Polyimide resin, polyimide varnish and polyimide film

By using a combination of specific structural units in the polyimide resin, the heat resistance, elongation and colorless transparency of the polyimide film are improved, solving the performance problems that are difficult to balance in the existing technology, and is suitable for Display substrate materials.

CN115038737BActive Publication Date: 2024-10-25MITSUBISHI GAS CHEM CO INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180011291.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-30
Filing Date
2021-01-20
Publication Date
2024-10-25
Estimated Expiration
2041-01-20

AI Technical Summary

Technical Problem

In liquid crystal displays and OLED displays, polyimide film substrates are required to have both heat resistance and elongation, as well as excellent colorless transparency. However, it is difficult to improve these properties simultaneously with existing technology.

Method used

Using a polyimide resin containing specific structural units, a polyimide resin with high heat resistance, elongation and colorless transparency is formed through a combination derived from tetracarboxylic dianhydride and diamine. The specific structure Unit includes deicing Plantan-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride and 2,2'-bis(trifluoro Methyl)-4,4'-diaminodiphenyl ether and other compounds.

Benefits of technology

The polyimide resin achieves both improved heat resistance and elongation, and significantly improves colorless transparency, making it suitable for substrate materials for liquid crystal displays and OLED displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115038737B_ABST
    Figure CN115038737B_ABST
Patent Text Reader

Abstract

A polyimide resin, comprising: a structural unit A derived from tetracarboxylic dianhydride and a structural unit B derived from diamine, wherein the structural unit A comprises: a structural unit (A1) derived from a compound represented by the following formula (a1), and the structural unit B comprises: a structural unit (B1) derived from a compound represented by the following formula (b1). #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyimide resin, a polyimide varnish and a polyimide film. Background Art

[0002] Polyimide resins have excellent mechanical properties, and therefore, various applications thereof in the fields of electrical / electronic components are being studied. For example, in order to make devices lighter and more flexible, it is desired to replace glass substrates used in image display devices such as liquid crystal displays and OLED displays with plastic substrates, and research on polyimide resins suitable as such plastic materials is also being promoted. For such applications, high transparency is also required.

[0003] For example, Patent Document 1 discloses a polyimide and a precursor thereof for the purpose of achieving high transparency, bending resistance, high heat resistance, and low linear thermal expansion coefficient. The polyimide comprises repeating units using norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic acids as raw materials, and has a linear thermal expansion coefficient of 100 ppm / K or less at 50 to 400°C.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2018-066017 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] When a polyimide film substrate is used as an image display device such as a liquid crystal display or an OLED display, heat resistance is required for the substrate, especially in the process of forming a polysilicon film on the substrate. In addition, in recent years, in order to achieve thinning and flexibility of devices, elongation, which is one of the indicators of toughness, is also required for polyimide films. However, films with excellent heat resistance are hard and have poor elongation.

[0009] Furthermore, for display applications, the aforementioned transparency is not only important, but colorlessness is also more important. As described above, a polyimide resin is required that can provide a polyimide film that has both heat resistance and elongation and is also excellent in colorlessness and transparency.

[0010] An object of the present invention is to provide a polyimide resin which has both heat resistance and elongation and is excellent in colorlessness and transparency.

[0011] Solutions for solving problems

[0012] The present inventors have found that a polyimide resin including a combination of specific structural units can solve the above-mentioned problems, and have thus completed the invention.

[0013] That is, the present invention relates to the following [1] to [8].

[0014] [1] A polyimide resin comprising: a structural unit A derived from tetracarboxylic dianhydride and a structural unit B derived from diamine,

[0015] The structural unit A comprises: a structural unit (A1) derived from a compound represented by the following formula (a1),

[0016] The structural unit B includes a structural unit (B1) derived from a compound represented by the following formula (b1).

[0017]

[0018] [2] The polyimide resin according to the above [1], wherein the structural unit A further comprises a structural unit (A2), and the structural unit (A2) is at least one selected from the group consisting of a structural unit (A21) derived from a compound represented by the following formula (a21), a structural unit (A22) derived from a compound represented by the following formula (a22), and a structural unit (A23) derived from a compound represented by the following formula (a23).

[0019]

[0020] [3] The polyimide resin according to [1] or [2] above, wherein the structural unit B further comprises a structural unit (B2), and the structural unit (B2) is at least one selected from the group consisting of a structural unit (B21) derived from a compound represented by the following formula (b21) and a structural unit (B22) derived from a compound represented by the following formula (b22).

[0021]

[0022] [4] The polyimide resin according to any one of [1] to [3] above, wherein the structural unit B further includes a structural unit (B2), and the structural unit (B2) includes a structural unit (B22) derived from a compound represented by the following formula (b22).

[0023]

[0024] [5] The polyimide resin according to any one of [1] to [4] above, wherein the structural unit A further includes a structural unit (A2), and the structural unit (A2) includes a structural unit (A22) derived from a compound represented by the following formula (a22).

[0025]

[0026] [6] A polyimide varnish obtained by dissolving the polyimide resin according to any one of [1] to [5] above in an organic solvent.

[0027] [7] A polyimide film comprising the polyimide resin according to any one of [1] to [5] above.

[0028] [8] A method for producing a polyimide film, comprising: applying or molding the polyimide varnish described in [6] into a film, and then removing the organic solvent.

[0029] Effects of the Invention

[0030] The polyimide resin of the present invention has both heat resistance and elongation and is also excellent in colorlessness and transparency. DETAILED DESCRIPTION

[0031] [Polyimide resin]

[0032] The polyimide resin of the present invention is a polyimide resin comprising: a structural unit A derived from tetracarboxylic dianhydride and a structural unit B derived from diamine, wherein the structural unit A comprises: a structural unit (A1) derived from a compound represented by the following formula (a1), and the structural unit B comprises: a structural unit (B1) derived from a compound represented by the following formula (b1).

[0033]

[0034] The reason why the polyimide resin of the present invention can achieve both heat resistance and elongation and is also excellent in colorlessness and transparency by including the structural units (A1) and (B1) is not clear, but it is believed that this is due to the combined effect of the rigidity and randomness of the molecular chain caused by the norbornane skeleton, ether bonds, etc.

[0035] <Structural unit A>

[0036] The structural unit A is a structural unit derived from tetracarboxylic dianhydride, and includes a structural unit (A1) derived from a compound represented by formula (a1). The structural unit (A1) improves heat resistance, elongation, and colorless transparency, and particularly improves heat resistance and colorless transparency.

[0037] The compound represented by formula (a1) is norbornane-2-spiro-α-cyclopentanone-α′-spiro-2″-norbornane-5,5″,6,6″-tetracarboxylic dianhydride.

[0038] The structural unit A may contain structural units other than the structural unit (A1).

[0039] The structural unit A preferably contains a structural unit (A2) in addition to the structural unit (A1). The structural unit (A2) is a structural unit derived from a compound represented by the following formula (a2). The structural unit (A2) improves the elongation, and further improves mechanical properties such as strength.

[0040]

[0041] In formula (a2), L is a single bond or a divalent linking group. The divalent linking group is preferably a substituted or unsubstituted alkylene group, more preferably -CR 1 R 2 -(Here, R 1 and R 2 are each independently a hydrogen atom or a substituted or unsubstituted alkyl group, or R 1 and R 2 bonded to each other to form a ring. ).

[0042] L is preferably one selected from the group consisting of a single bond, a group represented by the following formula (L1) and a group represented by the following formula (L2). In the following formulas (L1) and (L2), * represents a bonding site to an aromatic ring.

[0043]

[0044] The structural unit (A2) is preferably at least one selected from the group consisting of a structural unit (A21) derived from a compound represented by the following formula (a21), a structural unit (A22) derived from a compound represented by the following formula (a22), and a structural unit (A23) derived from a compound represented by the following formula (a23). It is preferably at least one selected from the group consisting of a structural unit (A21) derived from a compound represented by the following formula (a21) and a structural unit (A22) derived from a compound represented by the following formula (a22). From the viewpoint of improving elongation, the structural unit (A21) derived from the compound represented by the following formula (a21) is more preferred. From the viewpoint of heat resistance, the structural unit (A22) derived from the compound represented by the following formula (a22) is more preferred.

[0045] That is, it is more preferred that the structural unit A further includes the structural unit (A2), and the structural unit (A2) includes the structural unit (A21) derived from the compound represented by the following formula (a21). It is more preferred that the structural unit A further includes the structural unit (A2), and the structural unit (A2) includes the structural unit (A22) derived from the compound represented by the following formula (a22).

[0046]

[0047] The compound represented by formula (a21) is biphenyltetracarboxylic dianhydride (BPDA). Specific examples thereof include 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA) represented by the following formula (a21s), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA) represented by the following formula (a21a), and 2,2',3,3'-biphenyltetracarboxylic dianhydride (i-BPDA) represented by the following formula (a21i).

[0048]

[0049] The compound represented by formula (a22) is 9,9′-bis(3,4-dicarboxyphenyl)fluorene dianhydride.

[0050] The compound represented by formula (a23) is 4,4'-(hexafluoroisopropylidene)diphthalic anhydride.

[0051] The content ratio of the structural unit (A1) in the structural unit A is preferably 50 mol% or more, more preferably 55 mol% or more, further preferably 60 mol% or more, further preferably 80 mol% or more, further preferably 90 mol% or more, further preferably 95 mol% or more. The upper limit of the content ratio of the structural unit (A1) is not particularly limited, that is, 100 mol%. The structural unit A may be composed only of the structural unit (A1). By including the structural unit (A1) in the aforementioned content ratio in the structural unit A, the colorless transparency and heat resistance are particularly excellent.

[0052] When the structural unit A contains the structural unit (A2), the ratio of the structural unit (A2) in the structural unit A is preferably 5 to 50 mol%, more preferably 10 to 40 mol%, further preferably 15 to 35 mol%.

[0053] When the structural unit A contains the structural unit (A2), the molar ratio of the structural unit (A1) to the structural unit (A2) [(A1) / (A2)] is preferably 50 / 50 to 95 / 5, more preferably 60 / 40 to 90 / 10, and further preferably 65 / 35 to 85 / 15. When the structural unit A contains the structural unit (A2) at the above content ratio, the mechanical properties such as elongation and strength are particularly excellent.

[0054] The structural unit A may contain structural units other than the structural units (A1) and (A2). The tetracarboxylic dianhydride forming such a structural unit is not particularly limited, and examples thereof include aromatic tetracarboxylic dianhydrides such as pyromellitic dianhydride (excluding compounds represented by formula (a2)); alicyclic tetracarboxylic dianhydrides such as 1,2,3,4-cyclobutane tetracarboxylic dianhydride and 1,2,4,5-cyclohexane tetracarboxylic dianhydride (excluding compounds represented by formula (a1)); and aliphatic tetracarboxylic dianhydrides such as 1,2,3,4-butane tetracarboxylic dianhydride.

[0055] It should be noted that, in the present specification, aromatic tetracarboxylic dianhydride refers to a tetracarboxylic dianhydride containing one or more aromatic rings, alicyclic tetracarboxylic dianhydride refers to a tetracarboxylic dianhydride containing one or more alicyclic rings and no aromatic ring, and aliphatic tetracarboxylic dianhydride refers to a tetracarboxylic dianhydride containing neither an aromatic ring nor an alicyclic ring.

[0056] The structural unit other than the structural unit (A1) optionally contained in the structural unit A may be one kind or two or more kinds.

[0057] <Structural unit B>

[0058] Structural unit B is a structural unit derived from a diamine, and includes structural unit (B1) derived from a compound represented by formula (b1). Structural unit (B1) improves heat resistance, elongation, and colorless transparency, especially elongation, and further improves colorlessness.

[0059] The compound represented by formula (b1) is 2,2′-bis(trifluoromethyl)-4,4′-diaminodiphenyl ether (6FODA).

[0060] The structural unit B may contain structural units other than the structural unit (B1).

[0061] The structural unit B preferably contains a structural unit (B2) in addition to the structural unit (B1). The structural unit (B2) is preferably at least one selected from the group consisting of a structural unit (B21) derived from a compound represented by the following formula (b21) and a structural unit (B22) derived from a compound represented by the following formula (b22). The structural unit (B2) improves heat resistance in particular and further improves elastic modulus.

[0062] From the viewpoint of improving transparency, dimensional stability to heat, and elastic modulus, structural unit (B2) is preferably a structural unit (B22) derived from a compound represented by formula (b22). That is, it is preferred that structural unit B further comprises structural unit (B2), and structural unit (B2) comprises structural unit (B22) derived from a compound represented by the following formula (b22).

[0063] The structural unit (B2) is also preferably a structural unit (B21) derived from a compound represented by the formula (b21). The structural unit (B21) improves particularly the heat resistance and the elastic modulus.

[0064]

[0065] The compound represented by formula (b21) is 9,9-bis(4-aminophenyl)fluorene.

[0066] The compound represented by formula (b22) is 2,2'-bis(trifluoromethyl)benzidine.

[0067] The content ratio of the structural unit (B1) in the structural unit B is preferably 10 mol% or more, more preferably 20 mol% or more, further preferably 30 mol% or more, further preferably 50 mol% or more, further preferably 60 mol% or more, further preferably 80 mol% or more. The upper limit of the content ratio of the structural unit (B1) is not particularly limited, that is, it is 100 mol%. The structural unit B may be composed only of the structural unit (B1). By including the structural unit (B1) in the structural unit B at the above content ratio, the elongation is improved, and the colorlessness is also improved.

[0068] When the structural unit B contains the structural unit (B2), the ratio of the structural unit (B2) in the structural unit B is preferably 1 to 90 mol%, more preferably 1 to 80 mol%, further preferably 2 to 70 mol%, further preferably 3 to 50 mol%, further preferably 4 to 40 mol%, further preferably 5 to 20 mol%.

[0069] When the structural unit B contains the structural unit (B2), the molar ratio of the structural unit (B1) to the structural unit (B2) [(B1) / (B2)] is preferably 10 / 90 to 99 / 1, more preferably 20 / 80 to 99 / 1, further preferably 30 / 70 to 98 / 2, further preferably 50 / 50 to 97 / 3, further preferably 60 / 40 to 96 / 4, further preferably 80 / 20 to 95 / 5, particularly from the viewpoint of colorlessness, elongation and transparency.

[0070] In addition, from the viewpoint of improving mechanical properties such as elastic modulus, heat resistance, and thermal properties such as dimensional stability against heat, the molar ratio of structural unit (B1) to structural unit (B2) [(B1) / (B2)] is preferably 10 / 90 to 60 / 40, more preferably 10 / 90 to 50 / 50, further preferably 10 / 90 to 40 / 60, further preferably 10 / 90 to 30 / 70, further preferably 10 / 90 to 20 / 80, further preferably 10 / 90 to 15 / 85.

[0071] When structural unit B contains structural unit (B2) and structural unit (B2) contains structural unit (B22), the molar ratio of structural unit (B1) to structural unit (B22) [(B1) / (B22)] is preferably 10 / 90 to 99 / 1, more preferably 20 / 80 to 99 / 1, further preferably 30 / 70 to 98 / 2, further preferably 50 / 50 to 97 / 3, further preferably 60 / 40 to 96 / 4, further preferably 80 / 20 to 95 / 5, particularly from the viewpoint of colorlessness, elongation and transparency.

[0072] In addition, from the viewpoint of improving mechanical properties such as elastic modulus, heat resistance, and thermal properties such as dimensional stability against heat, the molar ratio of structural unit (B1) to structural unit (B22) [(B1) / (B22)] is preferably 10 / 90 to 60 / 40, more preferably 10 / 90 to 50 / 50, further preferably 10 / 90 to 40 / 60, further preferably 10 / 90 to 30 / 70, further preferably 10 / 90 to 20 / 80, further preferably 10 / 90 to 15 / 85.

[0073] The structural unit B may contain structural units other than the structural units (B1) and (B2). The diamine forming such a structural unit is not particularly limited, and examples thereof include 1,4-phenylenediamine, p-phenylenediamine, 3,5-diaminobenzoic acid, 2,2'-dimethylbiphenyl-4,4'-diamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 2,2-bis(4-aminophenyl)hexafluoropropane, bis(4-aminophenyl)sulfone, 4,4'-diaminobenzanilide, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-5-amine, α,α'-bis(4-aminophenyl)-1,4-diisocyanate, and α,α'-bis(4-aminophenyl)-1,4-diisocyanate. Aromatic diamines such as propylbenzene, N,N'-bis(4-aminophenyl)terephthalamide, 4,4'-bis(4-aminophenoxy)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and 2,2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane (excluding compounds represented by formula (b1), compounds represented by formula (b21), and compounds represented by formula (b22); alicyclic diamines such as 1,3-bis(aminomethyl)cyclohexane and 1,4-bis(aminomethyl)cyclohexane; and aliphatic diamines such as ethylenediamine and hexamethylenediamine.

[0074] In this specification, aromatic diamine refers to a diamine containing one or more aromatic rings, alicyclic diamine refers to a diamine containing one or more alicyclic rings and no aromatic ring, and aliphatic diamine refers to a diamine containing neither an aromatic ring nor an alicyclic ring.

[0075] The structural unit other than the structural unit (B1) optionally contained in the structural unit B may be one kind or two or more kinds.

[0076] <Characteristics of polyimide resin>

[0077] From the viewpoint of mechanical strength of the obtained polyimide film, the number average molecular weight of the polyimide resin of the present invention is preferably 5000 to 200000. The number average molecular weight of the polyimide resin can be determined, for example, from a standard polymethyl methacrylate (PMMA) conversion value measured by gel filtration chromatography.

[0078] The polyimide resin of the present invention has both heat resistance and elongation, is excellent in colorlessness and transparency, and can have the following physical property values.

[0079] When the polyimide resin of the present invention is made into a polyimide film having a thickness of 10 μm, the total light transmittance is preferably 85% or more, more preferably 88% or more, further preferably 90% or more, and further preferably 91% or more.

[0080] When the polyimide resin of the present invention is formed into a polyimide film having a thickness of 10 μm, the yellowness index (YI) is preferably 3.5 or less, more preferably 3.0 or less, and even more preferably 2.0 or less.

[0081] The glass transition temperature (Tg) of the polyimide resin of the present invention is preferably 350° C. or higher, more preferably 380° C. or higher, further preferably 400° C. or higher, and further preferably 430° C. or higher.

[0082] It should be noted that the total light transmittance, yellowness index (YI) and glass transition temperature (Tg) in the present invention can be specifically measured by the methods described in the Examples.

[0083] [Method for producing polyimide resin]

[0084] The polyimide resin of the present invention can be produced by reacting a tetracarboxylic acid component containing a compound providing the above structural unit (A1) with a diamine component containing a compound providing the above structural unit (B1).

[0085] As the compound providing the structural unit (A1), the compound represented by formula (a1) can be cited, but it is not limited thereto, and its derivative can be formed within the scope of the same structural unit. As the derivative, the tetracarboxylic acid corresponding to the compound represented by formula (a1) (i.e., norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic acid) and the alkyl ester of the tetracarboxylic acid can be cited. As the compound providing the structural unit (A1), the compound represented by formula (a1) (i.e., tetracarboxylic dianhydride) is preferred.

[0086] The tetracarboxylic acid component may contain a compound other than the compound providing the structural unit (A1). The tetracarboxylic acid component preferably contains a compound providing the structural unit (A2) in addition to the compound providing the structural unit (A1).

[0087] As the compound providing structural unit (A2), the compound shown in formula (a2) can be cited, but it is not limited thereto, and can be its derivative within the scope of forming the same structural unit. As the derivative, tetracarboxylic acid corresponding to the compound shown in formula (a2) and the alkyl ester of the tetracarboxylic acid can be cited. As the compound providing structural unit (A2), the compound shown in formula (a2) (i.e., tetracarboxylic dianhydride) is preferred.

[0088] The compound providing the structural unit (A2) is preferably: at least one selected from the group consisting of a compound providing the structural unit (A21) represented by formula (a21), a compound providing the structural unit (A22) represented by formula (a22), and a compound providing the structural unit (A23) represented by formula (a23); preferably: at least one selected from the group consisting of a compound providing the structural unit (A21) and a compound providing the structural unit (A22); from the viewpoint of improving elongation, a compound providing the structural unit (A21) is more preferred; from the viewpoint of heat resistance, a compound providing the structural unit (A22) is more preferred.

[0089] The tetracarboxylic acid component preferably contains 50 mol% or more, more preferably 55 mol% or more, further preferably 60 mol% or more, further preferably 80 mol% or more, further preferably 90 mol% or more, and further preferably 95 mol% or more of the compound providing the structural unit (A1). The upper limit of the content ratio of the compound providing the structural unit (A1) is not particularly limited, that is, 100 mol%. The tetracarboxylic acid component may be composed only of the compound providing the structural unit (A1).

[0090] When the tetracarboxylic acid component contains a compound providing structural unit (A2), the tetracarboxylic acid component preferably contains 5 to 50 mol%, more preferably 10 to 40 mol%, and further preferably 15 to 35 mol%.

[0091] When the tetracarboxylic acid component contains a compound providing the structural unit (A2), the molar ratio [(A1) / (A2)] of the compound providing the structural unit (A1) to the compound providing the structural unit (A2) is preferably 50 / 50 to 95 / 5, more preferably 60 / 40 to 90 / 10, and further preferably 65 / 35 to 85 / 15.

[0092] The tetracarboxylic acid component may contain compounds other than the compound providing the structural unit (A1) and the compound providing the structural unit (A2), and examples of such compounds include the above-mentioned aromatic tetracarboxylic dianhydride, alicyclic tetracarboxylic dianhydride, and aliphatic tetracarboxylic dianhydride, and derivatives thereof (tetracarboxylic acids, alkyl esters of tetracarboxylic acids, etc.).

[0093] The compound optionally contained in the tetracarboxylic acid component (that is, the compound other than the compound which provides the structural unit (A1)) may be one kind or two or more kinds.

[0094] As the compound providing the structural unit (B1), the compound shown in formula (b1) can be cited, but it is not limited thereto, and it can be a derivative thereof within the scope of being able to form the same structural unit. As the derivative, a diisocyanate corresponding to the compound shown in formula (b1) can be cited. As the compound providing the structural unit (B1), the compound shown in formula (b1) (i.e., diamine) is preferred.

[0095] The diamine component may contain a compound other than the compound providing the structural unit (B1). The diamine component preferably contains a compound providing the structural unit (B2) in addition to the compound providing the structural unit (B1).

[0096] From the viewpoint of improving transparency, dimensional stability to heat, and elastic modulus, the compound providing the structural unit (B2) is preferably a compound providing the structural unit (B22) shown in formula (b22), and from the viewpoint of improving heat resistance and elastic modulus, the structural unit (B2) is preferably a compound providing the structural unit (B21) shown in formula (b21).

[0097] As the compound providing structural unit (B2), the compound shown in formula (b21) and the compound shown in formula (b22) can be cited, but it is not limited thereto, and can be its derivative within the scope of forming the same structural unit. As the derivative, the diisocyanate corresponding to the compound shown in formula (b21) and the diisocyanate corresponding to the compound shown in formula (b22) can be cited. As the compound providing structural unit (B2), the compound shown in formula (b21) and the compound shown in formula (b22) (i.e., diamine) are preferred.

[0098] The diamine component preferably contains 10 mol% or more, more preferably 20 mol% or more, further preferably 30 mol% or more, further preferably 50 mol% or more, further preferably 60 mol% or more, further preferably 80 mol% or more of the compound providing the structural unit (B1). The upper limit of the content ratio of the compound providing the structural unit (B1) is not particularly limited, that is, 100 mol%. The diamine component may be composed only of the compound providing the structural unit (B1).

[0099] When the diamine component contains a compound that provides the structural unit (B2), the diamine component preferably contains 1 to 90 mol%, more preferably 1 to 80 mol%, further preferably 2 to 70 mol%, further preferably 3 to 50 mol%, further preferably 4 to 40 mol%, further preferably 5 to 20 mol% of the compound that provides the structural unit (B2).

[0100] When the diamine component contains a compound providing the structural unit (B2), the molar ratio [(B1) / (B2)] of the compound providing the structural unit (B1) to the compound providing the structural unit (B2) is preferably 10 / 90 to 99 / 1, more preferably 20 / 80 to 99 / 1, further preferably 30 / 70 to 98 / 2, further preferably 50 / 50 to 97 / 3, further preferably 60 / 40 to 96 / 4, further preferably 80 / 20 to 95 / 5, particularly from the viewpoint of colorlessness, elongation and transparency.

[0101] In addition, from the viewpoint of improving mechanical properties such as elastic modulus, heat resistance, and thermal properties such as dimensional stability against heat, the molar ratio of the compound providing the structural unit (B1) to the compound providing the structural unit (B2) [(B1) / (B2)] is preferably 10 / 90 to 60 / 40, more preferably 10 / 90 to 50 / 50, further preferably 10 / 90 to 40 / 60, further preferably 10 / 90 to 30 / 70, further preferably 10 / 90 to 20 / 80, further preferably 10 / 90 to 15 / 85.

[0102] When the diamine component contains a compound providing the structural unit (B2), and the compound providing the structural unit (B2) contains a compound providing the structural unit (B22), the molar ratio [(B1) / (B22)] of the compound providing the structural unit (B1) to the compound providing the structural unit (B22) is preferably 10 / 90 to 99 / 1, more preferably 20 / 80 to 99 / 1, further preferably 30 / 70 to 98 / 2, further preferably 50 / 50 to 97 / 3, further preferably 60 / 40 to 96 / 4, further preferably 80 / 20 to 95 / 5, particularly from the viewpoint of colorlessness, elongation and transparency.

[0103] In addition, from the viewpoint of improving mechanical properties such as elastic modulus, heat resistance, and thermal properties such as dimensional stability against heat, the molar ratio [(B1) / (B22)] of the compound providing the structural unit (B1) to the compound providing the structural unit (B22) is preferably 10 / 90 to 60 / 40, more preferably 10 / 90 to 50 / 50, further preferably 10 / 90 to 40 / 60, further preferably 10 / 90 to 30 / 70, further preferably 10 / 90 to 20 / 80, further preferably 10 / 90 to 15 / 85.

[0104] The diamine component may contain compounds other than the compound providing the structural unit (B1) and the compound providing the structural unit (B2), and examples of such compounds include the above-mentioned aromatic diamines, alicyclic diamines, and aliphatic diamines, and derivatives thereof (such as diisocyanates).

[0105] The compound optionally contained in the diamine component (that is, the compound other than the compound which provides the structural unit (B1)) may be one kind or two or more kinds.

[0106] In the present invention, the charging amount ratio of the tetracarboxylic acid component and the diamine component used for producing the polyimide resin is preferably 0.9 to 1.1 mol of the diamine component relative to 1 mol of the tetracarboxylic acid component.

[0107] In addition, in the present invention, in the manufacture of the polyimide resin, in addition to the aforementioned tetracarboxylic acid component and diamine component, an end-capping agent can also be used. As the end-capping agent, monoamines or dicarboxylic acids are preferred. The amount of the introduced end-capping agent is preferably 0.0001 to 0.1 moles, particularly preferably 0.001 to 0.06 moles, relative to 1 mole of the tetracarboxylic acid component. As monoamine end-capping agents, for example, methylamine, ethylamine, propylamine, butylamine, benzylamine, 4-methylbenzylamine, 4-ethylbenzylamine, 4-dodecylbenzylamine, 3-methylbenzylamine, 3-ethylbenzylamine, aniline, 3-methylaniline, 4-methylaniline, etc. are recommended. Among them, benzylamine and aniline can be suitably used. As dicarboxylic acid end-capping agents, dicarboxylic acids are preferred, and a part of them can be ring-closed. For example, phthalic acid, phthalic anhydride, 4-chlorophthalic acid, tetrafluorophthalic acid, 2,3-benzophenone dicarboxylic acid, 3,4-benzophenone dicarboxylic acid, cyclohexane-1,2-dicarboxylic acid, cyclopentane-1,2-dicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, etc. are recommended. Among them, phthalic acid and phthalic anhydride can be preferably used.

[0108] The method for reacting the tetracarboxylic acid component and the diamine component is not particularly limited, and a known method can be used.

[0109] As specific reaction methods, the following methods can be cited: method (1), a tetracarboxylic acid component, a diamine component, and a reaction solvent are added to a reactor, stirred at 0 to 80° C. for 0.5 to 30 hours, and then heated to carry out an imidization reaction; method (2), after adding a diamine component and a reaction solvent to dissolve them in a reactor, a tetracarboxylic acid component is added, and as needed, stirred at 0 to 80° C. for 0.5 to 30 hours, and then heated to carry out an imidization reaction; method (3), a tetracarboxylic acid component, a diamine component, and a reaction solvent are added to a reactor, and the temperature is immediately raised to carry out an imidization reaction; etc.

[0110] The reaction solvent used in the production of the polyimide resin may be any solvent that does not inhibit the imidization reaction and can dissolve the generated polyimide, and examples thereof include aprotic solvents, phenolic solvents, etheric solvents, carbonate solvents, and the like.

[0111] Specific examples of aprotic solvents include amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-methylcaprolactam, 1,3-dimethylimidazolidinone, and tetramethylurea, lactone solvents such as γ-butyrolactone and γ-valerolactone, phosphorus-containing amide solvents such as hexamethylphosphoramide and hexamethylphosphinetriamide, sulfur-containing solvents such as dimethyl sulfone, dimethyl sulfoxide, and cyclopentane, ketone solvents such as acetone, cyclohexanone, and methylcyclohexanone, amine solvents such as picoline and pyridine, and ester solvents such as (2-methoxy-1-methylethyl)acetate.

[0112] Specific examples of the phenolic solvent include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol.

[0113] Specific examples of the ether solvent include 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, and 1,4-dioxane.

[0114] Specific examples of the carbonate-based solvent include diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, and propylene carbonate.

[0115] Among the above reaction solvents, amide solvents or lactone solvents are preferred. In addition, the above reaction solvents may be used alone or in combination of two or more.

[0116] In the imidization reaction, it is preferred to use a Dean-Stark water trap apparatus or the like to carry out the reaction while removing water generated during the production. By carrying out such an operation, the degree of polymerization and the imidization ratio can be further increased.

[0117] In the above-mentioned imidization reaction, a known imidization catalyst can be used. Examples of the imidization catalyst include a base catalyst and an acid catalyst.

[0118] Examples of the base catalyst include organic base catalysts such as pyridine, quinoline, isoquinoline, α-methylpyridine, β-methylpyridine, 2,4-lutidine, 2,6-lutidine, trimethylamine, triethylamine, tripropylamine, tributylamine, triethylenediamine, imidazole, N,N-dimethylaniline, and N,N-diethylaniline; and inorganic base catalysts such as potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, potassium hydrogen carbonate, and sodium hydrogen carbonate.

[0119] Examples of the acid catalyst include crotonic acid, acrylic acid, trans-3-hexenoic acid, cinnamic acid, benzoic acid, methylbenzoic acid, hydroxybenzoic acid, terephthalic acid, benzenesulfonic acid, p-toluenesulfonic acid, and naphthalenesulfonic acid. The imidization catalysts described above may be used alone or in combination of two or more.

[0120] Among the above, from the viewpoint of operability, it is preferred to use a base catalyst, more preferably to use an organic base catalyst, further preferably to use triethylamine, and particularly preferably to use triethylamine and triethylenediamine in combination.

[0121] From the viewpoint of reaction rate and suppression of gelation, the temperature of the imidization reaction is preferably 120 to 250° C., more preferably 160 to 200° C. The reaction time is preferably 0.5 to 10 hours after the start of distillation of generated water.

[0122] [Polyimide varnish]

[0123] The polyimide varnish of the present invention is obtained by dissolving the polyimide resin of the present invention in an organic solvent. That is, the polyimide varnish of the present invention contains the polyimide resin of the present invention and an organic solvent, and the polyimide resin is dissolved in the organic solvent.

[0124] The organic solvent is not particularly limited as long as it can dissolve the polyimide resin, and it is preferred to use the above-mentioned compounds used as a reaction solvent in the production of the polyimide resin alone or in combination of two or more.

[0125] The polyimide resin of the present invention has solvent solubility, and therefore, a stable high-concentration varnish can be formed at room temperature. The polyimide varnish of the present invention preferably contains 3 to 40% by mass, and more preferably contains 5 to 30% by mass of the polyimide resin of the present invention. The viscosity of the polyimide varnish is preferably 0.1 to 200 Pa·s, and more preferably 0.5 to 150 Pa·s.

[0126] In addition, the polyimide varnish of the present invention may contain various additives such as inorganic fillers, adhesion promoters, release agents, flame retardants, ultraviolet stabilizers, surfactants, leveling agents, defoaming agents, fluorescent brighteners, crosslinking agents, polymerization initiators, and photosensitizers within the range that the required properties of the polyimide film are not impaired.

[0127] The method for producing the polyimide varnish of the present invention is not particularly limited, and a known method can be applied.

[0128] [Polyimide film and method for producing polyimide film]

[0129] The polyimide film of the present invention contains the polyimide resin of the present invention. Therefore, the polyimide film of the present invention has good heat resistance and elongation, and is also excellent in colorless transparency.

[0130] There is no particular limitation on the method for manufacturing the polyimide film of the present invention, and a known method can be used. For example, a method of removing an organic solvent after the polyimide varnish of the present invention is applied or formed into a film, etc. From the viewpoint of obtaining a smooth film of a target thickness, a method of removing an organic solvent after the polyimide varnish of the present invention is preferably applied or formed into a film.

[0131] The polyimide film of the present invention has good heat resistance and elongation, and is also excellent in colorless transparency, and is therefore suitable for use as a film for various components such as color filters, flexible displays, semiconductor components, and optical components. The polyimide film of the present invention is particularly suitable for use as a substrate for image display devices such as liquid crystal displays and OLED displays.

[0132] Example

[0133] Hereinafter, the present invention will be specifically described based on examples, but the present invention is not limited to these examples.

[0134] The solid content concentration of the varnish obtained in the examples and comparative examples and the various physical properties of the polyimide films were measured by the methods shown below.

[0135] (1) Solid content concentration

[0136] The solid content concentration of the varnish was measured by heating a sample at 320° C. for 120 minutes using a small electric furnace “MMF-1” manufactured by AS ONE Corporation, and calculating the solid content concentration from the difference in mass of the sample before and after heating.

[0137] (2) Film thickness

[0138] The film thickness was measured using a micrometer manufactured by Mitutoyo Co., Ltd.

[0139] (3) Total light transmittance, yellowness index (YI)

[0140] The measurement was performed in accordance with JIS K7361-1 using a color / turbidity simultaneous measuring device "COH400" manufactured by Nippon Denshoku Industries, Ltd.

[0141] (4)Haze

[0142] The measurement was performed in accordance with JIS K7361-1 using a color / turbidity simultaneous measuring device "COH7700" manufactured by Nippon Denshoku Industries Co., Ltd.

[0143] (5) Glass transition temperature (Tg)

[0144] Using a thermomechanical analyzer "TMA / SS6100" manufactured by Hitachi High-Tech Science Corporation, in tensile mode, the temperature was raised to above Tg under the conditions of a sample size of 2 mm × 20 mm, a load of 0.1 N, and a heating rate of 10°C / min to remove residual stress, and then TMA measurement was performed from 50°C to 500°C under the same conditions to determine Tg.

[0145] (6) Coefficient of thermal expansion (CTE)

[0146] Using a thermomechanical analyzer "TMA / SS6100" manufactured by Hitachi High-Tech Science Corporation, TMA measurement was performed in a tensile mode under the conditions of a sample size of 2 mm×20 mm, a load of 0.1 N, and a heating rate of 10°C / min to determine CTE at 100 to 350°C.

[0147] (7) 1% weight loss temperature (Td1%)

[0148] A differential thermal and thermogravimetric simultaneous measuring device "TG / DTA6200" manufactured by Hitachi High-Tech Science Corporation was used. The sample was heated from 40°C to 550°C at a heating rate of 10°C / min, and the temperature at which the weight decreased by 1% compared to the weight at 300°C was taken as the 1% weight loss temperature. The larger the value of the weight loss temperature, the better.

[0149] (8) Elastic modulus and strength

[0150] The elastic modulus and strength are measured in accordance with the tensile elastic modulus and tensile strength of JIS K7127 using a tensile testing machine "Strograph VG-1E" manufactured by Toyo Seiki Co., Ltd.

[0151] (9) Elongation

[0152] The elongation was measured by a tensile test (elongation measurement) in accordance with JIS K7127. A test piece having a width of 10 mm and a thickness of 10 to 60 μm was used.

[0153] The tetracarboxylic acid component and the diamine component used in Examples and Comparative Examples, and their abbreviations and the like are as follows.

[0154] <Tetracarboxylic acid component>

[0155] CpODA: Norbornane-2-spiro-α-cyclopentanone-α′-spiro-2″-norbornane-5,5″,6,6″-tetracarboxylic dianhydride (manufactured by JX Energy Ltd.; compound represented by formula (a1))

[0156] s-BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride (compound represented by formula (a21s))

[0157] BPAF: 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride (manufactured by JFE Chemical Corporation; compound represented by formula (a22))

[0158] TAHQ: p-phenylene bis(trimellitate) dianhydride (manufactured by Manac Inc.)

[0159] <Diamine component>

[0160] 6FODA: 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (manufactured by ChinaTech (Tianjin) Chemical Co., Ltd., a compound represented by formula (b1))

[0161] BAFL: 9,9-bis(4-aminophenyl)fluorene (produced by Taoka Chemical Industry Co., Ltd.; compound represented by formula (b21))

[0162] TFMB: 2,2'-bis(trifluoromethyl)benzidine (manufactured by Wakayama Seika Industries, Ltd.; compound represented by formula (b22))

[0163] The abbreviations and the like of the solvents and imidization catalysts used in Examples and Comparative Examples are as follows.

[0164] NMP: N-methyl-2-pyrrolidone (manufactured by Mitsubishi Chemical Corporation)

[0165] GBL: γ-butyrolactone (manufactured by Mitsubishi Chemical Corporation)

[0166] TEDA: triethylenediamine

[0167] TEA: triethylamine

[0168] <Example 1>

[0169] Into a 500 mL five-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet tube, a Dean-Stark trap equipped with a condenser, a thermometer, and glass end caps, 33.624 g (0.100 mol) of 6FODA and 86.474 g of GBL were added, and the mixture was stirred at a temperature of 70° C. in a nitrogen atmosphere at a rotation speed of 200 rpm to obtain a solution.

[0170] To this solution, 38.438 g (0.100 mol) of CpODA and 21.619 g of GBL were added simultaneously, and then 0.506 g of TEA and 0.056 g of TEDA were added as imidization catalysts, and the mixture was heated in a hooded heater to raise the temperature in the reaction system to 190° C. over about 20 minutes. The components removed by distillation were collected, and the rotation speed was adjusted according to the increase in viscosity, and the temperature in the reaction system was maintained at 190° C., and reflux was performed for about 5 hours.

[0171] Thereafter, 279.836 g of GBL was added so as to have a solid content concentration of 15% by mass, and after the temperature in the reaction system was cooled to 100° C., the mixture was further stirred for about 1 hour for homogenization to obtain a polyimide varnish.

[0172] The obtained polyimide varnish was then applied onto a glass plate by spin coating, maintained on a hot plate at 80°C for 20 minutes, and then heated at 400°C for 30 minutes (heating rate 5°C / min) in a hot air dryer under a nitrogen atmosphere to evaporate the solvent and obtain a thin film.

[0173] <Example 2>

[0174] A polyimide varnish was prepared in the same manner as in Example 1 except that the amount of CpODA was changed from 38.438 g (0.100 mol) to 30.750 g (0.080 mol) and 5.884 g (0.020 mol) of s-BPDA was added to obtain a polyimide varnish having a solid content concentration of 15% by mass.

[0175] A film was obtained by the same method as in Example 1 using the obtained polyimide varnish.

[0176] <Example 3>

[0177] A polyimide varnish was prepared in the same manner as in Example 1 except that the amount of 6FODA was changed from 33.624 g (0.100 mol) to 3.362 g (0.010 mol) and 8.822 g (0.090 mol) of TFMB was added to obtain a polyimide varnish having a solid content concentration of 15% by mass.

[0178] A film was obtained by the same method as in Example 1 using the obtained polyimide varnish.

[0179] <Example 4>

[0180] A polyimide varnish was prepared in the same manner as in Example 1 except that the amount of 6FODA was changed from 33.624 g (0.100 mol) to 6.725 g (0.020 mol) and 25.619 g (0.080 mol) of TFMB was added to obtain a polyimide varnish having a solid content concentration of 15% by mass.

[0181] A film was obtained by the same method as in Example 1 using the obtained polyimide varnish.

[0182] <Example 5>

[0183] A polyimide varnish was prepared in the same manner as in Example 1 except that the amount of 6FODA was changed from 33.624 g (0.100 mol) to 16.812 g (0.050 mol) and 16.012 g (0.050 mol) of TFMB was additionally added to obtain a polyimide varnish having a solid content concentration of 15% by mass.

[0184] A film was obtained by the same method as in Example 1 using the obtained polyimide varnish.

[0185] <Example 6>

[0186] The amount of 6FODA was changed from 33.624 g (0.100 mol) to 20.174 g (0.060 mol), 13.938 g (0.040 mol) of BAFL was added, the amount of CpODA was changed from 38.438 g (0.100 mol) to 23.063 g (0.060 mol), and 11.769 g (0.040 mol) of s-BPDA was added. In addition, a polyimide varnish was prepared by the same method as in Example 1 to obtain a polyimide varnish having a solid content concentration of 15% by mass.

[0187] A film was obtained by the same method as in Example 1 using the obtained polyimide varnish.

[0188] <Example 7>

[0189] The amount of 6FODA was changed from 33.624 g (0.100 mol) to 18.493 g (0.055 mol), 15.680 g (0.045 mol) of BAFL was added, the amount of CpODA was changed from 38.438 g (0.100 mol) to 34.594 g (0.090 mol), and 4.584 g (0.010 mol) of BPAF was added. A polyimide varnish was prepared in the same manner as in Example 1 to obtain a polyimide varnish having a solid content concentration of 15% by mass.

[0190] A film was obtained by the same method as in Example 1 using the obtained polyimide varnish.

[0191] <Comparative Example 1>

[0192] In a 500 mL five-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet tube, a Dean-Stark trap equipped with a condenser, a thermometer, and a glass end cap, 32.024 g (0.100 mol) of TFMB and 84.554 g of GBL were added, and the mixture was stirred at a temperature of 70° C. in a nitrogen atmosphere at a rotation speed of 200 rpm to obtain a solution.

[0193] To this solution, 38.438 g (0.100 mol) of CpODA and 21.139 g of GBL were added simultaneously, and then 0.506 g of TEA and 0.056 g of TEDA were added as imidization catalysts, and the mixture was heated in a hooded heater to raise the temperature in the reaction system to 190° C. over about 20 minutes. The components removed by distillation were collected, and the rotation speed was adjusted according to the increase in viscosity, and the temperature in the reaction system was maintained at 190° C., and reflux was performed for about 5 hours.

[0194] Then, 273.169 g of GBL was added to a solid content concentration of 15% by mass, and the temperature in the reaction system was cooled to 100° C., and then stirred for about 1 hour for homogenization to obtain a turbid (foggy) polyimide varnish. After 24 hours, the varnish gelled and lost its fluidity, making it difficult to form a film, and no thin film was obtained.

[0195] <Comparative Example 2>

[0196] In a 500 mL five-necked round-bottom flask equipped with a stainless steel half-moon-shaped stirring blade, a nitrogen inlet tube, a Dean-Stark trap equipped with a condenser, a thermometer, and a glass end cap, 33.624 g (0.100 mol) of 6FODA and 201.747 g of NMP were added, and the mixture was stirred at a temperature of 50° C. in a nitrogen atmosphere at a rotation speed of 200 rpm to obtain a solution.

[0197] To this solution, 29.422 g (0.100 mol) of s-BPDA and 50.437 g of NMP were simultaneously added, and the mixture was stirred for 5 hours while being maintained at 50° C. in a mantle heater.

[0198] Thereafter, 105.077 g of NMP was added and homogenized, and then the temperature was returned to room temperature to obtain a polyamic acid varnish having a solid content concentration of 15% by mass.

[0199] Then, the obtained polyamic acid varnish is applied on a glass plate by spin coating, maintained at 80°C for 20 minutes on a hot plate, and then heated at 400°C for 30 minutes (heating rate 5°C / min) in a hot air dryer under a nitrogen atmosphere to evaporate the solvent, and further thermal imidization is carried out to obtain a polyimide film.

[0200] <Comparative Example 3>

[0201] A polyamic acid varnish was prepared in the same manner as in Comparative Example 2 except that 38.438 g (0.100 mol) of CpODA was changed to 45.833 g (0.100 mol) of TAHQ to obtain a polyamic acid varnish having a solid content concentration of 15% by mass.

[0202] A polyimide film was obtained by the same method as in Comparative Example 2 using the obtained polyamic acid varnish.

[0203] [Table 1]

[0204] Table 1

[0205]

[0206] As shown in Table 1, it can be seen that the polyimide films of Examples have good heat resistance and elongation, and are also excellent in colorless transparency.

Claims

1. A polyimide resin comprising: a structural unit A derived from tetracarboxylic dianhydride and a structural unit B derived from diamine, The structural unit A comprises: a structural unit (A1) derived from a compound represented by the following formula (a1), The structural unit B comprises: a structural unit (B1) derived from a compound represented by the following formula (b1), The content ratio of the structural unit (A1) in the structural unit A is 55 mol% or more, The content ratio of the structural unit (B1) in the structural unit B is 10 mol% or more.

2. The polyimide resin according to claim 1, wherein The structural unit A further includes a structural unit (A2), wherein the structural unit (A2) is at least one selected from the group consisting of a structural unit (A21) derived from a compound represented by the following formula (a21), a structural unit (A22) derived from a compound represented by the following formula (a22), and a structural unit (A23) derived from a compound represented by the following formula (a23), 3. The polyimide resin according to claim 1 or 2, wherein The structural unit B further includes a structural unit (B2), wherein the structural unit (B2) is at least one selected from the group consisting of a structural unit (B21) derived from a compound represented by the following formula (b21) and a structural unit (B22) derived from a compound represented by the following formula (b22).

4. The polyimide resin according to claim 1 or 2, wherein The structural unit B further includes a structural unit (B2), and the structural unit (B2) includes: a structural unit (B22) derived from a compound represented by the following formula (b22), 5. The polyimide resin according to claim 1 or 2, wherein The structural unit A further includes a structural unit (A2), and the structural unit (A2) includes: a structural unit (A22) derived from a compound represented by the following formula (a22), 6 . A polyimide varnish, comprising the polyimide resin according to claim 1 dissolved in an organic solvent. 7 . A polyimide film comprising the polyimide resin according to claim 1 .

8. A method for producing a polyimide film, wherein: After the polyimide varnish according to claim 6 is applied or formed into a film, the organic solvent is removed.

Citation Information

Patent Citations

  • Method for producing resin thin film, and composition for forming resin thin film

    CN106164178A

  • Polyimide resin, polyimide varnish, and polyimide film

    CN114729122A