Heterojunction solar cell and method for preparing the same

By forming staggered doped regions on the back and using alkaline etching, the preparation process of heterojunction solar cells is simplified, solving the problems of traditional process complexity and pollution risks, and achieving a more efficient production process.

CN115050856BActive Publication Date: 2024-10-25SUZHOU MAXWELL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210719108.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-23
Publication Date
2024-10-25
Estimated Expiration
2042-06-23

AI Technical Summary

Technical Problem

The preparation process of traditional back-contact heterojunction solar cells is complex and requires multiple patterning processes and cleaning steps, resulting in high process difficulty and high cost, which limits its industrial application.

Method used

By forming staggered first and second doped regions on the back side of the semiconductor substrate, oxygen-doped microcrystalline silicon and amorphous or microcrystalline silicon doped layers are formed respectively, and unnecessary masks are removed by alkaline etching. layer, simplifying the process and reducing the use of intermediate isolation layers, thereby reducing the risk of contamination.

Benefits of technology

The preparation process is simplified, the risk of contamination is reduced, the production efficiency is improved, additional isolation layer processing steps are avoided, more controllable doping layer etching is achieved, and costs are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115050856B_ABST
    Figure CN115050856B_ABST
Patent Text Reader

Abstract

The present application discloses a heterojunction solar cell and a preparation method thereof, belonging to the technical field of solar cells. A preparation method of a heterojunction solar cell, the method comprising: patterning on the back side of a semiconductor substrate to form a first doped region and a second doped region, the first doped region is formed with a first intrinsic i layer and an n-type doped layer, the n-type doped layer is an oxygen-doped microcrystalline silicon layer doped with a Group VA element; forming a second intrinsic i layer and a p-type doped layer, the p-type doped layer is an amorphous or microcrystalline silicon layer doped with a Group IIIA element; forming a patterned mask layer on the second intrinsic i layer and the p-type doped layer, exposing the second intrinsic i layer and the p-type doped layer on the first doped region, removing the exposed second intrinsic i layer and the p-type doped layer and retaining the first intrinsic i layer and the n-type doped layer. The present invention can simplify the preparation process, reduce the risk of contamination caused by the isolation layer entering the cavity, and reduce the cumbersome steps of adding or removing the isolation layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of solar cells, and specifically relates to a heterojunction solar cell and a preparation method thereof. Background Art

[0002] As a new type of solar cell, heterojunction solar cells have become a new hot spot in the photovoltaic field in recent years. They have many advantages such as simple structure, wide source of raw materials, high open circuit voltage, high conversion efficiency, and low temperature coefficient. Since there is no main grid line on the front of the back-contact solar cell, and even no electrode pattern, the positive and negative electrodes are located on the back of the cell, which reduces the shading of the cell, thereby effectively increasing the short-circuit current of the cell and improving the energy conversion efficiency of the cell. The back-contact heterojunction (HBC) cell is a crystalline silicon solar cell with relatively high photoelectric conversion efficiency. The back-contact heterojunction cell is a combination of heterojunction (HJT) technology and back contact (IBC) technology, and has many advantages of both cell structures. As the ultimate structure of high-efficiency single-crystal silicon cells, the back-contact heterojunction cell has occupied the throne of the highest conversion efficiency record of crystalline silicon cells in recent years.

[0003] The realization of the back-side interdigital structure of the traditional back-contact heterojunction solar cell requires at least three patterning processes and multiple cleaning steps. Multiple high-precision patterning processes and multiple cleaning steps greatly increase the difficulty and cost of the preparation process of the back-contact heterojunction cell. The factors such as the cumbersome preparation process and the complex process restrict the industrial application progress of the back-contact heterojunction cell. Therefore, there is still a need for improvement in the existing preparation method of the back-contact heterojunction solar cell. Summary of the invention

[0004] In view of the above problems, the present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the present invention provides a heterojunction solar cell and a method for preparing the same, which can simplify the preparation process, reduce the risk of contamination caused by the isolation layer (ink or dry film) entering the cavity, reduce the cumbersome steps of adding or removing the isolation layer, and overcome the shortcomings of the prior art.

[0005] In order to solve the above technical problems, this application is implemented as follows:

[0006] According to one aspect of the present application, a method for preparing a heterojunction solar cell is provided, the method comprising:

[0007] Patterning the back side of the semiconductor substrate to form a staggered first doped region and a second doped region, wherein the first doped region is formed with a first intrinsic i layer and an n-type doped layer, wherein the n-type doped layer is an oxygen-doped microcrystalline silicon layer doped with a Group VA element;

[0008] forming a second intrinsic i-layer and a p-type doped layer on the first doped region and the second doped region, wherein the p-type doped layer is an amorphous or microcrystalline silicon layer doped with a Group IIIA element;

[0009] forming a patterned mask layer on the second intrinsic i layer and the p-type doped layer, wherein the patterned mask layer exposes the second intrinsic i layer and the p-type doped layer on the first doped region, removing the exposed second intrinsic i layer and the p-type doped layer and retaining the first intrinsic i layer and the n-type doped layer;

[0010] The patterned mask layer is removed, and the second intrinsic i layer and the p-type doping layer are formed in the second doping region.

[0011] In some embodiments, the patterning on the back side of the semiconductor substrate to form a staggered first doped region and a second doped region, wherein the first doped region is formed with a first intrinsic i-layer and an n-type doped layer, specifically comprises:

[0012] forming the first intrinsic i-layer and the n-type doped layer on the back side of the semiconductor substrate;

[0013] Prepare a mask on the surface of the first intrinsic i-layer and the n-type doped layer, and perform exposure and development to form a patterned mask layer;

[0014] removing the first intrinsic i-layer and the n-type doped layer not covered by the mask to form the second doped region;

[0015] The patterned mask layer is removed so that the first doped region is formed with the first intrinsic i-layer and the n-type doped layer.

[0016] In some embodiments, the thickness of the first intrinsic i layer and / or the second intrinsic i layer is 5 nm to 20 nm, and the second intrinsic i layer covers the upper surface and side surfaces of the first intrinsic i layer and the n-type doping layer in the first doping region.

[0017] In some embodiments, forming a patterned mask layer on the second intrinsic i layer and the p-type doped layer, wherein the patterned mask layer exposes the second intrinsic i layer and the p-type doped layer on the first doped region, and removing the exposed second intrinsic i layer and the p-type doped layer and retaining the first intrinsic i layer and the n-type doped layer specifically includes:

[0018] Prepare a mask on the surface of the second intrinsic i-layer and the p-type doped layer, and perform exposure and development to form a patterned mask layer;

[0019] The patterned mask layer exposes the second intrinsic i-layer and the p-type doped layer on the first doped region;

[0020] The second intrinsic i layer and the p-type doped layer exposed to the outside are removed by chemical etching, and the etching rate of the second intrinsic i layer and the p-type doped layer is greater than the etching rate of the n-type doped layer, so that the first intrinsic i layer and the n-type doped layer located below the second intrinsic i layer and the p-type doped layer are retained.

[0021] In some embodiments, the process conditions of the chemical etching include:

[0022] The etching is performed using an alkali solution, wherein the mass concentration of the alkali solution does not exceed 1.5%;

[0023] The etching temperature is 18-35°C.

[0024] In some embodiments, after removing the patterned mask layer and forming the second intrinsic i layer and the p-type doping layer in the second doping region, the method further includes:

[0025] Prepare a back TCO layer on the surfaces of the first intrinsic i layer and the n-type doped layer and the second intrinsic i layer and the p-type doped layer;

[0026] A metal electrode is prepared on the surface of the back TCO layer and the back TCO layer and the metal electrode are patterned.

[0027] In some of the embodiments, the metal electrode patterning includes a first gate line electrode located on the first intrinsic i layer and the n-type doped layer, and a second gate line electrode located on the second intrinsic i layer and the p-type doped layer;

[0028] The width of the first gate line electrode is 50 μm to 300 μm, the width of the second gate line electrode is 500 μm to 1200 μm, and the interval between the first gate line electrode and the second gate line electrode is 100 μm to 500 μm.

[0029] In some embodiments, the method further comprises:

[0030] forming a first intrinsic i-layer and an n-type doped layer on the front side of the semiconductor substrate;

[0031] A front anti-reflection layer is formed on the surfaces of the first intrinsic i-layer and the n-type doping layer.

[0032] In some of the embodiments, in the process step of forming the n-type doping layer: carbon dioxide and / or nitrous oxide are used as an oxygen source, and the flow ratio of the oxygen source to silane is between 1:8 and 2:1.

[0033] According to another aspect of the present application, a heterojunction solar cell is provided, the heterojunction solar cell comprising:

[0034] Semiconductor substrate;

[0035] The back side of the semiconductor substrate is provided with a doping layer, a back side TCO layer and a metal electrode in sequence, wherein the doping layer consists of a first doping region and a second doping region, the first doping region and the second doping region are arranged in an interdigitated manner, the first doping region is provided with a first intrinsic i layer and an n-type doping layer, and the second doping region is provided with a second intrinsic i layer and a p-type doping layer;

[0036] The front side of the semiconductor substrate is provided with a first intrinsic i-layer, an n-type doping layer and a front anti-reflection layer in sequence.

[0037] It should be noted that the above numerical ranges all include endpoint values.

[0038] Implementing the technical solution of the present invention has at least the following beneficial effects:

[0039] In the process of preparing heterojunction solar cells, the present application forms a first intrinsic i layer and an n-type doped layer in the first doped region, wherein the n-type doped layer is an oxygen-doped microcrystalline silicon layer doped with a Group VA element. Thus, when removing the second intrinsic i layer and the p-type doped layer on the first doped region, the difference in the reaction between the n-type doped layer (oxygen-doped microcrystalline silicon layer) and the amorphous i layer (non-oxygen-doped amorphous silicon layer) and the etching solution can be utilized to remove the second intrinsic i layer and the p-type doped layer above the first doped region in one step, and the first intrinsic i layer and the n-type doped layer below the first doped region can be retained. Thus, the present invention can make the originally uncontrollable non-intermediate isolation layer (such as ink or dry film, SiO x or SiN x Etching the second intrinsic i layer and the p-type doped layer (such as ink or dry film) becomes controllable; there is no need to retain an isolation layer (such as ink or dry film) into the cavity, reducing or avoiding the risk of contamination, and no additional isolation layer (such as SiO x or SiN x The tedious steps of removing the isolation layer, etc., simplify the preparation process, simplify the preparation process, and improve the production efficiency.

[0040] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is a schematic diagram of step S110 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0042] Figure 2is a schematic diagram of step S120 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0043] Figure 3 is a schematic diagram of step S130 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0044] Figure 4 is a schematic diagram of step S140 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0045] Figure 5 is a schematic diagram of step S200 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0046] Figure 6 is a schematic diagram of step S300 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0047] Figure 7 is a schematic diagram of step S400 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0048] Figure 8 is a schematic diagram of step S510 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0049] Fig. 9 is a schematic diagram of step S520 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0050] Fig.10 is a schematic diagram of step S530 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0051] Fig.11 is a schematic diagram of step S540 in the method for preparing a heterojunction solar cell provided in some embodiments of the present invention;

[0052] Fig.12 It is a schematic diagram of the structure of a heterojunction solar cell provided by some embodiments of the present invention.

[0053] Description of reference numerals:

[0054] 10- semiconductor substrate;

[0055] 20-a first intrinsic i-layer and an n-type doped layer;

[0056] 31-patterned mask layer; 32-mask (ink or dry film);

[0057] 40-a second intrinsic i-layer and a p-type doped layer;

[0058] 51-back TCO layer; 52-front anti-reflection layer;

[0059] 60- copper seed layer;

[0060] 70 - metal electrode; 71 - first gate line electrode; 72 - second gate line electrode. DETAILED DESCRIPTION

[0061] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0062] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges.

[0063] In the related art, the back of a back contact heterojunction (HJT-IBC, i.e. HBC) solar cell has an n-type region and a p-type region. The n-type region is an intrinsic i layer and a phosphorus-doped n layer grown on the back of a silicon substrate, and the p-type region is an intrinsic i layer and a boron-doped p layer grown on the back of a silicon substrate. This requires complicated mask preparation and removal steps to achieve n-region selectivity and p-region selectivity. Usually, in the preparation process, dry film, ink or inorganic SiO x 、SiN x As an intermediate isolation layer, selective protection is performed on the grown i+n layer, that is, dry film or ink is generally retained on the surface of the i+n layer, which increases the etching and cleaning steps, making the etching and cleaning steps complicated, and requires orderly removal step by step through cleaning, and there is also a risk of contamination. The inventor found that this is because the general n layer and p layer are made of amorphous silicon or microcrystalline silicon. When the i+p is grown on the i+n layer as a whole, the i+p cannot be removed well and it cannot be guaranteed that the i+n layer will not be removed or removed in a controllable manner. Therefore, an intermediate isolation layer such as dry film or ink is generally retained on the surface of the i+n layer, so the etching and cleaning steps are complicated, and it is necessary to remove them in an orderly manner step by step through cleaning, making the entire preparation process cumbersome; or, it is difficult to achieve etching of the phosphorus-doped n layer by one-step alkali etching without etching the underlying intrinsic i layer in the prior art. In addition, intermediate isolation layers such as organic dry films are generally not resistant to high temperatures, and there is a great risk of contaminating the cavity when entering the CVD-plated i+p layer.

[0064] In view of this, the technical solution of the embodiment of the present application provides a method for preparing a heterojunction solar cell and a heterojunction solar cell. The technical solution of the embodiment of the present application is conducive to reducing the cleaning steps, can simplify the preparation process, and reduce the risk of contamination caused by the isolation layer (ink or dry film) entering the cavity. The specific technical solution is described below.

[0065] See also Figures 1 to 12 As shown, in some embodiments, a method for preparing a heterojunction solar cell is provided, the method comprising:

[0066] Patterning the back side of the semiconductor substrate to form a staggered first doping region and a second doping region, wherein the first doping region is formed with a first intrinsic i layer and an n-type doping layer (i+n layer), wherein the n-type doping layer is an oxygen-doped microcrystalline silicon layer doped with a Group VA element;

[0067] forming a second intrinsic i layer and a p-type doped layer (i+p layer) on the first doped region and the second doped region, wherein the p-type doped layer is an amorphous or microcrystalline silicon layer doped with a Group IIIA element;

[0068] forming a patterned mask layer on the second intrinsic i layer and the p-type doped layer, wherein the patterned mask layer exposes the second intrinsic i layer and the p-type doped layer on the first doped region, removing the exposed second intrinsic i layer and the p-type doped layer and retaining the first intrinsic i layer and the n-type doped layer;

[0069] The patterned mask layer is removed, and a second intrinsic i layer and a p-type doping layer are formed in the second doping region, thereby completing the preparation of n and p in the selective region.

[0070] In the method for preparing a heterojunction solar cell provided by an embodiment of the present invention, the n-type doped layer formed is an oxygen-doped microcrystalline silicon layer doped with a Group VA element, and the p-type doped layer formed is an amorphous or microcrystalline silicon layer doped with a Group IIIA element. In this way, when removing the second intrinsic i layer and the p-type doped layer on the first doped region, there is no need to set an intermediate isolation layer. The difference in the reaction between the n-type doped layer (oxygen-doped microcrystalline silicon layer) and the amorphous i layer (non-oxygen-doped amorphous silicon layer) and the etching solution such as an alkaline solution can be used to remove the second intrinsic i layer and the p-type doped layer above the first doped region in one step, and the first intrinsic i layer and the n-type doped layer below the first doped region can be retained, that is, when the alkaline solution is used to etch the second intrinsic i layer and the p-type doped layer located above, it can be ensured that the first intrinsic i layer and the n-type doped layer located below are basically unaffected. Therefore, the present invention can make the originally less controllable non-intermediate isolation layer (such as ink or dry film, SiO x or SiN xThe etching of the second intrinsic i layer and the p-type doping layer becomes controllable; the present invention does not need to retain an isolation layer (such as ink or dry film) into the cavity, reducing or avoiding the risk of contamination, and does not need to add an additional isolation layer (such as SiO x or SiN x The tedious steps of removing the isolation layer, etc., simplify the preparation process, simplify the preparation process, and improve the production efficiency.

[0071] The method for preparing a heterojunction solar cell provided in an embodiment of the present invention grows an i layer on the patterned i+n layer to cover the i+n layer, while achieving the technical effect of insulation. There is no need to perform electrical insulation etching on the p layer and the n layer in the subsequent process, which simplifies the preparation process and facilitates operation.

[0072] The above-mentioned Group VA elements include one or more of nitrogen, phosphorus, arsenic, and antimony. Preferably, in this embodiment, the Group VA element is phosphorus. The above-mentioned Group IIIA elements include one or more of indium, boron, aluminum, and gallium. Preferably, in this embodiment, the Group IIIA element is boron.

[0073] Optionally, the n-type doped layer is an oxygen-doped microcrystalline silicon layer doped with phosphorus. Optionally, the p-type doped layer is an amorphous or microcrystalline silicon layer doped with boron.

[0074] The method provided in the embodiment of the present invention is suitable for application in the field of solar cells, and can be applied to the preparation of various solar cells, such as HBC cells, etc. The method of the present invention is described in detail below mainly by taking HBC cells as an example. However, it can be understood by those skilled in the art that the method of the present invention is not limited to application in HBC cells, but is suitable for application in various solar cells.

[0075] In an embodiment of the present invention, the semiconductor substrate may be a silicon substrate, such as a single crystal silicon substrate, a polycrystalline silicon substrate, or a quasi-single crystal silicon substrate, etc. The embodiment of the present invention does not limit the specific type of the semiconductor substrate. The semiconductor substrate may be P-type doped or N-type doped, that is, the semiconductor substrate may be a P-type semiconductor substrate or an N-type semiconductor substrate. The heterojunction solar cell of the embodiment of the present invention may be an N-type heterojunction solar cell, or may be a P-type heterojunction solar cell. Exemplarily, in some embodiments, the heterojunction solar cell may be an N-type heterojunction solar cell, and the semiconductor substrate may be an N-type silicon substrate (also referred to as an N-type silicon wafer).

[0076] In an embodiment of the present invention, the semiconductor substrate includes two side surfaces arranged opposite to each other, namely a front side and a back side; the front side (light-receiving side) of the semiconductor substrate is the surface facing the sun, that is, the surface facing sunlight, and the back side (backlight side) of the semiconductor substrate is the surface facing away from the sun.

[0077] In the process of preparing heterojunction solar cells, the present invention mainly improves the preparation of the back structure of the semiconductor substrate. The preparation of the front structure of the semiconductor substrate can refer to the preparation of solar cells in the relevant field, and this embodiment does not limit this.

[0078] In some specific embodiments, a method for preparing a heterojunction solar cell comprises the following steps:

[0079] S100, patterning the back side of the semiconductor substrate to form a first doped region and a second doped region, so that the first doped region and the second doped region are arranged in an interdigitated manner, and a first intrinsic i layer and an n-type doped layer are formed in the first doped region, wherein the n-type doped layer is an oxygen-doped microcrystalline silicon layer doped with phosphorus. Specifically, step S100 includes:

[0080] S110, such as Figure 1 As shown, a semiconductor substrate 10 is provided, a first intrinsic i layer and an n-type doped layer 20 are formed on the back side of the semiconductor substrate 10, and a first intrinsic i layer and an n-type doped layer 20 are also formed on the front side of the semiconductor substrate 10; wherein the n-type doped layer is an oxygen-doped microcrystalline silicon layer doped with phosphorus.

[0081] In this step, a double-sided plating process is performed on the semiconductor substrate to form a first intrinsic i layer and an n-type doped layer on both the front and back sides of the semiconductor substrate. In this embodiment, the method for forming the first intrinsic i layer and the n-type doped layer can adopt the existing conventional process method for forming the intrinsic i layer and the doped layer. Exemplarily, a chemical vapor deposition method (CVD) can be used to sequentially deposit the first intrinsic i layer and the n-type doped layer on the front and back sides of the semiconductor substrate. Optionally, the chemical vapor deposition method (plating method) includes but is not limited to PECVD or Cat-CVD. The specific operation method and process conditions for forming the first intrinsic i layer and the n-type doped layer can be selected and regulated by a technician in this field according to actual conditions, and this embodiment does not limit this.

[0082] The n-type doped layer on the front side of the semiconductor substrate can be used as both a front side passivation layer and a light-transmitting window layer.

[0083] Optionally, the provided semiconductor substrate is a textured semiconductor substrate. Exemplarily, providing the semiconductor substrate includes: providing an n-type single crystal silicon substrate, cleaning and textured the n-type single crystal silicon substrate, and forming a textured structure on the clean surface of the n-type single crystal silicon substrate.

[0084] Optionally, the thickness of the first intrinsic i layer is 5 nm to 20 nm. Further, the thickness of the first intrinsic i layer may be 7 nm to 10 nm. For example, the first intrinsic i layer may be 5 nm, 6 nm, 4 nm, 8 nm, 9 nm, 10 nm, 12 nm, 15 nm, 16 nm, 18 nm, 20 nm, etc.

[0085] Optionally, the thickness of the n-type doping layer may be 8 nm to 200 nm. Further, the thickness of the n-type doping layer may be 10 nm to 150 nm.

[0086] Optionally, the n-type doped layer is prepared by chemical vapor deposition. Preferably, in the process step of preparing the n-type doped layer, i.e., the n-doped oxygen-doped microcrystalline silicon layer, carbon dioxide or nitrous oxide can be used as an oxygen source, and the flow ratio of the oxygen source to silane is between 1:8 and 2:1. In this way, it is easy to obtain the desired n-doped oxygen-doped microcrystalline silicon layer, and when removing the second intrinsic i layer and the p-type doped layer on the first doped region, the difference in the reaction between the n-type doped layer (oxygen-doped microcrystalline silicon layer) and the amorphous i layer (non-oxygen-doped amorphous silicon layer) and the etching solution can be used to remove the second intrinsic i layer and the p-type doped layer above the first doped region in one step, and the first intrinsic i layer and the n-type doped layer below the first doped region can be retained.

[0087] S120, such as Figure 2 As shown, a mask is prepared on the surface of the first intrinsic i layer and the n-type doped layer 20 on the back side of the semiconductor substrate 10, and is exposed and developed to form a patterned mask layer 31; and a mask 32 is prepared on the surface of the first intrinsic i layer and the n-type doped layer 20 on the front side of the semiconductor substrate 10, and the entire mask layer on the front side is retained.

[0088] In this step, the front and back sides of the semiconductor substrate 10 are laminated, and the film refers to an organic film layer (which can be called a photomask) that can be or has photosensitive development characteristics. The back side of the semiconductor substrate 10 is exposed and developed, and the mask area is removed at the developed area to form a patterned mask layer 31; the developed area on the back side of the semiconductor substrate is the second doping area, that is, the area for the subsequent deposition of the p-type doping layer. The front side of the semiconductor substrate 10 is fully exposed and the mask 32 layer on the entire surface is retained to protect the first intrinsic i layer and the n-type doping layer 20 on the front side from being removed.

[0089] It is worth noting that the above-mentioned photomask is required to be resistant to alkali, but is not required to be resistant to other solutions.

[0090] S130, such as Figure 3 As shown, the first intrinsic i-layer and the n-type doping layer 20 not covered by the mask are removed to form the second doping region.

[0091] In this step, for the back side of the semiconductor substrate 10, since part of the first intrinsic i layer and the n-type doping layer 20 are covered by the photomask, and the other part of the first intrinsic i layer and the n-type doping layer 20 are not covered by the photomask, the first intrinsic i layer and the n-type doping layer 20 not covered by the photomask can be removed by conventional methods, and the area after the first intrinsic i layer and the n-type doping layer 20 are removed is the second doping area. For the front side of the semiconductor, the first intrinsic i layer and the n-type doping layer 20 will be protected by the entire photomask 32 so as not to be removed.

[0092] Optionally, the sample obtained in step S120 is placed in an alkaline solution for cleaning to remove the first intrinsic i layer and the n-type doping layer 20 in the area not protected by the photomask after development. This embodiment does not specifically limit the concentration or temperature of the alkaline solution used in this step, and can be selected and adjusted by those skilled in the art according to actual conditions, as long as the first intrinsic i layer and the n-type doping layer not covered by the mask can be cleaned.

[0093] S140, such as Figure 4 As shown, the patterned mask layer 31 is removed, so that the first doped region is formed with a first intrinsic i-layer and an n-type doped layer 20 .

[0094] This step mainly removes the remaining photomask (patterned mask layer 31) on the back side of the semiconductor substrate 10 so that the first doped region is only provided with the first intrinsic i layer and the n-type doped layer 20; while the entire photomask 32 on the front side of the semiconductor substrate 10 is still retained.

[0095] Optionally, the sample obtained in step S130 is placed in a solution capable of etching away the photomask after exposure, so as to remove the photomask on the first intrinsic i layer and the n-type doping layer, thereby forming the first intrinsic i layer and the n-type doping layer only in the first doping region. The solution capable of etching away the photomask is a solution that does not react with silicon, that is, the solution only needs to be able to remove the photomask and not react with silicon, and this embodiment does not limit the specific type or operation method of the solution.

[0096] S200, such as Figure 5 As shown, a second intrinsic i layer and a p-type doped layer 40 are sequentially formed on the first doped region and the second doped region, wherein the p-type doped layer is an amorphous or microcrystalline silicon layer doped with boron; that is, the p-type doped layer can be an amorphous silicon layer doped with boron, or the p-type doped layer can be a microcrystalline silicon layer doped with boron.

[0097] In step S200, a second intrinsic i layer and a p-type doped layer 40 are prepared on the back side of the semiconductor substrate 10. Since in the sample obtained in step S140, the first doped region is provided with the first intrinsic i layer and the n-type doped layer 20, therefore, in the first doped region, the second intrinsic i layer and the p-type doped layer 40 cover the upper surface and the side surface of the first intrinsic i layer and the n-type doped layer 20, and in the second doped region, the second intrinsic i layer and the p-type doped layer 40 cover the back surface of the semiconductor substrate 10.

[0098] In this embodiment, the method for forming the second intrinsic i layer and the p-type doping layer can adopt the existing conventional process method for forming the intrinsic i layer and the doping layer. For example, the second intrinsic i layer and the p-type doping layer can be prepared by the same or similar method and process conditions as step S110. Exemplarily, the second intrinsic i layer and the p-type doping layer can be deposited in sequence on the back side of the semiconductor substrate by chemical vapor deposition (CVD). Optionally, the chemical vapor deposition method (coating method) includes but is not limited to PECVD or Cat-CVD. The specific operation method and process conditions for forming the second intrinsic i layer and the p-type doping layer can refer to step S110 or be selected and regulated by those skilled in the art according to actual conditions, and this embodiment does not limit this.

[0099] Generally, in the existing process steps, after the n-doped layer and the p-doped layer are formed, a process step of performing electrical insulation treatment on the n-doped layer and the p-doped layer is also included. However, in the embodiment of the present application, in step S200, the second intrinsic i-layer can completely cover the upper surface and side surface of the first intrinsic i-layer and the n-type doped layer 20 in the first doped region, so that the p-type doped layer formed by subsequent deposition can be electrically insulated from the n-type doped layer, without adding additional electrical insulation treatment process steps, thereby achieving the purpose of simplifying the process and reducing costs.

[0100] Optionally, the thickness of the second intrinsic i layer is 5nm to 20nm. Further, the thickness of the second intrinsic i layer may be 7nm to 10nm. For example, the second intrinsic i layer may be 5nm, 6nm, 4nm, 8nm, 9nm, 10nm, 12nm, 15nm, 16nm, 18nm, 20nm, etc. The thickness of the second intrinsic i layer may be consistent with the thickness of the first intrinsic i layer.

[0101] Optionally, the thickness of the p-type doping layer may be 8 nm to 200 nm. Further, the thickness of the p-type doping layer may be 10 nm to 150 nm.

[0102] S300, such as Figure 6As shown, a patterned mask layer 31 is formed on the second intrinsic i layer and the p-type doped layer 40, and the patterned mask layer 31 exposes the second intrinsic i layer and the p-type doped layer 40 on the first doped region, removes the exposed second intrinsic i layer and the p-type doped layer 40 and retains the first intrinsic i layer and the n-type doped layer 20.

[0103] In step S300, for the back side of the semiconductor substrate 10, the sample obtained in step S200 is subjected to lamination, exposure and development to expose the second intrinsic i layer and the p-type doping layer 40 above the first intrinsic i layer and the n-type doping layer 20 formed in the first doping region, and then the sample can be placed in an etching solution (such as an alkaline solution) to etch away the exposed second intrinsic i layer and the p-type doping layer 40, but the first intrinsic i layer and the n-type doping layer 20 below are not etched. Specifically, step S300 includes:

[0104] S310, for the back side of the semiconductor substrate 10, the sample obtained in step S200 is laminated, that is, a mask is prepared on the surface of the second intrinsic i layer and the p-type doping layer 40, and then exposed and developed to form a patterned mask layer 31. The patterned mask layer 31 covers the second intrinsic i layer and the p-type doping layer 40 located in the second doping region, and exposes the second intrinsic i layer and the p-type doping layer 40 located on the first doping region.

[0105] The operation method and conditions of preparing the mask, exposing and developing in step S310 can refer to step S120 and will not be described in detail here.

[0106] S320, using chemical etching to remove the second intrinsic i layer and the p-type doping layer 40 that are exposed to the outside (not covered by the photomask). In the first doping region, since the etching rate of the second intrinsic i layer and the p-type doping layer 40 is greater than the etching rate of the n-type doping layer, the first intrinsic i layer and the n-type doping layer 20 located below the second intrinsic i layer and the p-type doping layer 40 are retained.

[0107] In this embodiment, in the first doped region, the second intrinsic i layer and the p-type doped layer are etched away while the first intrinsic i layer and the n layer are retained, mainly by utilizing the characteristic that the n-doped oxygen-doped microcrystalline silicon layer reacts more slowly with the alkaline solution than the non-oxygen-doped amorphous intrinsic i layer, so that after the amorphous intrinsic i layer located on the upper layer is etched, the reaction rate with the n-doped oxygen-doped microcrystalline silicon layer drops sharply, so that the n layer located below will not be etched too much. The above-mentioned chemical etching can be carried out with an alkaline solution, and the temperature and concentration of the alkaline solution can be adjusted according to the amount of oxygen doping in the microcrystalline n layer, and the oxygen doping amount can be adjusted by adjusting the flow rate of the oxygen source. Because the more oxygen doping, the slower the reaction rate of the microcrystalline n layer with the alkaline solution, and the etching rate generally shows the difference in etching rate at a certain specific oxygen doping ratio of the solution concentration and temperature.

[0108] Optionally, the process conditions of the chemical etching include: etching with alkaline solution, the mass concentration of the alkaline solution does not exceed 1.5%; the etching temperature is 18-35° C. Optionally, the alkaline solution used can be a NaOH solution, and of course other types of alkaline solutions can also be used, which is not limited in this embodiment.

[0109] When etching the exposed second intrinsic i layer and the p-type doped layer, the concentration of the alkaline solution used is not easy to be too high, and the etching temperature is not easy to be too high. For example, the mass concentration of the alkaline solution can be ≤1.5%, or ≤1%, ≤0.8%, etc., and exemplary, the mass concentration of the alkaline solution can be 1.5%, 1.2%, 1.0%, 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4%, 0.3%, etc. The etching temperature can be 18-35°C, and further can be 20-30°C, for example, it can be 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 28°C, 30°C, 35°C, etc. The concentration of the above alkaline solution and the etching problem can be adjusted according to the oxygen doping amount of the n-type doped layer. Within the above range, it is helpful to make the etching rate moderate, improve production efficiency, reduce costs, and ensure the quality of the silicon wafer.

[0110] S400, such as Figure 7 As shown, the patterned mask layer 31 on the back side of the semiconductor substrate 10 is removed, a second intrinsic i layer and a p-type doping layer 40 are formed in the second doping region, and the entire mask layer 32 on the front side of the semiconductor substrate 10 is removed.

[0111] In this step, the photomask (patterned mask layer 31) remaining on the back side of the semiconductor substrate 10 is mainly removed, that is, the photomask located in the second doping region is removed, so that the second doping region is only provided with the second intrinsic i layer and the p-type doping layer 40, thereby completing the preparation of the n-type region and the p-type region of the selective region. At the same time, in this step, while removing the mask remaining on the back side, the entire mask 32 layer on the front side of the semiconductor substrate 10 can also be removed.

[0112] Optionally, the sample obtained in step S320 may be placed in an appropriate dry film removing solution capable of removing the developed dry film to remove the dry film on the front and back sides of the semiconductor substrate.

[0113] The requirements for removing the photomask in step S400 and the solution or operating conditions used can refer to the method for removing the photomask in step S140 and will not be described in detail here.

[0114] S500, preparing a back TCO layer on the surfaces of the first intrinsic i layer and the n-type doped layer and the second intrinsic i layer and the p-type doped layer; preparing a metal electrode on the surface of the back TCO layer and patterning the back TCO layer and the metal electrode.

[0115] This step S500 is mainly used to prepare a metal electrode. It should be noted that the embodiment of the present application does not limit the specific operation method and process conditions for forming the metal electrode, which can be selected and regulated by those skilled in the art according to actual conditions, such as the conventional method for preparing metal electrodes in the field of solar cells. Exemplarily, this step S500 may include:

[0116] S510, such as Figure 8 As shown, a back TCO layer 51 and a copper seed layer 60 are prepared on the back side of the semiconductor substrate 10, and a front anti-reflection layer 52 is prepared on the front side of the semiconductor substrate 10. Specifically, for the back side of the semiconductor substrate 10, the back TCO layer 51 is formed on the surfaces of the first intrinsic i layer and the n-type doping layer 20 and the second intrinsic i layer and the p-type doping layer 40, that is, the back TCO layer 51 is formed on the surfaces of the first doping region and the second doping region, and the copper seed layer 60 is formed on the surface of the back TCO layer 51. For the front side of the semiconductor substrate 10, the front anti-reflection layer 52 is formed on the surfaces of the first intrinsic i layer and the n-type doping layer 20.

[0117] The front anti-reflection layer 52 is a transparent conductive layer or other non-conductive anti-reflection layer and the back TCO layer 51 is a transparent conductive layer. The anti-reflection layer on the front side of the semiconductor substrate may include but is not limited to a transparent conductive layer ITO film, IWO film or AZO film or a non-conductive anti-reflection layer SiN x Thin film, SiN x O y One or more of the films, the transparent conductive layer on the back can include one or more of ITO film, IWO film or AZO film but not limited to other transparent conductive films.

[0118] In this embodiment, the method of forming the front anti-reflection layer 52, the back TCO layer 51 and the copper seed layer 60 can adopt the existing conventional process method; illustratively, the preparation method of the front anti-reflection layer, the back TCO layer and the copper seed layer includes but is not limited to PVD or RPD or evaporation and other film deposition methods.

[0119] Optionally, the thickness of the front anti-reflection layer and the back TCO layer may be 50 to 150 nm; further, the thickness of the front anti-reflection layer and the back TCO layer may be 70 to 900 nm.

[0120] Optionally, the thickness of the copper seed layer may be 50-1000 nm; further, the thickness of the copper seed layer may be 100-20 nm.

[0121] The use of the front anti-reflection layer, the back TCO layer and the copper seed layer within the above range is easy to implement and can be prepared using conventional process conditions, which helps to reduce costs and improve production efficiency.

[0122] S520, such as Fig. 9 As shown, the sample obtained in step S510 is electroplated to prepare a metal gate electrode. Specifically, electroplating is performed on the back of the semiconductor substrate 10 to prepare a metal electrode 70, and the metal electrode 70 (gate electrode) is arranged at intervals on the surface of the copper seed layer 60. It is worth noting that in the subsequent steps, the copper seed layer 60 needs to be etched away.

[0123] Optionally, the metal electrode patterning includes a first gate electrode 71 located on the first intrinsic i layer and the n-type doped layer 20, and a second gate electrode 72 located on the second intrinsic i layer and the p-type doped layer 40; that is, the metal electrode patterning includes a first gate electrode 71 located on the first doped region and a second gate electrode 72 located on the second doped region. The metal electrode may include a copper gate electrode, and the width of the first gate electrode 71 and the second gate electrode 72 (copper gate line) may be 50 μm to 1500 μm.

[0124] Optionally, the width of the first gate line electrode may be 50 μm to 300 μm. Further, the width of the first gate line electrode may be 100 μm to 200 μm.

[0125] Optionally, the width of the second gate line electrode may be 500 μm to 1200 μm. Further, the width of the first gate line electrode may be 600 μm to 1000 μm.

[0126] Optionally, the spacing between the first gate line electrode and the second gate line electrode may be 100 μm to 500 μm. Further, the spacing between the first gate line electrode and the second gate line electrode may be 150 μm to 350 μm. In this way, by maintaining a certain spacing between the first gate line electrode and the second gate line electrode, it can be ensured that the n-type region and the p-type region are not turned on to cause leakage.

[0127] S530, such as Fig.10 As shown, the sample obtained in step S520 is subjected to lamination on the entire front surface of the semiconductor substrate 10, and then exposed; the sample is then placed in an alkaline solution for film removal. The purpose of this step is mainly to etch away the TCO layer in the gate line isolation area of ​​the n-type region and the p-type region, and further achieve isolation of the n-type region and the p-type region.

[0128] The lamination and drying materials or requirements in this step may refer to step S120, and this embodiment does not limit this.

[0129] S540, such as Fig.11 As shown, the front side of the semiconductor substrate of the sample obtained in step S530 is placed in an alkaline solution capable of removing dry films to remove the photomask on the front side of the semiconductor substrate, and then washed and dried to obtain a heterojunction solar cell.

[0130] The solution or operation requirements for removing the dry film in this step may refer to step S140 , and this embodiment does not limit this.

[0131] See also Fig.12 As shown, in some embodiments, a heterojunction solar cell is provided, the heterojunction solar cell comprising: a semiconductor substrate 10;

[0132] A doping layer, a back TCO layer 51 and a metal electrode 70 are sequentially arranged on the back side of the semiconductor substrate 10, wherein the doping layer consists of a first doping region and a second doping region, the first doping region and the second doping region are arranged in an interlaced manner in a finger-like manner, the first doping region is provided with a first intrinsic i layer and an n-type doping layer 20, and the second doping region is provided with a second intrinsic i layer and a p-type doping layer 40; the metal electrode 70 includes a first gate line electrode 71 located on the first doping region and a second gate line electrode 72 located on the second doping region.

[0133] The front surface of the semiconductor substrate 10 is provided with a first intrinsic i-layer, an n-type doping layer 20 , and a front anti-reflection layer 52 in sequence.

[0134] Those skilled in the art can understand that the heterojunction solar cell and the aforementioned method for preparing a heterojunction solar cell are based on the same inventive concept, and the features and advantages described above for the method for preparing a heterojunction solar cell are also applicable to the heterojunction solar cell. Therefore, the heterojunction solar cell has at least the same or different features and advantages as the aforementioned method for preparing a heterojunction solar cell, which will not be described in detail herein.

[0135] According to step S300 in the method provided in the embodiment of the present application, different types or different composition film layers react to different degrees with the alkaline solution. In order to show the etching degree of the alkaline solution on different types of film layers, this embodiment carried out multiple groups of test verifications, using alkaline solution to etch different film layers. The test results are shown in Table 1 below.

[0136] Table 1

[0137]

[0138]

[0139] In Table 1, α-i-1 to α-i-4 respectively represent amorphous i layer-1 (1# amorphous i layer), amorphous i layer-2 (2# amorphous i layer), amorphous i layer-3, amorphous i layer-4; μc-SiO x -1 to μc-SiO x -3 respectively represent microcrystalline n oxygen-doped layer-1 (1# microcrystalline n oxygen-doped layer), microcrystalline n oxygen-doped layer-2, and microcrystalline n oxygen-doped layer-3; μc-Si-1 to μc-Si-3 respectively represent microcrystalline silicon (non-oxygen-doped) layer-1, microcrystalline silicon layer-2, and microcrystalline silicon layer-3.

[0140] From the data in Table 1, it can be seen that there is a difference in the reaction of the oxygen-doped microcrystalline n layer and the non-oxygen-doped amorphous i layer with the alkaline solution. Therefore, the present application utilizes the characteristic that the reaction of the microcrystalline oxygen-doped microcrystalline silicon oxide with the alkaline solution is slower than that of the non-oxygen-doped amorphous intrinsic i layer, and removes the second intrinsic i layer and the p-type doped layer above the first doped region in one step, and can retain the first intrinsic i layer and the n-type doped layer below the first doped region. That is, when the alkaline solution is used to etch the second intrinsic i layer and the p-type doped layer located above, it can ensure that the first intrinsic i layer and the n-type doped layer located below are basically unaffected, thereby simplifying the preparation process, simplifying the preparation process, improving production efficiency, and reducing or avoiding the risk of pollution.

[0141] The terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable under appropriate circumstances, so that the embodiments of the present application can be implemented in an order other than those illustrated or described here, and the objects distinguished by "first", "second", etc. are generally a class, and the number of objects is not limited. For example, the first object can be one or more. In addition, the term "and / or" used in this article is only a kind of association relationship describing associated objects, indicating that three relationships can exist, for example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone.

[0142] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.

Claims

1. A method for preparing a heterojunction solar cell, characterized in that: The method comprises: Patterning the back side of the semiconductor substrate to form a staggered first doped region and a second doped region, wherein the first doped region is formed with a first intrinsic i layer and an n-type doped layer, wherein the first intrinsic i layer is an oxygen-free amorphous silicon layer, and the n-type doped layer is an oxygen-doped microcrystalline silicon layer doped with a Group VA element; forming a second intrinsic i layer and a p-type doped layer on the first doped region and the second doped region, wherein the second intrinsic i layer is an oxygen-free amorphous silicon layer, and the p-type doped layer is an amorphous or microcrystalline silicon layer doped with a Group IIIA element; A mask is prepared on the surface of the second intrinsic i layer and the p-type doped layer, and exposed and developed to form a patterned mask layer; the patterned mask layer exposes the second intrinsic i layer and the p-type doped layer on the first doped region; Removing the exposed second intrinsic i layer and p-type doped layer by chemical etching, wherein the etching rate of the second intrinsic i layer and p-type doped layer is greater than the etching rate of the n-type doped layer, so that the first intrinsic i layer and n-type doped layer located below the second intrinsic i layer and p-type doped layer are retained; wherein the chemical etching is performed by alkaline solution; The patterned mask layer is removed, and the second intrinsic i layer and the p-type doping layer are formed in the second doping region.

2. The method for preparing a heterojunction solar cell according to claim 1, characterized in that: The patterning on the back side of the semiconductor substrate to form a staggered first doping region and a second doping region, wherein the first doping region is formed with a first intrinsic i-layer and an n-type doping layer, specifically comprises: forming the first intrinsic i-layer and the n-type doped layer on the back side of the semiconductor substrate; Prepare a mask on the surface of the first intrinsic i-layer and the n-type doped layer, and perform exposure and development to form a patterned mask layer; removing the first intrinsic i-layer and the n-type doped layer not covered by the mask to form the second doped region; The patterned mask layer is removed so that the first doped region is formed with the first intrinsic i-layer and the n-type doped layer.

3. The method for preparing a heterojunction solar cell according to claim 1 or 2, characterized in that: The thickness of the first intrinsic i layer and / or the second intrinsic i layer is 5 nm to 20 nm, and the second intrinsic i layer covers the upper surface and side surfaces of the first intrinsic i layer and the n-type doping layer in the first doping region.

4. The method for preparing a heterojunction solar cell according to claim 1, characterized in that: The process conditions of the chemical etching include: The mass concentration of the alkali solution does not exceed 1.5%; The etching temperature is 18-35°C.

5. The method for preparing a heterojunction solar cell according to claim 1, characterized in that: After removing the patterned mask layer and forming the second intrinsic i layer and the p-type doping layer in the second doping region, the method further includes: Prepare a back TCO layer on the surfaces of the first intrinsic i layer and the n-type doped layer and the second intrinsic i layer and the p-type doped layer; A metal electrode is prepared on the surface of the back TCO layer and the back TCO layer and the metal electrode are patterned.

6. The method for preparing a heterojunction solar cell according to claim 5, characterized in that: The metal electrode patterning includes a first gate line electrode located on the first intrinsic i layer and the n-type doped layer, and a second gate line electrode located on the second intrinsic i layer and the p-type doped layer; The width of the first gate line electrode is 50 μm to 300 μm, the width of the second gate line electrode is 500 μm to 1200 μm, and the interval between the first gate line electrode and the second gate line electrode is 100 μm to 500 μm.

7. The method for preparing a heterojunction solar cell according to claim 1, characterized in that: The method further comprises: forming a first intrinsic i-layer and an n-type doped layer on the front side of the semiconductor substrate; A front anti-reflection layer is formed on the surfaces of the first intrinsic i-layer and the n-type doping layer.

8. The method for preparing a heterojunction solar cell according to any one of claims 1-2 and 4-7, characterized in that: In the process steps of forming the n-type doping layer: carbon dioxide and / or nitrous oxide are used as oxygen sources, and the flow ratio of the oxygen source to silane is between 1:8 and 2:

1.

9. A heterojunction solar cell, characterized in that: The heterojunction solar cell is prepared by the method according to claim 1, and the heterojunction solar cell comprises: Semiconductor substrate; The back side of the semiconductor substrate is provided with a doping layer, a back side TCO layer and a metal electrode in sequence, wherein the doping layer consists of a first doping region and a second doping region, the first doping region and the second doping region are arranged in an interdigitated manner, the first doping region is provided with a first intrinsic i layer and an n-type doping layer, and the second doping region is provided with a second intrinsic i layer and a p-type doping layer; The front side of the semiconductor substrate is provided with a first intrinsic i-layer, an n-type doping layer and a front anti-reflection layer in sequence.