A device and method for accelerating corrosion fatigue test and life evaluation of high-strength steel wire

By exposing the corrosion solution in the local micro area of ​​the high-strength steel wire surface and applying electrochemical three-electrode system to accelerate corrosion and reciprocating loads, the problem that the corrosion fatigue life of high-strength steel wire cannot be accurately obtained in the prior art is solved, and the complete corrosion fatigue damage is achieved Process research and life prediction provide a reliable life evaluation method for bridge cables.

CN115046916BActive Publication Date: 2024-11-15UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202210330973.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-29
Publication Date
2024-11-15
Estimated Expiration
2042-03-29

AI Technical Summary

Technical Problem

The existing high-strength steel wire corrosion fatigue life test methods cannot truly reflect the fatigue life under the coupling effect of corrosion fatigue, and have limitations, so the corrosion fatigue life and performance evaluation of high-strength steel wire cannot be accurately obtained.

Method used

By exposing local tiny areas of the steel wire surface to corrosion solution and applying electrochemical three-electrode system to accelerate corrosion, and applying reciprocating loads at both ends of the steel wire, the influence of different factors on corrosion fatigue damage is studied, and accelerated corrosion fatigue tests and real service status are established. The corresponding relationship between the two factors is determined, the control parameters are determined, and the probability distribution of corrosion fatigue life is established through repeated experiments.

Benefits of technology

The whole process of corrosion fatigue damage of high-strength steel wire was studied, the main control factors of the coupling effect of corrosion and fatigue were determined, and the reliability evaluation and prediction of the fatigue life of cable corrosion was provided, and the durability evaluation was provided for bridge pulling slings. Base.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115046916B_ABST
    Figure CN115046916B_ABST
Patent Text Reader

Abstract

The present invention provides a device and method for accelerating corrosion fatigue test and life evaluation of high-strength steel wire, belonging to the technical field of metal corrosion fatigue test. The device includes an accelerated corrosion system and a fatigue loading system, the fatigue loading system includes a fatigue testing machine, an upper clamp and a lower clamp, the accelerated corrosion system is placed between the upper clamp and the lower clamp of the fatigue loading system, the accelerated corrosion system is connected to an electrochemical workstation, and the electrochemical workstation and the fatigue loading system are controlled by an industrial control computer. The device constructs a local micro-exposed area on the surface of the high-strength steel wire as a working electrode, and at the same time applies fatigue loads at both ends of the steel wire to realize accelerated corrosion fatigue of the steel wire. According to the actual service environment and load conditions of the steel wire, the corrosion rate, fatigue stress amplitude and fatigue load frequency of the steel wire are controlled by similar principles, and a mapping relationship with the actual service conditions of the sling is established. Through repeated tests, a probability distribution model is established, and the reliability or failure probability of corrosion fatigue of the high-strength steel wire is determined according to a given service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal corrosion fatigue testing, and in particular to a device and method for accelerating corrosion fatigue testing and life evaluation of a high-strength steel wire. Background Art

[0002] The evaluation of corrosion fatigue performance of high-strength steel wire in the cable system of large-span bridges is the basis for predicting the service life of cable system stay cables. Compared with the main cables of suspension bridges, the live load fluctuation of cable-stayed bridges, suspension bridges and arch bridge hangers is larger, and corrosion is inevitable during service. Therefore, the risk of corrosion fatigue of stay cables is significantly increased. The steel wires used for stay cables are mostly 5mm or 7mm diameter pearlite high-strength steel wires, which are made by multiple cold drawing. They have strong resistance to crack initiation and poor resistance to crack propagation. Once corrosion occurs, it causes significant stress concentration under load. At this time, the ability of high-strength steel wire to resist crack initiation is significantly reduced, greatly shortening the fatigue life of high-strength steel wire. In particular, stress will increase the corrosion rate of steel wire in the natural state and accelerate crack nucleation. After crack nucleation, corrosion will further accelerate the crack propagation rate. In the natural state, the corrosion development process of steel wire in the service process is relatively slow. The design service life of stay cables exceeds 20 years. It is difficult to evaluate the corrosion fatigue performance of high-strength steel wire by in-situ corrosion test. The laboratory mainly accelerates the corrosion of high-strength steel wire, and conducts fatigue tests on high-strength steel wires with different corrosion degrees after accelerated corrosion to study the remaining fatigue life after corrosion. This cannot truly reflect the fatigue life of high-strength steel wire under the coupling effect of corrosion fatigue; there are also methods to pre-crack the steel wire, immerse it in a corrosive solution, and study the corrosion fatigue crack growth rate of the steel wire under different solutions and different fatigue frequencies by applying stress amplitudes. This method can only obtain the corrosion fatigue coupling crack growth rate under different solution conditions, different stress amplitudes, and different loading frequencies. Compared with the corrosion fatigue crack growth life, the corrosion fatigue crack initiation life of high-strength steel wire accounts for a higher proportion of the total life, and once the crack initiates, the corrosion fatigue crack expands. The life span accounts for a small proportion, and it is impossible to fully obtain the life prediction of the steel wire under the coupling of corrosion and fatigue. In addition, electrochemical accelerated corrosion and coupled fatigue load can be used to study the corrosion fatigue life of the steel wire. The steel wire is exposed to the solution and a three-electrode system is used for accelerated corrosion (constant potential accelerated corrosion, constant current accelerated corrosion). However, during the electrochemical accelerated corrosion process, the surface of the steel wire exposed to the solution dissolves to form a state similar to uniform corrosion. The cross-section of the steel wire surface in the solution is uniformly reduced, and steel wire damage is prone to occur at the solution interface. Because the cross-section of the steel wire at the solution interface is uniformly reduced, there is a significant stress concentration there, which cannot truly reflect the fatigue life of the steel wire under the coupling of local corrosion and fatigue.

[0003] As can be seen from the above, the existing corrosion fatigue life test methods for high-strength steel wires cannot truly obtain their corrosion fatigue life, and all have certain limitations. The fatigue life obtained by the fatigue test after accelerated corrosion ignores the effect of stress amplitude in the accelerated corrosion process. The stress amplitude effect will increase the accelerated corrosion rate, and the fatigue process after corrosion cannot consider the contribution of the coupling effect of corrosion rate and stress amplitude to crack initiation. The obtained corrosion fatigue life will be used to evaluate the service performance of the sling. The method of exposing the steel wire with prefabricated cracks to the corrosive solution can obtain the effect of corrosion fatigue coupling on the crack growth rate, but it is impossible to obtain the results of the entire process of corrosion fatigue coupling, and it is impossible to evaluate the corrosion fatigue life of the steel wire. The test method of directly exposing the steel wire to the solution using electrochemical accelerated corrosion and fatigue coupling cannot accurately obtain the corrosion fatigue life of the steel wire. The cross-section of the steel wire exposed to the solution is uniformly reduced, which significantly increases the real stress amplitude of the steel wire within the solution exposure range, and a large stress concentration is formed at the solution interface. The fatigue fracture of the steel wire occurs at the solution interface, which is inconsistent with the actual situation. It can be seen that the existing high-strength steel wire corrosion fatigue coupled accelerated test methods have certain limitations. They cannot accurately obtain the corrosion fatigue life of high-strength steel wire, and cannot perform reliability evaluation of the corrosion fatigue performance and service life of high-strength steel wire based on experimental data, and cannot provide support for the corrosion fatigue evaluation of slings. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a high-strength steel wire corrosion fatigue accelerated test and life evaluation device and method to solve the problem that the corrosion fatigue process of high-strength steel wire is slow in situ or in natural state, and rapid evaluation of corrosion fatigue performance cannot be achieved.

[0005] The present invention exposes a local micro area on the surface of the steel wire to a corrosive solution, realizes accelerated corrosion of the local micro area on the surface of the steel wire through an electrochemical three-electrode system, and simultaneously applies a reciprocating load at both ends of the steel wire to realize the coupling effect of corrosion and fatigue. By applying a given corrosion potential or corrosion current, fatigue stress amplitude and loading frequency, the influence of different factors on the corrosion fatigue damage of the high-strength steel wire of the cable is studied, the occurrence, development and evolution of the corrosion fatigue damage of the high-strength steel wire are revealed, the interaction mechanism of corrosion and fatigue at each stage of the corrosion fatigue fracture process of the high-strength steel wire is explored, and the main control factors of the corrosion fatigue damage of the high-strength steel wire are determined; The similarity principle is further used to establish the correspondence between the accelerated corrosion fatigue test and the actual service status according to the actual corrosion rate, design fatigue stress amplitude and fatigue load frequency of the bridge cable steel wire, and the values ​​of each control parameter in the accelerated corrosion fatigue test are determined. Then, the similarity principle is used to determine the life of the steel wire in the pull cable under the actual service conditions based on the corrosion fatigue life of the steel wire obtained from the accelerated corrosion fatigue test. Through a certain number of repeated tests, the probability distribution of the corrosion fatigue life of the steel wire under the actual service environment is established, and the fatigue reliability of the cable under the actual service status is studied, providing a basis for the prediction of the corrosion fatigue life of the cable and the durability evaluation.

[0006] The device of the present invention comprises an accelerated corrosion system and a fatigue loading system. The fatigue loading system comprises a fatigue testing machine, an upper fixture and a lower fixture. The accelerated corrosion system is placed between the upper fixture and the lower fixture of the fatigue loading system. The accelerated corrosion system is connected to an electrochemical workstation. The electrochemical workstation and the fatigue loading system are controlled by an industrial computer.

[0007] Among them, the accelerated corrosion system adopts a three-electrode electrochemical system, including a corrosion solution pool, a counter electrode, a reference electrode and a working electrode.

[0008] Three holes are opened on the upper part of the corrosion solution pool, and the counter electrode, working electrode and reference electrode are installed respectively, and the three openings are sealed by rubber plugs, and the counter electrode, working electrode and reference electrode are connected to the electrochemical workstation through wires respectively;

[0009] A hole is opened at the bottom of the corrosion solution pool for the steel wire sample to pass through, and the opening is sealed by a rubber plug.

[0010] The working electrode is a local tiny area on the surface of the exposed steel wire sample, that is, the exposed area, and the other parts of the surface of the steel wire sample in the corrosion solution pool are covered with sealing silicone; the steel wire sample passes through the corrosion solution pool, the upper end of the steel wire sample is fixed on the upper clamp, and the lower end is fixed on the lower clamp, and the corrosion solution pool is fixed on the steel wire sample through a rubber stopper.

[0011] The corrosion solution tank is filled with NaCl solution.

[0012] The counter electrode was a platinum electrode and the reference electrode was a saturated calomel electrode.

[0013] The exposed area is the surface with a diameter less than 1mm along the length of the wire, and the exposed area is less than 0.79mm 2 .

[0014] The application method of the device comprises the following steps:

[0015] S1: Take the high-strength steel wire to be tested as the steel wire sample, and apply sealing silicone to the middle part of the steel wire sample. When applying silicone, leave a small exposed area;

[0016] S2: The steel wire sample coated with sealing silicone in S1 is passed through the corrosion solution pool, and the steel wire sample is sealed and fixed with a rubber plug between the steel wire sample and the corrosion solution pool;

[0017] S3: injecting the corrosion solution into the corrosion solution pool, installing the counter electrode and the reference electrode, and connecting the counter electrode, the reference electrode and the working electrode to the electrochemical workstation through wires;

[0018] S4: The corrosion potential is controlled by the industrial computer, and the corrosion current is collected synchronously when the electrochemical workstation is performing accelerated corrosion, which is used to calculate the total amount of iron ions dissolved in a small local area on the surface of the working electrode steel wire. The pit depth and corrosion rate are determined based on the total amount of dissolved iron ions and the area of ​​the exposed area.

[0019] S5: The working electrode is controlled to be at a certain corrosion potential or corrosion current through the electrochemical workstation, and the fatigue stress amplitude and loading frequency applied to the steel wire sample by the fatigue testing machine are synchronously controlled until the local micro-area of ​​the surface of the steel wire sample exposed in the solution breaks. The corrosion fatigue life under this accelerated corrosion condition is determined according to the number of fatigue cycles or the total duration at the time of breaking; the total number of fatigue cycles is the corrosion fatigue life, because at this time the corrosion fatigue is coupled together, and similarly the total duration can also be converted into the corresponding number of cycles through the fatigue load loading frequency;

[0020] S6: Determine the corrosion fatigue life of the steel wire under different accelerated corrosion fatigue conditions by changing the corrosion potential of the working electrode, the fatigue stress amplitude and loading frequency of the steel wire sample, and determine the influence of corrosion potential, fatigue stress amplitude and loading frequency on the corrosion fatigue damage of the steel wire.

[0021] As mentioned above, the etch pit in S4 is the intersection of the sphere and the steel wire cylinder, wherein the sphere is formed with the exposed area as the interface.

[0022] The determination process of corrosion potential or corrosion current as well as fatigue stress amplitude and loading frequency in S5 is as follows:

[0023] According to the actual service environment conditions of specific large-span bridges, the annual corrosion rate of the steel wire in the cable, the design fatigue stress amplitude of the cable and the number of cycles per year are determined. The corrosion rate and the number of fatigue cycles per unit time of the accelerated corrosion fatigue test are determined using a similar principle. The accelerated corrosion potential and fatigue loading frequency corresponding to the accelerated corrosion fatigue test are determined. The stress amplitude of the accelerated corrosion fatigue test is taken as the design fatigue stress amplitude of the cable.

[0024] After the corrosion fatigue life of the steel wire is obtained in S6, the life of the steel wire in the sling under the corresponding actual service conditions is determined according to the similarity principle. Specifically, by obtaining the steel wire corrosion fatigue life sample through repeated tests, a probability distribution model of the steel wire corrosion fatigue life is established, and the cumulative distribution function of the steel wire corrosion fatigue life is used to determine the reliability or failure probability of the high-strength steel wire corrosion fatigue at a given service life.

[0025] The beneficial effects of the above technical solution of the present invention are as follows:

[0026] In the above scheme, the accelerated corrosion fatigue test and life evaluation of high-strength steel wire of bridge cables can be realized. By setting different corrosion potentials or corrosion currents, fatigue stress amplitudes, loading frequencies and other parameter values, the whole process of corrosion fatigue damage evolution of high-strength steel wire under different conditions can be obtained, and the influence law of different influencing factors on the corrosion fatigue life of high-strength steel wire can be determined. Further, according to the corrosion rate of the cable steel wire in the actual service environment and the relevant fatigue load design conditions, the values ​​of the control parameters in the accelerated corrosion fatigue test are designed by the similarity principle to determine the corrosion fatigue life of the high-strength steel wire under the accelerated corrosion fatigue conditions. The service life of the high-strength steel wire under the actual service conditions is determined by the similarity ratio, and the probability distribution of the corrosion fatigue life of the high-strength steel wire is established through a certain number of repeated test data to obtain the corrosion fatigue life of the high-strength steel wire under the condition of probability guarantee rate, and the corrosion fatigue reliability of the high-strength steel wire under the actual service conditions for a specified service life can be further determined, providing an accelerated corrosion fatigue test and life evaluation method for bridge suspension cables. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of the structure of the high-strength steel wire corrosion fatigue acceleration test and life evaluation device of the present invention;

[0028] Figure 2 A schematic diagram of a corrosion system of a high-strength steel wire corrosion fatigue accelerated test and life evaluation device of the present invention;

[0029] Figure 3 A cross-sectional view of the corrosion system of the device for accelerating corrosion fatigue testing and life evaluation of high-strength steel wire of the present invention;

[0030] Figure 4The probability density function of the two-parameter Weibull distribution is obtained by repeating the high-strength steel wire corrosion fatigue accelerated test 15 times in the embodiment of the present invention and estimating the service life under the corresponding actual service conditions;

[0031] Figure 5 The cumulative distribution function of the two-parameter Weibull distribution is obtained by repeating the high-strength steel wire corrosion fatigue accelerated test 15 times in the embodiment of the present invention and estimating the life under the corresponding actual service conditions.

[0032] Among them: 1- steel wire sample; 2- fatigue testing machine; 3- upper fixture; 4- lower fixture; 5- corrosion solution pool; 6- rubber plug; 7- counter electrode; 8- reference electrode; 9- working electrode; 10- sealing silica gel; 11- 3.5% NaCl solution; 12- conductor; 13- electrochemical workstation; 14- industrial computer. DETAILED DESCRIPTION

[0033] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0034] The invention provides a device and method for accelerating corrosion fatigue testing and life evaluation of a high-strength steel wire.

[0035] like Figure 1 , Figure 2 and Figure 3 As shown, the device includes an accelerated corrosion system and a fatigue loading system. The fatigue loading system includes a fatigue testing machine 2, an upper clamp 3 and a lower clamp 4. The accelerated corrosion system is placed between the upper clamp 3 and the lower clamp 4 of the fatigue loading system. The accelerated corrosion system is connected to an electrochemical workstation 13. The electrochemical workstation 13 and the fatigue loading system are controlled by an industrial computer 14.

[0036] The accelerated corrosion system adopts a three-electrode electrochemical system, including a corrosion solution pool 5, a counter electrode 7, a reference electrode 8 and a working electrode 9.

[0037] Three holes are opened on the upper part of the corrosion solution pool 5, and the counter electrode 7, the working electrode 9 and the reference electrode 8 are installed respectively, and the three openings are sealed by rubber plugs 6, and the counter electrode 7, the working electrode 9 and the reference electrode 8 are connected to the electrochemical workstation 13 through wires 12 respectively;

[0038] A hole is opened at the bottom of the corrosion solution pool 5 for the steel wire sample 1 to pass through, and the opening is sealed by a rubber plug.

[0039] The working electrode 9 is a local tiny area on the surface of the exposed steel wire sample 1, and the other parts of the surface of the steel wire sample 1 in the corrosion solution pool 5 are covered with sealing silicone 10; the steel wire sample 1 passes through the corrosion solution pool 5, the upper end of the steel wire sample 1 is fixed on the upper clamp 3, and the lower end is fixed on the lower clamp 4, and the corrosion solution pool 5 is fixed on the steel wire sample 1 through a rubber stopper.

[0040] The corrosion solution pool 5 contains NaCl solution.

[0041] The counter electrode 7 is a metal platinum electrode, and the reference electrode 8 is a saturated calomel electrode.

[0042] The application method of the device comprises the following steps:

[0043] S1: Take the high-strength steel wire to be tested as the steel wire sample 1, and apply sealing silicone 10 on the middle part of the steel wire sample. When applying the silicone, reserve a small exposed area;

[0044] S2: The steel wire sample coated with sealing silicone in S1 is passed through the corrosion solution pool 5, and the steel wire sample is sealed and fixed to the corrosion solution pool 5 by a rubber stopper 6;

[0045] S3: injecting the corrosion solution into the corrosion solution pool 5, installing the counter electrode 7 and the reference electrode 8, and connecting the counter electrode 7, the reference electrode 8 and the working electrode 9 to the electrochemical workstation 13 through the wire 12;

[0046] S4: The corrosion potential is controlled by the industrial computer 14, and the corrosion current is synchronously collected when the electrochemical workstation 13 performs accelerated corrosion, which is used to calculate the total amount of iron ions dissolved in a local micro-area on the surface of the steel wire of the working electrode 9, and the pit depth and corrosion rate are determined according to the total amount of dissolved iron ions and the area of ​​the exposed area;

[0047] S5: Control the working electrode 9 to be at a certain corrosion potential or corrosion current through the electrochemical workstation 13, and synchronously control the fatigue stress amplitude and loading frequency applied by the fatigue testing machine 2 to the steel wire sample 1, until a local micro-area of ​​the surface of the steel wire sample 1 exposed in the solution breaks, and determine the corrosion fatigue life under this accelerated corrosion condition according to the number of fatigue cycles or the total duration at the time of breaking;

[0048] S6: Determine the corrosion fatigue life of the steel wire under different accelerated corrosion fatigue conditions by changing the corrosion potential of the working electrode 9, the fatigue stress amplitude and loading frequency of the steel wire sample 1, and determine the influence of the corrosion potential, fatigue stress amplitude and loading frequency on the corrosion fatigue damage of the steel wire.

[0049] The fatigue loading system in the present invention applies fatigue load along the axial direction of the steel wire by clamping both ends of the steel wire. The corrosion fatigue accelerated test of high-strength steel wire under different working conditions is realized by controlling the constant potential or constant current, fatigue stress amplitude and fatigue loading frequency. The corrosion fatigue damage evolution process of high-strength steel wire under different conditions is determined according to different control parameter values, and the corrosion fatigue life of high-strength steel wire under different conditions is obtained. According to the corrosion rate of high-strength steel wire under the actual service environment of the cable, the design stress amplitude of the cable and the fatigue load frequency, the accelerated corrosion fatigue test parameters are determined by similarity principle to obtain the accelerated corrosion fatigue life of high-strength steel wire, and then the service life of high-strength steel wire under actual service conditions is determined according to the similarity ratio. The probability distribution model is established through the life data of a certain number of steel wire samples to obtain the corrosion fatigue life of high-strength steel wire with a specified probability guarantee rate, and then the corrosion fatigue reliability of high-strength steel wire under actual service conditions is evaluated.

[0050] In the specific test, the following steps are performed:

[0051] A 1770MPa grade high-strength steel wire with a diameter of 5mm and a length of 500mm to be tested is taken as a steel wire sample 1, and a sealing silicone gel 10 is coated on the middle part of the steel wire sample. When coating the silicone gel, a disc with a diameter of 1mm is pre-attached to the surface of the steel wire sample, and then the silicone gel is coated. After the coating is completed, the disc is removed to form an exposed area; the steel wire sample coated with the sealing silicone gel passes through a corrosion solution pool 5, and is sealed and fixed to the corrosion solution pool 5 by a rubber plug 6; a 3.5% NaCl solution 11 is injected into the corrosion solution pool 5, and a counter electrode 7 and a reference electrode 8 are installed, and the counter electrode 7, the reference electrode 8 and the working electrode 9 are connected to an electrochemical workstation 13 through a wire 12; the corrosion potential is controlled by an industrial computer 14, and the corrosion current is synchronously collected when the electrochemical workstation 13 performs accelerated corrosion, which is used to calculate the local surface of the steel wire of the working electrode 9. The total amount of iron ions dissolved in a tiny area, the corrosion pit formed by the dissolution of iron ions on the surface of the steel wire of the working electrode 9 is the intersection of a sphere and a steel wire cylinder, and the depth of the corrosion pit and the corrosion rate are determined according to the total amount of iron ions dissolved at any time; the working electrode 9 is controlled to be at a certain corrosion potential or corrosion current by the electrochemical workstation 13, and the stress amplitude and loading frequency applied to the steel wire sample 1 by the fatigue testing machine 2 are synchronously controlled until a local tiny area on the surface of the steel wire sample 1 exposed in the solution breaks, and the corrosion fatigue life under this accelerated corrosion condition is determined according to the number of fatigue cycles or the total duration at the time of breaking; the corrosion fatigue life of the steel wire under different accelerated corrosion fatigue conditions is determined by changing the corrosion potential of the working electrode 9, the fatigue stress amplitude and the loading frequency of the steel wire sample 1, and the influence of the corrosion potential, fatigue stress amplitude and loading frequency on the corrosion fatigue damage of the steel wire is determined.

[0052] Scanning electron microscopy observation of the fatigue fracture of steel wire sample 1 was used to determine the occurrence, development and evolution of corrosion fatigue damage of high-strength steel wire under different accelerated corrosion fatigue conditions. The interaction mechanism and respective contribution of corrosion and fatigue at each stage of the steel wire corrosion fatigue fracture process were determined according to different accelerated corrosion fatigue test conditions.

[0053] According to the actual service environment conditions of the specific large-span bridge, the annual corrosion rate of the steel wire in the cable, the designed fatigue stress amplitude and the annual cycle number of the cable are determined. The corrosion rate and fatigue cycle number per unit time of the corresponding accelerated corrosion fatigue test are determined by the similarity principle, and the accelerated corrosion potential and fatigue loading frequency corresponding to the accelerated corrosion fatigue test are determined. The stress amplitude of the accelerated corrosion fatigue test can be taken as the designed fatigue stress amplitude of the cable. The accelerated corrosion fatigue life of the high-strength steel wire is obtained through the accelerated corrosion fatigue test. The accelerated corrosion fatigue test is repeated to obtain a certain number of accelerated corrosion fatigue lives of the steel wire, and then the life under the corresponding actual service conditions is determined according to the similarity principle.

[0054] If the measured surface corrosion rate of 5mm diameter 1770MPa grade high-strength steel wire in the cable of a large-span cable-stayed bridge is 0.02mm / year, the design fatigue stress amplitude of the cable is 200MPa, and it cycles 20,000 times per year, the similarity principle is used to compress the one-year corrosion fatigue condition to a unit time (1 hour) to complete, and the stress amplitude remains unchanged. The constant potential value is determined according to the corrosion rate, and the unit loading number, i.e., the loading frequency, is determined according to the annual number of cycles. The total number of cycles when the steel wire is damaged by corrosion fatigue is obtained using the accelerated corrosion test conditions, and then the corresponding actual service life (total number of cycles / number of cycles per year) is inferred based on the similarity principle. In theory, the corrosion fatigue life of high-strength steel wire is a random variable, and the corrosion fatigue life of steel wire obeys the standard two-parameter Weibull distribution. The maximum likelihood estimation is used to obtain the shape parameters and characteristic parameters of the standard two-parameter Weibull distribution, such as Figure 4 and Figure 5 As shown in the figure, the life estimation under the actual service conditions obtained by repeating the high-strength steel wire corrosion fatigue accelerated test 15 times is the probability density function of the two-parameter Weibull distribution ( Figure 4 ) and the cumulative distribution function ( Figure 5 ), the failure probability of corrosion fatigue damage of high-strength steel wire under actual service conditions at any specified service life can be determined. At the same time, the corrosion fatigue life of high-strength steel wire in the cable under the service environment conditions can also be determined according to the acceptable failure probability, providing a theoretical basis for cable corrosion fatigue life prediction, durability evaluation and replacement of cable. When the acceptable failure probability is 2.3%, Figure 5 As shown by the dotted line, the corrosion fatigue service life of the high-strength steel wire is 20.56 years.

[0055] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A high-strength steel wire corrosion fatigue accelerated test and life evaluation method, characterized in that: The steps include: S1: Take the high-strength steel wire to be tested as the steel wire sample, and apply sealing silicone to the middle part of the steel wire sample. When applying silicone, leave a small exposed area; S2: The steel wire sample coated with sealing silicone in S1 is passed through the corrosion solution pool, and the steel wire sample is sealed and fixed with a rubber plug between the steel wire sample and the corrosion solution pool; S3: injecting the corrosion solution into the corrosion solution pool, installing the counter electrode and the reference electrode, and connecting the counter electrode, the reference electrode and the working electrode to the electrochemical workstation through wires; S4: The corrosion potential is controlled by the industrial computer, and the corrosion current is collected synchronously when the electrochemical workstation is performing accelerated corrosion, which is used to calculate the total amount of iron ions dissolved in a small local area on the surface of the working electrode steel wire. The pit depth and corrosion rate are determined based on the total amount of dissolved iron ions and the area of ​​the exposed area. S5: Control the working electrode to a certain corrosion potential or corrosion current through the electrochemical workstation, and synchronously control the fatigue stress amplitude and loading frequency applied to the steel wire sample by the fatigue testing machine until the local micro-area of ​​the surface of the steel wire sample exposed in the solution breaks, and determine the corrosion fatigue life under this accelerated corrosion condition according to the number of fatigue cycles or total duration at the time of breaking; S6: Determine the corrosion fatigue life of the steel wire under different accelerated corrosion fatigue conditions by changing the corrosion potential of the working electrode, the fatigue stress amplitude and loading frequency of the steel wire sample, and determine the influence of the corrosion potential, fatigue stress amplitude and loading frequency on the corrosion fatigue damage of the steel wire; After obtaining the corrosion fatigue life of the steel wire in S6, the corrosion fatigue life samples of the steel wire are obtained through repeated tests, and a probability distribution model of the corrosion fatigue life of the steel wire is established. The cumulative distribution function of the corrosion fatigue life of the steel wire is used to determine the reliability or failure probability of the corrosion fatigue of the high-strength steel wire at a given service life.

2. The high-strength steel wire corrosion fatigue accelerated test and life evaluation method according to claim 1, characterized in that: The etch pit in S4 is the intersection of a sphere and a steel wire cylinder, wherein the sphere is formed with the exposed area as the interface.

3. The high-strength steel wire corrosion fatigue accelerated test and life evaluation method according to claim 1, characterized in that: The process of determining the corrosion potential or corrosion current and the fatigue stress amplitude and the loading frequency in S5 is as follows: According to the actual service environment conditions of specific large-span bridges, the annual corrosion rate of the steel wire in the cable, the design fatigue stress amplitude of the cable and the number of cycles per year are determined. The corrosion rate and the number of fatigue cycles per unit time of the accelerated corrosion fatigue test are determined using a similar principle. The accelerated corrosion potential and fatigue loading frequency corresponding to the accelerated corrosion fatigue test are determined. The stress amplitude of the accelerated corrosion fatigue test is taken as the design fatigue stress amplitude of the cable.

4. A device for the high-strength steel wire corrosion fatigue accelerated test and life evaluation method according to claim 1, characterized in that: It includes an accelerated corrosion system and a fatigue loading system. The fatigue loading system includes a fatigue testing machine, an upper fixture and a lower fixture. The accelerated corrosion system is placed between the upper fixture and the lower fixture of the fatigue loading system. The accelerated corrosion system is connected to an electrochemical workstation. The electrochemical workstation and the fatigue loading system are controlled by an industrial computer.

5. The device according to claim 4, characterized in that The accelerated corrosion system adopts a three-electrode electrochemical system, including a corrosion solution pool, a counter electrode, a reference electrode and a working electrode. Three holes are opened on the upper part of the corrosion solution pool, and the counter electrode, working electrode and reference electrode are installed respectively, and the three openings are sealed by rubber plugs, and the counter electrode, working electrode and reference electrode are connected to the electrochemical workstation through wires respectively; A hole is opened at the bottom of the corrosion solution pool for the steel wire sample to pass through, and the opening is sealed by a rubber plug.

6. The device according to claim 5, characterized in that The working electrode is a local tiny area on the surface of the exposed steel wire sample, that is, the exposed area, and the other parts of the surface of the steel wire sample in the corrosion solution pool are covered with sealing silicone; the steel wire sample passes through the corrosion solution pool, the upper end of the steel wire sample is fixed on the upper clamp, and the lower end is fixed on the lower clamp, and the corrosion solution pool is fixed on the steel wire sample through a rubber stopper.

7. The device according to claim 5, characterized in that The corrosion solution pool contains NaCl solution.

8. The device according to claim 5, characterized in that The counter electrode is a metal platinum electrode, and the reference electrode is a saturated calomel electrode.

9. The device according to claim 6, characterized in that The exposed area has a diameter of less than 1 mm along the length of the steel wire and an area of ​​less than 0.79 mm 2 .

Citation Information

Cited By

  • Novel steel wire spiral contact device suitable for steel wire bending friction fatigue machine

    CN116202893A

  • A wire spiral contact device suitable for a wire bending friction fatigue machine

    CN116202893B