence Corporation. The measurement of Ra, RSm, and Rz was calculated using a calculation formula based on JIS B 0601 (2013). In the data analysis, the cutoff value λs, the phase compensation type high-pass filter λc, and the phase compensation type low-pass filter λf were set to none.

[0192] (Haze rate)

[0193] The haze ratio (%) of the etched surface of the glass plate was measured. The haze ratio was measured using a haze meter (manufactured by Suga Test Instruments Co., Ltd., trade name: HZ-V3) in accordance with JIS K 7136 (2000).

[0194] (Reflection image diffusion index value R)

[0195] A glass plate (100 mm × 100 mm × 1.3 mm) was placed with the first main surface facing upward, and the brightness of the reflected light obtained by irradiating a slit-shaped light with a width of 101 mm from above was measured using SMS-1000 manufactured by DM&S. At this time, in order to eliminate the reflected light from the second main surface (back reflection), a matte black plate was set on the second main surface side. As for the camera lens, a C1614A lens with a focal length of 16 mm was used under the condition of an aperture of 5.6, the distance from the above-mentioned first main surface of the glass plate to the camera lens was set to 300 mm, and the image scale was set in the range of 0.0276 to 0.0278.

[0196] When the direction parallel to the thickness direction of the glass plate is set to angle φ=0°, the angle φ=-5.7° when the light is irradiated from an angle of φ=5.7°±0.1° and totally reflected is used as a reference (angle α=0°). When the average value of the brightness of the reflected light in the range of angle α=0°±0.1° is set to R1, the average value of the brightness of the reflected light in the range of angle α=0.5°±0.1° is set to R2, and the average value of the brightness of the reflected light in the range of angle α=-0.5°±0.1° is set to R3, the value calculated according to the following formula (1) is used as the reflection image diffusion index value R.

[0197] Reflection image diffusion index value R = (R2 + R3) / (2 × R1) Formula (1)

[0198] (Flash value S a )

[0199] A glass plate (100 mm × 100 mm × 1.6 mm) was placed on the display surface side of a display device (iPad (registered trademark)-Air, manufactured by Apple Inc.) having a resolution of 264 ppi so that the second main surface of the glass plate was in contact with the display surface side of the display device. A single green image consisting of RGB (0, 255, 0) was displayed on the display device, and the image analysis was performed using SMS-1000 manufactured by DM&S Co., Ltd., which was placed above the glass plate, to obtain the sparkle value, and the sparkle value was used as the sparkle value S. a The distance d between the solid-state imaging element and the glass plate was set to 540 mm, and as the camera lens, a 23FM50SP lens with a focal length of 50 mm was used under the condition of an aperture of 16.

[0200] (G60)

[0201] The specular gloss GS (60°) of the etched surface of the glass plate at 60° was determined in accordance with JIS Z 8741 (1997). The measurement was performed using Rhopoint IQ-S manufactured by Konica Minolta.

[0202]

[0203] As shown in Table 1, in Examples 1 to 11 as embodiments of the present invention, the basic composition of the glass is within the prescribed range, so the shape count and the sparkle value S a The RSm is good, the flash is effectively suppressed, and the cleaning property is excellent.

[0204] On the other hand, in Example 12 as a comparative example, the content of K2O was not within the prescribed range, the value of the shape count was outside the prescribed range, and the flash value S was a In addition, RSm is slightly higher than that of the embodiment.

[0205] In Example 13 as a comparative example, the content of Al2O3 was not within the prescribed range, the value of the shape count was outside the prescribed range, and the flash value S a and RSm is unsatisfactory.

[0206] In Example 14 as a comparative example, the total content of Na2O, K2O and Li2O was 30% or more, and the value of the shape count was outside the prescribed range. In addition, RSm was also lower than that of the examples, indicating poor cleaning properties.

[0207] In the above, various embodiments are described with reference to the accompanying drawings, but the present invention is not limited to such examples. It is obvious to those skilled in the art that various variations or modifications can be thought of within the scope described in the claims, and these certainly also belong to the technical scope of the present invention. In addition, the various constituent elements in the above embodiments may also be arbitrarily combined within the scope of the purpose of the invention.

[0208] It should be noted that the present application is based on the Japanese patent application (Japanese Patent Application No. 2020-013695) filed on January 30, 2020, the contents of which are incorporated herein by reference.

[0209] Description of symbols

[0210] 50 glass substrate (transparent substrate)

[0211] 52 First main surface

[0212] 53 Second main surface

[0213] 54 Display device

[0214] 70 Measurement device

[0215] 71 Linear light source device

[0216] 75 Surface brightness meter

[0217] 711 Light Source

[0218] 712 Black Tablet

[0219] 731 First incident light

[0220] 732 First Reflected Light

[0221] 733, 734, 735, 736 Light

[0222] 733-2 Hypothetical incident light

[0223] θi Angle of incidence

[0224] θr Reflection angle

Claims

1. A glass substrate, wherein: The glass substrate contains, in terms of molar percentage on an oxide basis: SiO2: 50%~75%, Al2O3: 0.1%~25%, B2O3: 0~10%, Y2O3: 0~5%, MgO: 0-20%, CaO: 0-15%, Li2O: 0~15% Na2O: 1% to 25%, K2O: 0.1%~20%, TiO2: 0-1%, and ZrO2: 0~2% As the basic composition, The content of K2O is less than that of Na2O. and At least one main surface of the glass substrate includes an etched surface having a number of protrusions of 400 or more and 2000 or less as determined by the following method, Method: The XYZ data of the surface shape were obtained by measuring an area of ​​285.12 μm × 213.77 μm using a laser microscope. In the shape analysis of the XYZ data using the image processing software SPIP manufactured by Image Metrology, after the entire surface was leveled, the number of protrusions when the particle detection was set to a threshold level of 50.0000 nm was calculated. Under the condition that there is no cutoff value, the arithmetic mean inclination angle RΔa of the etched surface is greater than or equal to 1.50° and less than or equal to 15°.

2. The glass substrate according to claim 1, wherein The value of the average interval RSm between the concavities and convexities of the etched surface is 30 μm or less.

3. The glass substrate according to claim 1 or 2, wherein: The haze rate of transmitted light of the etched surface measured by a method in accordance with JIS K7136 (2000) is 0.2% to 75%.

4. The glass substrate according to claim 1 or 2, wherein: The flash value S of the etched surface is quantified by the following method: a Below 8, Method: a glass plate is arranged on the display surface side of a display device having a resolution of 264 ppi so that the etched surface contacts the display surface side of the display device; a single green image consisting of RGB (0, 255, 0) is displayed on the display device, an image analysis is performed using SMS-1000 manufactured by DM&S Co., Ltd. arranged above the glass plate to obtain a sparkle value, and the sparkle value is set as the sparkle value S a ; The distance d between the solid-state imaging element and the glass plate is set to 568 mm. As for the camera lens, a 23FM50SP lens with a focal length of 50 mm is used under the condition of an aperture of 16; the measurement is carried out by the difference method (DIM), and 0 is entered in the PixelRatio value to obtain the flash value S a .

5. The glass substrate according to claim 1 or 2, wherein: The total content of Na2O, K2O and Li2O in the basic composition is less than 30% in molar percentage based on oxides.

6. A display device, wherein: The display device comprises the glass substrate according to any one of claims 1 to 5.

7. A method for manufacturing a glass substrate according to any one of claims 1 to 5, wherein the method comprises an etched surface on at least one main surface of which the number of protrusions determined by the following method is 400 or more and 2000 or less and the arithmetic mean inclination angle RΔa is 1.50° or more and 15° or less under the condition that there is no cutoff value, wherein: The method for manufacturing a glass substrate comprises a step of frosting the glass substrate. The glass substrate contains, in terms of molar percentage based on oxides: SiO2: 50%~75%, Al2O3: 0.1%~25%, B2O3: 0~10%, Y2O3: 0~5%, MgO: 0-20%, CaO: 0-15%, Li2O: 0~15% Na2O: 1% to 25%, K2O: 0.1%~20%, TiO2: 0-1%, and ZrO2: 0~2%, The content of K2O is less than that of Na2O. Method: A laser microscope was used to measure an area of ​​285.12 μm × 213.77 μm to obtain XYZ data of the surface shape. In the shape analysis of the XYZ data using the image processing software SPIP manufactured by Image Metrology, after the entire surface was smoothed, the number of protrusions was calculated when the particle detection was set to a threshold level of 50.0000 nm.