A perovskite solar cell doped with a hydrazide passivating agent and a preparation method thereof
By adding benzoyl hydrazide as a doped hydrazide passivator in perovskite solar cells, the stability problems caused by defects and iodide ion migration during the annealing process of perovskite solar cells are solved, significantly improving the performance of solar cells. power conversion efficiency and stability.
Patent Information
- Application Number
- CN202210502825.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-07-15
AI Technical Summary
Perovskite solar cells produce a large number of defects during the annealing process, resulting in insufficient efficiency and stability, and the migration of iodine ions causes film instability and affects battery performance.
Using a doped hydrazide passivator, benzoyl hydrazide is added to the perovskite light-absorbing layer and used as a Lewis base to coordinate with the lead in the perovskite to passivate defects and inhibit the generation of iodine elements. , slow down ion migration and prepare efficient and stable perovskite solar cells.
It effectively reduces defects in the perovskite film, improves carrier transport efficiency and structural stability, and significantly improves the power conversion efficiency and stability of solar cells.
Smart Images

Figure CN115050891B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optoelectronic materials, and in particular relates to a perovskite solar cell doped with a hydrazide passivating agent and a preparation method thereof. Background Art
[0002] Metal halide perovskites are widely considered to be one of the most promising optoelectronic materials due to their excellent optoelectronic properties, including tunable band gap, high molar absorption coefficient, long carrier diffusion length and low exciton binding energy. Nowadays, they have been widely used in various light-emitting devices, such as light-emitting diodes, photodetectors, solar cells, etc. Among them, perovskite solar cells (PSCs) have received the most attention. Since Park's pioneering report on all-solid-state perovskite photovoltaic devices, a record of 25.7% certified power conversion efficiency (PCE) has been achieved. PSCs have made great progress in efficiency and stability, mainly due to various modification engineering, including composition engineering, solvent engineering, additive engineering and interface engineering. However, the current stability and efficiency are still not up to the level of commercialization. Therefore, it is urgent to develop a new strategy to minimize the efficiency and stability loss.
[0003] As we all know, perovskite will rapidly crystallize and grow during the annealing process, inevitably generating a large number of defects that hinder the transport, transfer and extraction of carriers, leading to severe bulk and interface non-radiative recombination. Among these defects, the defects in the bulk are mostly shallow-level defects, while the defects at the grain boundaries are mainly deep-level defects, which will lead to severe non-radiative recombination losses. Additive engineering is a very effective defect passivation strategy. So far, a variety of additive molecules have been explored to passivate defects in perovskite films, such as Lewis acids, Lewis bases, organic small molecules, inorganic salts, etc. Among them, Lewis bases have been widely reported to improve the efficiency of batteries. Therefore, it is urgent to find suitable Lewis bases to passivate film defects and improve battery efficiency and stability.
[0004] In addition, the migration of iodine ions is also considered to be harmful. This is mainly because the migration of I ions will form iodine, and the volatile iodine will escape from the perovskite film. This not only causes a large number of voids in the film, but also the formation of a large number of anion vacancies will increase the defects of the film. Therefore, how to inhibit the migration of iodine ions and increase the stability of the film becomes very important. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a highly efficient and stable perovskite solar cell doped with a hydrazide passivating agent and a preparation method thereof.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A perovskite solar cell doped with a hydrazide passivator comprises, from bottom to top, conductive glass, an electron transport layer, a perovskite light absorption layer, a hole transport layer and a metal back electrode, wherein benzoyl hydrazide is added to the perovskite light absorption layer.
[0008] Furthermore, the conductive glass is ITO or FTO; the electron transport layer is titanium dioxide; the metal back electrode is gold, silver, copper or aluminum;
[0009] The perovskite light absorbing layer is an ABX3 perovskite light absorbing layer, wherein A is CH3NH3 + or CH(NH2) 2+ One or two of the following, B is Pb 2+ , X is I - Br - or Cl - ;
[0010] The hole transport layer is 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene.
[0011] A method for preparing the perovskite solar cell doped with a hydrazide passivating agent comprises the following steps:
[0012] Step 1, the conductive glass is sequentially treated with detergent, deionized water, and anhydrous ethanol, then blown dry, and then treated with ultraviolet ozone, and then taken out for use;
[0013] Step 2, mixing distilled water and titanium tetrachloride to obtain a mixed solution, immersing the conductive glass treated with ozone in step 1 in the mixed solution, and then drying, taking out after drying, rinsing with distilled water, and then drying with nitrogen, annealing, to obtain an electron transport layer, and then subjecting the electron transport layer to ultraviolet ozone treatment;
[0014] Step 3, dissolving the perovskite light absorbing layer material in a mixed solvent of DMF and DMSO to obtain a perovskite precursor solution, then adding benzoyl hydrazide, shaking, filtering, and then spin-coating on the electron transport layer, followed by annealing, and before the perovskite precursor solution is spin-coated, chlorobenzene is added dropwise;
[0015] Step 4, dissolving the hole transport layer material in chlorobenzene, adding an anhydrous acetonitrile solution containing TBP and Li-TFSI, mixing well and spin coating the mixture on the perovskite light absorbing layer prepared in step 3 to prepare a hole transport layer;
[0016] Step 5: Deposit a metal back electrode on the hole transport layer prepared in step 4 by thermal evaporation under high vacuum.
[0017] Furthermore, in step 1, the conductive glass is ITO or FTO, the ultrasonic treatment time is 20 minutes, and the ozone treatment time is 20 to 30 minutes.
[0018] Furthermore, in step 2, the volume ratio of distilled water to titanium tetrachloride is 1:1-3, the drying temperature is 75°C, the time is 45 minutes, the annealing temperature is 200°C, the time is 30 minutes, and the ozone treatment time is 20-30 minutes.
[0019] Furthermore, in step 3, the perovskite light-absorbing layer material is an organic amine salt and a lead halide salt, and the volume ratio of DMF and DMSO is 4:1.
[0020] Furthermore, in step 3, the shaking time is 5 minutes, the spin coating speed is 4000 rpm, the time is 30 seconds, and the annealing temperature is 130° C., and the time is 28 minutes.
[0021] Furthermore, in step 3, benzoyl hydrazide is added so that the concentration of the perovskite precursor solution of benzoyl hydrazide is 0.015-1 mg / mL.
[0022] Furthermore, in step 4, the hole transport layer material is 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, the concentration of the anhydrous acetonitrile solution of Li-TFSI is 520 mg / mL, the spin coating speed is 3000 rpm, and the time is 30 s.
[0023] Furthermore, in step 5, the metal back electrode is gold, silver, copper or aluminum, and the evaporation thickness is 100 nm.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] 1. The present invention uses benzamide as an additive to regulate the crystallization process of the film. Benzamide is a typical Lewis base, and the -NH2 and -C=O contained in it can coordinate with the lead in the perovskite, which can passivate the anion defects in the perovskite film.
[0026] 2. Hydrazine substances are reducing, which inhibits the formation of iodine and slows down ion migration, thereby promoting the stability of the perovskite structure.
[0027] 3. The device produced by the present invention has a higher PCE. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The scanning electron microscope images of the perovskite film in the comparative example and embodiment 1;
[0029] Figure 2 It is a defect test diagram of the perovskite film in the comparative example and embodiment 1;
[0030] Figure 3 is a carrier lifetime diagram of the perovskite film in the comparative example and example 1;
[0031] Figure 4 The current-voltage curves of the perovskite solar cells in the comparative example and example 1;
[0032] Figure 5 is a current-voltage forward scan curve of the perovskite solar cell in Example 2;
[0033] Figure 6 This is a current-voltage forward scan curve of the perovskite solar cell in Example 3. DETAILED DESCRIPTION
[0034] Comparative Examples
[0035] A method for preparing a perovskite solar cell comprises the following steps:
[0036] (1) The FTO conductive substrate was treated with detergent, deionized water, and anhydrous ethanol in sequence for 20 minutes by ultrasonic treatment, then blown dry, and then treated with ultraviolet ozone for 30 minutes, and then taken out for use;
[0037] (2) Distilled water and titanium tetrachloride were mixed in a volume ratio of 1:2.25, and then the FTO prepared in (1) was immersed in the mixed solution, and then placed in an oven at 75°C for 45 minutes, and then taken out and rinsed with distilled water several times, and then dried with nitrogen, and then annealed on a hot stage at 200°C for 30 minutes to obtain an electron transport layer (titanium dioxide), and then the electron transport layer was treated with ultraviolet ozone for 20 minutes;
[0038] (3) FAI (248 mg), PbBr2 (8.5 mg), RbI (6.6 mg), MACl (35.0 mg), PbI2 (682.7 mg), CsI (19.7 mg) and PbCl2 (12.7 mg) were dissolved in a mixture of DMF and DMSO (V DMF :V DMSO =4:1), after shaking for 5 minutes, the perovskite precursor solution was added dropwise onto the electron transport layer prepared in step (2), and spin-coated at a speed of 4000 rpm for 30 seconds, followed by annealing at 130° C. for 28 minutes, wherein 16 seconds before the end of the spin coating of the perovskite precursor solution, 80 μL of chlorobenzene was added dropwise within 2 seconds to prepare the perovskite light absorbing layer;
[0039] (4) Dissolve 72.3 mg of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) in 1 mL of chlorobenzene, add 29 μL of TBP and 18 μL of Li-TFSI (concentration of 520 mg / mL, solvent is anhydrous acetonitrile), mix well and dropwise add to the perovskite light absorbing layer prepared in step (3), and spin coat at 3000 rpm for 30 s to prepare a hole transport layer;
[0040] (5) In high vacuum (10 -4 At 250 Å / min, a Ag electrode with a thickness of 80 nm is deposited on the hole transport layer prepared in step (4) by thermal evaporation.
[0041] Example 1
[0042] A method for preparing a perovskite solar cell doped with a hydrazide passivating agent,
[0043] The difference from the comparative example is that in step (3), benzoyl hydrazide is added so that the concentration of benzoyl hydrazide in the perovskite precursor solution is 0.25 mg / mL.
[0044] Figure 1 The scanning electron microscope images of the perovskite film in the comparative example and Example 1 show that the morphology of the perovskite film in Example 1 is significantly improved.
[0045] Figure 2 The defect test diagrams of the perovskite film in the comparative example and Example 1 show that the defects of the perovskite film in Example 1 are significantly reduced.
[0046] Figure 3 To compare the carrier lifetime diagrams of the perovskite film in Example 1 and Example 1, it can be seen that the carrier extraction of the perovskite film in Example 1 is significantly improved.
[0047] Figure 4 For the current-voltage curves of the perovskite solar cells in the comparative example and example 1, Figure 1 It can be seen that the efficiency of the perovskite solar cell in Example 1 is significantly improved.
[0048] Example 2
[0049] The difference from Example 1 is that the concentration of the precursor solution of benzoyl hydrazide is changed to 0.015 mg / mL.
[0050] Figure 5 This is a current-voltage positive scan curve of the perovskite solar cell in Example 2. It can be seen that the efficiency of the cell is 22.02%. Compared with the efficiency of the cell in the comparative example (20.73%), the device efficiency is significantly improved.
[0051] Example 3
[0052] The difference from Example 1 is that the concentration of the precursor solution of benzoyl hydrazide is changed to 1 mg / mL.
[0053] Figure 6 This is a current-voltage positive scan curve of the perovskite solar cell in Example 3. It can be seen that the efficiency of the cell is 21.94%. Compared with the efficiency of the cell in the comparative example (20.73%), the device efficiency is significantly improved.
[0054] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A perovskite solar cell doped with a hydrazide passivating agent, characterized in that: From bottom to top, they are conductive glass, electron transport layer, perovskite light absorption layer, hole transport layer and metal back electrode, and benzoyl hydrazide is added to the perovskite light absorption layer; The conductive glass is ITO or FTO; the electron transport layer is titanium dioxide; the metal back electrode is gold, silver, copper or aluminum; The perovskite light absorbing layer is an ABX3 perovskite light absorbing layer, wherein A is CH3NH3 + or CH(NH2) 2+ One or two of the following, B is Pb 2+ , X is I - ,Br - or Cl - ; The hole transport layer is 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene; The preparation method of the perovskite solar cell doped with a hydrazide passivating agent comprises the following steps: Step 1, the conductive glass is sequentially treated with detergent, deionized water, and anhydrous ethanol, then blown dry, and then treated with ultraviolet ozone, and then taken out for use; Step 2, mixing distilled water and titanium tetrachloride to obtain a mixed solution, immersing the conductive glass treated with ozone in step 1 in the mixed solution, and then drying, taking out after drying, rinsing with distilled water, and then drying with nitrogen, annealing, to obtain an electron transport layer, and then subjecting the electron transport layer to ultraviolet ozone treatment; Step 3, dissolving the perovskite light absorbing layer material in a mixed solvent of DMF and DMSO to obtain a perovskite precursor solution, then adding benzoyl hydrazide, shaking, filtering, and then spin-coating on the electron transport layer, followed by annealing, and before the perovskite precursor solution is spin-coated, chlorobenzene is added dropwise; Step 4, dissolving the hole transport layer material in chlorobenzene, adding an anhydrous acetonitrile solution containing TBP and Li-TFSI, mixing well and spin coating the mixture on the perovskite light absorbing layer prepared in step 3 to prepare a hole transport layer; Step 5: Deposit a metal back electrode on the hole transport layer prepared in step 4 by thermal evaporation under high vacuum.
2. A method for preparing a perovskite solar cell doped with a hydrazide passivating agent according to claim 1, characterized in that: The following steps are involved: Step 1, the conductive glass is sequentially treated with detergent, deionized water, and anhydrous ethanol, then blown dry, and then treated with ultraviolet ozone, and then taken out for use; Step 2, mixing distilled water and titanium tetrachloride to obtain a mixed solution, immersing the conductive glass treated with ozone in step 1 in the mixed solution, and then drying, taking out after drying, rinsing with distilled water, and then drying with nitrogen, annealing, to obtain an electron transport layer, and then subjecting the electron transport layer to ultraviolet ozone treatment; Step 3, dissolving the perovskite light absorbing layer material in a mixed solvent of DMF and DMSO to obtain a perovskite precursor solution, then adding benzoyl hydrazide, shaking, filtering, and then spin-coating on the electron transport layer, followed by annealing, and before the perovskite precursor solution is spin-coated, chlorobenzene is added dropwise; Step 4, dissolving the hole transport layer material in chlorobenzene, adding an anhydrous acetonitrile solution containing TBP and Li-TFSI, mixing well and spin coating the mixture on the perovskite light absorbing layer prepared in step 3 to prepare a hole transport layer; Step 5: Deposit a metal back electrode on the hole transport layer prepared in step 4 by thermal evaporation under high vacuum.
3. The method for preparing a perovskite solar cell doped with a hydrazide passivating agent according to claim 2, characterized in that: In the step 1, the conductive glass is ITO or FTO, the ultrasonic treatment time is 20 minutes, and the ozone treatment time is 20 to 30 minutes.
4. The method for preparing a perovskite solar cell doped with a hydrazide passivating agent according to claim 2, characterized in that: In step 2, the volume ratio of distilled water to titanium tetrachloride is 1:1-3, the drying temperature is 75°C, the time is 45 minutes, the annealing temperature is 200°C, the time is 30 minutes, and the ozone treatment time is 20-30 minutes.
5. The method for preparing a perovskite solar cell doped with a hydrazide passivating agent according to claim 2, characterized in that: In the step 3, the perovskite light-absorbing layer materials are organic amine salts and lead halide salts, and the volume ratio of DMF to DMSO is 4:
1.
6. The method for preparing a perovskite solar cell doped with a hydrazide passivating agent according to claim 2, characterized in that: In step 3, the shaking time is 5 minutes, the spin coating speed is 4000 rpm, the time is 30 seconds, and the annealing temperature is 130° C., and the time is 28 minutes.
7. The method for preparing a perovskite solar cell doped with a hydrazide passivating agent according to claim 2, characterized in that: Benzoyl hydrazide is added in step 3 so that the concentration of the perovskite precursor solution of benzoyl hydrazide is 0.015-1 mg / mL.
8. The method for preparing a perovskite solar cell doped with a hydrazide passivating agent according to claim 2, characterized in that: In step 4, the hole transport layer material is 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, the concentration of the anhydrous acetonitrile solution of Li-TFSI is 520 mg / mL, the spin coating speed is 3000 rpm, and the time is 30 s.
9. The method for preparing a perovskite solar cell doped with a hydrazide passivating agent according to claim 2, characterized in that: In step 5, the metal back electrode is gold, silver, copper or aluminum, and the evaporation thickness is 100 nm.
Citation Information
Patent Citations
Perovskite type solar cell with sputtering ZnO as electron transfer layer and preparation
CN104319349A
Inorganic perovskite solar cell based on substituted hydrazide and preparation method thereof
CN114725289A