Neutral color low-reflective LOW-E coated glass and preparation method thereof

By introducing neutral color low-reflection LOW-E coated glass technology into low-emissivity coated glass, and using NiCrMo barrier layer and Ag+Cu functional layer, the problem of high visible light reflectivity of existing low-emissivity coated glass is solved and low reflection is achieved High efficiency and neutral transmission color, reducing light pollution and improving the look and feel.

CN115057628BActive Publication Date: 2024-10-11WUJIANG CSG HUADONG ARCHITECTURAL GLASS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210742156.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-27
Publication Date
2024-10-11
Estimated Expiration
2042-06-27

AI Technical Summary

Technical Problem

Existing low-emissivity coated glass has high visible light reflectivity, resulting in light pollution and poor visual effects.

Method used

Use neutral color low-reflective LOW-E coated glass, including glass substrate, anti-reflection film layer, two or three composite film layers and top protective layer. The composite film layer is composed of dielectric layer, seed layer, functional layer and barrier layer , using NiCrMo as a blocking layer to reduce visible light reflectivity and adjust the transmitted color.

Benefits of technology

It effectively reduces the visible light reflectance of coated glass, provides neutral transmission color, enhances the toughness and hardness of the film layer, reduces light pollution, and improves the realism of observing outdoor scenes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a neutral-color, low-reflection (LOW-E) coated glass and its preparation method. The coated glass includes a glass substrate and, from the inside out, an anti-reflection film layer, two or three composite film layers, and a top protective layer, sequentially deposited on one side surface of the glass substrate. Each composite film layer includes a dielectric layer, a seed layer, a functional layer, and a barrier layer, sequentially arranged. The anti-reflection film layer is adjacent to the dielectric layer of the adjacent composite film layer, and the barrier layer of the adjacent composite film layer is adjacent to the dielectric layer of the adjacent composite film layer. The top protective layer is adjacent to the barrier layer of the adjacent composite film layer. The barrier layer is a NiCrMo layer or a NiCr layer, and at least one composite film layer has a NiCrMo layer as its barrier layer. The coated glass provided by this invention, by adding an anti-reflection film layer, achieves extremely low visible light reflectivity, and by using NiCrMo as the barrier layer of the functional layer, the coated glass exhibits a relatively neutral color transmittance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coated glass, and in particular relates to a neutral color low-reflective LOW-E coated glass and a preparation method thereof. Background Art

[0002] As an energy-saving building material, in the existing technology, low-emissivity coated glass generally refers to a low-emissivity functional layer deposited on the surface of float glass, thereby reflecting near-infrared rays in sunlight and far-infrared rays in the living environment, thereby reducing the glass's absorption and radiation of infrared rays, so it is called low-emissivity coated glass.

[0003] Low-E coated glass can be used for home doors and windows, as well as glass curtain walls of shopping malls, office buildings, high-end hotels and other places where it is needed. With the large-scale use of traditional low-E coated glass, "light pollution" has become an urgent problem that troubles urban residents due to its high reflectivity of visible light. In order to reduce the "light pollution" phenomenon caused by the large-scale use of glass curtain walls, local governments have issued policies and regulations to restrict the external reflection of architectural glass.

[0004] The existing low-emissivity coated glass has the following disadvantages: 1. The visible light reflectivity is high, which easily causes light pollution; 2. The product has color difference in transmission, which affects people's visual effects. Summary of the invention

[0005] The purpose of the present invention is to provide a neutral color low-reflection LOW-E coated glass and a preparation method thereof, so as to solve the problem that the existing coated glass has a high visible light reflectivity, a product transmission color difference, and affects the visual effect.

[0006] In order to achieve the above object, a technical solution adopted by the present invention is:

[0007] A neutral color low-reflection LOW-E coated glass, the neutral color low-reflection LOW-E coated glass comprises a glass substrate and an anti-reflection film layer, two or three composite film layers, and a top protective layer coated on a surface of one side of the glass substrate from the inside to the outside, each of the composite film layers comprises a dielectric layer, a seed layer, a functional layer, and a barrier layer arranged in sequence, the anti-reflection film layer is adjacent to the dielectric layer of the composite film layer adjacent to it, the barrier layer of the composite film layer adjacent to the anti-reflection film layer is adjacent to the dielectric layer of the composite film layer adjacent to it, the top protective layer is adjacent to the barrier layer of the composite film layer adjacent to it, the barrier layer is a NiCrMo layer or a NiCr layer, and the barrier layer of at least one of the composite film layers is a NiCrMo layer.

[0008] Preferably, the thickness of the barrier layer of at least one of the composite film layers is greater than or equal to 1 nm.

[0009] Preferably, the anti-reflection film layer is a NiCr layer.

[0010] Preferably, the functional layer is an Ag layer or an Ag+Cu layer; if the functional layer is an Ag+Cu layer, the Ag layer is adjacent to the seed layer of the adjacent composite film layer, and the Cu layer is adjacent to the barrier layer of the adjacent composite film layer.

[0011] Preferably, the dielectric layer and the top protective layer are a combination of one or more layers of a SiNx layer, a SiOx layer, a SiNxOy layer, and a TiOx layer.

[0012] Preferably, the seed layer is one of a ZnOx layer and a ZnSnOx layer, or a combination of two layers.

[0013] Preferably, two composite film layers are provided, the composite film layer adjacent to the anti-reflection film layer includes a first dielectric layer, a first seed layer, a first functional layer, and a first barrier layer, and the composite film layer adjacent to the top protective layer includes a second dielectric layer, a second seed layer, a second functional layer, and a second barrier layer. The anti-reflection film layer, the first dielectric layer, the first seed layer, the first functional layer, the first barrier layer, the second dielectric layer, the second seed layer, the second functional layer, the second barrier layer, and the top protective layer are deposited in sequence from the inside to the outside on the surface of one side of the glass substrate.

[0014] Preferably, the composite film layer is set to three, the composite film layer adjacent to the anti-reflection film layer includes a first dielectric layer, a first seed layer, a first functional layer, and a first barrier layer, the middle composite film layer located between the two composite film layers includes a second dielectric layer, a second seed layer, a second functional layer, and a second barrier layer, the composite film layer adjacent to the top protective layer includes a third dielectric layer, a third seed layer, a third functional layer, and a third barrier layer, and the anti-reflection film layer, the first dielectric layer, the first seed layer, the first functional layer, the first barrier layer, the second dielectric layer, the second seed layer, the second functional layer, the second barrier layer, the third dielectric layer, the third seed layer, the third functional layer, the third barrier layer, and the top protective layer are deposited in sequence from the inside to the outside on the surface of one side of the glass substrate.

[0015] Preferably, in each of the composite film layers, the thickness of the functional layer is greater than or equal to 7 and less than or equal to 16 nm; if the functional layer is an Ag+Cu layer, the thickness of the Cu layer is greater than or equal to 5 and less than 7 nm; the thickness of the barrier layer is greater than 0 and less than or equal to 4 nm; the thickness of the anti-reflection film layer is greater than 1.3 and less than or equal to 3 nm; the thickness of the dielectric layer ranges from 28 to 70 nm; the thickness of the top protective layer ranges from 25 to 43 nm; and the thickness of the seed layer ranges from 5 to 10 nm.

[0016] Another object of the present invention is to provide a method for preparing the neutral color low-reflection LOW-E coated glass, which comprises the following steps: adopting a magnetron sputtering coating method to sequentially coat an anti-reflection film layer, a composite film layer, and a top protective layer on one side surface of a glass substrate, wherein two or three composite film layers are arranged, and the composite film layer comprises a dielectric layer, a seed layer, a functional layer, and a barrier layer arranged in sequence; when coating the composite layer, the anti-reflection film layer is adjacent to the dielectric layer of the composite film layer adjacent to it, the functional layer of the composite film layer adjacent to the anti-reflection film layer is adjacent to the barrier layer of the composite film layer adjacent to it, and the top protective layer is adjacent to the barrier layer of the composite film layer adjacent to it.

[0017] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0018] The neutral color low-reflection LOW-E coated glass provided by the present invention has an anti-reflection film layer added so that the coated glass can have an extremely low visible light reflectivity, and uses NiCrMo as a barrier layer of the functional layer, so that the coated glass has a relatively neutral transmission color, and a more realistic viewing experience is obtained when observing outdoor scenery from indoors; the visible light transmittance of the entire film system can be flexibly adjusted by adjusting the thickness of the barrier layer, and the neutrality of the transmission color of the glass product can be maintained to the maximum extent. The perspective color adjustment range of the glass product is wide, which can meet the requirements of customers in different regions; NiCrMo as a barrier layer can increase the toughness and hardness of the film layer, and prevent the coated layer from defects such as scratches, wear, corrosion and oxidation. DETAILED DESCRIPTION

[0019] The present invention is further described below in conjunction with the illustrated embodiments.

[0020] Neutral color low-reflection LOW-E coated glass comprises a glass substrate and an anti-reflection film layer, two or three composite film layers, and a top protective layer which are sequentially coated on a surface of one side of the glass substrate from the inside to the outside, wherein each composite film layer comprises a dielectric layer, a seed layer, a functional layer, and a barrier layer which are sequentially arranged, the anti-reflection film layer is adjacent to the dielectric layer of the composite film layer adjacent thereto, the barrier layer of the composite film layer adjacent to the anti-reflection film layer is adjacent to the dielectric layer of the composite film layer adjacent thereto, and the top protective layer is adjacent to the barrier layer of the composite film layer adjacent thereto, wherein:

[0021] The main component of the anti-reflection film layer is NiCr, which has high visible light absorption capacity, high hardness, strong wear resistance and chemical stability. It provides strong anti-reflection ability while having a strong protective effect on the film layer. NiCr has good adhesion to glass and good adhesion to the dielectric layer.

[0022] The barrier layer is a NiCrMo layer or a NiCr layer, and the barrier layer of at least one composite film layer is a NiCrMo layer. The barrier layer material NiCrMo is used to make the glass product's transmittance color neutral. The transmittance of the glass product can be adjusted by adjusting its thickness, thereby maximizing the neutrality of the glass product's transmittance color and obtaining a more realistic viewing experience when observing outdoor scenery from indoors; it can also protect the functional layer from damage during thermal processing.

[0023] Conventional double-silver and triple-silver coated glass uses NiCr as a barrier layer to adjust the light transmittance of the product. However, due to the inherent properties of the NiCr film material, the perspective color is greenish, and there has been no new material to replace this defective barrier layer material for a long time, so it has been used.

[0024] If two composite film layers are provided, the barrier layer in one of the two composite film layers is a NiCrMo layer, or the barrier layers in both composite film layers are NiCrMo layers. If three composite film layers are provided, the barrier layer in one composite film layer is a NiCrMo layer, or the barrier layers in both composite film layers are NiCrMo layers, or the barrier layers in all three composite film layers are NiCrMo layers.

[0025] The advantage of NiCrMo over NiCr is that adding Mo to the alloy can improve the product's transparent color. The advantage of NiCrMo over a single Mo layer is that the alloy can increase the toughness and hardness of the film, and its main function is to prevent defects such as scratches, wear, corrosion and oxidation on the coated film.

[0026] Among them, the thickness of the barrier layer of at least one composite film layer is greater than or equal to 1nm. If the barrier layer is too thin, the light transmittance of the product is relatively high, and the reflection of the matching film has a greater impact on the overall outdoor reflection of the product, which is not conducive to reducing the reflectivity of the product.

[0027] The dielectric layer is a combination of one or more layers of a SiNx layer, a SiOx layer, a SiNxOy layer, and a TiOx layer, with the SiNx layer being the best. SiNx has good bonding properties with glass, and has strong resistance to corrosion, mechanical scratches, and high-temperature oxidation. It is a super-strength and super-hardness material with excellent chemical stability. It can improve the adhesion of the functional silver layer to the glass surface, protect the functional silver layer, adjust the color, and improve the hardness of the film system, and can improve the mechanical processing performance of the film layer.

[0028] The seed layer is a combination of one or two layers of ZnOx layer and ZnSnOx layer, with ZnOx being the best. Using ZnOx as the seed layer can improve the flatness of the film layer, provide a clean surface without pollution for the functional layer, increase the adhesion of the functional layer metal in the film layer, and enable it to perform better.

[0029] The functional layer is an Ag layer or an Ag+Cu layer. Metal Ag has very good conductivity, which can reduce the surface resistance and emissivity of the entire film layer, and also plays a role in adjusting the color and performance of the film layer. If the functional layer is an Ag+Cu layer, the Ag layer is adjacent to the seed layer of the adjacent composite film layer, and the Cu layer is adjacent to the barrier layer of the adjacent composite film layer.

[0030] The top protective layer is a combination of one or more layers of SiNx layer, SiOx layer, SiNxOy layer and TiOx layer, with SiNx layer being the best and having strong corrosion resistance, mechanical scratch resistance and high temperature oxidation resistance.

[0031] The thickness ranges of the above film layers are as follows: in each composite film layer, the thickness of the anti-reflection film layer is greater than 1.3 and less than or equal to 3nm; the thickness range of the dielectric layer is 28-70nm; the thickness range of the seed layer is 5-10nm; the thickness of the functional layer is greater than or equal to 7 and less than or equal to 16nm; the thickness of the barrier layer is greater than 0 and less than or equal to 4nm; the thickness range of the top protective layer is 25-43nm.

[0032] According to different requirements for transmittance color, two or three composite film layers can be provided. When two composite film layers are provided, one side surface of the glass substrate of the neutral color low-reflection LOW-E coated glass is coated with an anti-reflection film layer, two composite film layers, and a top protective layer in sequence from inside to outside. One composite film layer includes a first dielectric layer, a first seed layer, a first functional layer, and a first barrier layer. The other composite film layer includes a second dielectric layer, a second seed layer, a second functional layer, and a second barrier layer. The anti-reflection film layer, the first dielectric layer, the first seed layer, the first functional layer, the first barrier layer, the second dielectric layer, the second seed layer, the second functional layer, the second barrier layer, and the top protective layer are deposited in sequence from inside to outside on the glass substrate. Specifically:

[0033] The thickness of the anti-reflection film layer is greater than 1.3 and less than or equal to 3nm; the thickness range of the first dielectric layer is 28 to 35nm; the thickness range of the first seed layer is 5 to 8nm; the first functional layer is an Ag layer or an Ag+Cu layer; the thickness range of the first barrier layer is 0 to 2nm; the thickness range of the second dielectric layer is 43 to 70nm; the thickness range of the second seed layer is 5 to 10nm; the second functional layer is an Ag layer or an Ag+Cu layer; the thickness range of the second barrier layer is 0 to 4nm; the thickness range of the top protective layer is 25 to 43nm.

[0034] The first functional layer is an Ag layer or an Ag+Cu layer, and the film thickness is greater than or equal to 7 and less than or equal to 16nm. If the functional layer is an Ag+Cu layer, the Ag layer is adjacent to the seed layer of the adjacent composite film layer, and the Cu layer is adjacent to the barrier layer of the adjacent composite film layer, that is, the Ag layer and the Cu layer are plated in sequence, and at this time, the thickness of the Cu layer is greater than or equal to 5 and less than 7nm; the second functional layer is an Ag layer or an Ag+Cu layer, and the film thickness ranges from 10 to 15nm. If the functional layer is an Ag+Cu layer, the Ag layer is adjacent to the seed layer of the adjacent composite film layer, and the Cu layer is adjacent to the barrier layer of the adjacent composite film layer, that is, the Ag layer and the Cu layer are plated in sequence, and at this time, the thickness of the Cu layer ranges from 5 to 7nm.

[0035] When three composite film layers are provided, one side surface of the glass substrate of the neutral color low-reflection LOW-E coated glass is coated with an anti-reflection film layer, three composite film layers, and a top protective layer in sequence from the inside to the outside, the composite film layer adjacent to the anti-reflection film layer includes a first dielectric layer, a first seed layer, a first functional layer, and a first barrier layer, the middle composite film layer located between the two composite film layers includes a second dielectric layer, a second seed layer, a second functional layer, and a second barrier layer, the composite film layer adjacent to the top protective layer includes a third dielectric layer, a third seed layer, a third functional layer, and a third barrier layer, the anti-reflection film layer, the first dielectric layer, the first seed layer, the first functional layer, the first barrier layer, the second dielectric layer, the second seed layer, the second functional layer, the second barrier layer, the third dielectric layer, the third seed layer, the third functional layer, the third barrier layer, and the top protective layer are deposited in sequence from the inside to the outside on the glass substrate.

[0036] The thickness range of the anti-reflection film layer is 1.3 to 3nm; the thickness range of the first dielectric layer is 28 to 35nm; the thickness range of the first seed layer is 5 to 8nm; the first functional layer is an Ag layer or an Ag+Cu layer; the thickness range of the first barrier layer is 0 to 2nm; the thickness range of the second dielectric layer is 43 to 70nm; the thickness range of the second seed layer is 5 to 10nm; the second functional layer is an Ag layer or an Ag+Cu layer; the thickness range of the second barrier layer is 0 to 4nm; the thickness range of the third dielectric layer is 25 to 43nm; the thickness range of the third seed layer is 5 to 8nm, the thickness range of the third functional layer is 12 to 17nm, the thickness range of the third barrier layer is 0 to 2nm, and the thickness range of the top protective layer is 25-43nm.

[0037] The following is a specific description using two or three composite membrane layers as an example, see Example 1-2.

[0038] Example 1

[0039] Two composite film layers are provided. The neutral color low-reflection LOW-E coated glass includes a glass substrate and an anti-reflection film layer, two composite film layers, and a top protective layer, which are sequentially coated on the surface of one side of the glass substrate from the inside to the outside. Among them, the anti-reflection film layer is a NiCr layer with a film thickness of 1.3nm; the first dielectric layer is a SiNx layer with a film thickness of 29.5nm; the first seed layer is a ZnOx layer with a film thickness of 7nm; the first functional layer is an Ag+Cu layer with a film thickness of 7nm+5.2nm; the first barrier layer is a NiCrMo layer with a film thickness of 1.5nm; the second dielectric layer is a SiNx layer with a film thickness of 49nm; the second seed layer is a ZnOx layer with a film thickness of 7nm; the second functional layer is an Ag layer with a film thickness of 11.2nm; the second barrier layer is a NiCrMo layer with a film thickness of 2.7nm; and the top protective layer is a SiNx layer with a film thickness of 35.5nm.

[0040] The standard hollow outdoor reflectivity and transmittance color data of the coated glass product provided in this embodiment are as follows:

[0041] Table 1 Outdoor reflectance and transmittance data of Example 1

[0042] Outdoor reflectivity Light transmittance Transmittance color a* Transmittance b* Standard hollow 7% 48% -1.1 0.8

[0043] It can be seen from Table 1 that the reflectivity of the coated glass product shown in this embodiment is as low as 7%, and the transmitted color is neutral, which is close to the natural color.

[0044] Comparative Example 1

[0045] The difference from Example 1 is that this example does not have an anti-reflection film layer.

[0046] In this example, the specific film structure and thickness are:

[0047] The first dielectric layer is a SiNx layer with a thickness of 29.5nm; the first seed layer is a ZnOx layer with a thickness of 7nm; the first functional layer is an Ag+Cu layer with a thickness of 7nm+5.2nm; the first barrier layer is a NiCrMo layer with a thickness of 1.5nm; the second dielectric layer is a SiNx layer with a thickness of 49nm; the second seed layer is a ZnOx layer with a thickness of 7nm; the second functional layer is an Ag layer with a thickness of 11.2nm; the second barrier layer is a NiCrMo layer with a thickness of 2.7nm; and the top protective layer is a SiNx layer with a thickness of 35.5nm.

[0048] The standard hollow outdoor reflectivity and transmittance color data of the coated glass products provided in this example are as follows:

[0049] Table 2 Outdoor reflectance and transmittance data of comparative examples

[0050] Outdoor reflectivity Light transmittance Transmittance color a* Transmittance b* Standard hollow 9% 52% -0.8 1.5

[0051] It can be seen from Table 1 and Table 2 that the outdoor reflectivity of the coated glass of Example 1 is lower than that of the coated glass of the comparative example, and the anti-reflection film layer NiCr layer of Example 1 can effectively reduce the outdoor reflectivity of the glass product.

[0052] Comparative Example 2

[0053] The difference from Example 1 is that the first barrier layer and the second barrier layer are both NiCr layers.

[0054] In this example, the specific film structure and thickness are:

[0055] The anti-reflection film layer is a NiCr layer with a thickness of 1.3nm; the first dielectric layer is a SiNx layer with a thickness of 29.5nm; the first seed layer is a ZnOx layer with a thickness of 7nm; the first functional layer is an Ag+Cu layer with a thickness of 7nm and a Cu layer thickness of 5.2nm; the first barrier layer is a NiCr layer with a thickness of 1.5nm; the second dielectric layer is a SiNx layer with a thickness of 49nm; the second seed layer is a ZnOx layer with a thickness of 7nm; the second functional layer is an Ag layer with a thickness of 11.2nm; the second barrier layer is a NiCr layer with a thickness of 2.7nm; and the top protective layer is a SiNx layer with a thickness of 35.5nm.

[0056] The standard hollow outdoor reflectivity and transmittance color data of the coated glass products provided in this example are as follows:

[0057] Outdoor reflectivity Light transmittance Transmittance color a* Transmittance b* Standard hollow 7% 46% -2.5 -1

[0058] From the comparison between Example 1 and Comparative Example 2, it can be seen that the use of the NiCrMo layer in the barrier layer in Example 1 can effectively improve the transmittance color of the product.

[0059] Example 2

[0060] There are three composite film layers. The neutral color low-reflection LOW-E coated glass includes a glass substrate and an anti-reflection film layer, three composite film layers, and a top protective layer coated on the surface of one side of the glass substrate from the inside to the outside. The specific film layer structure and thickness are as follows: the anti-reflection film layer is a NiCr layer with a film thickness of 1.3nm; the first dielectric layer is a SiNx layer with a film thickness of 24.5nm; the first seed layer is a ZnOx layer with a film thickness of 7nm; the first functional layer is an Ag layer with a film thickness of 8.1nm; the first barrier layer is a NiCrMo layer with a film thickness of 0.8nm; the second dielectric layer is a Si Nx layer, the film thickness is 61nm; the second seed layer is ZnOx layer, the film thickness is 7nm; the second functional layer is Ag+Cu layer, the film thickness is 7nm+4.6nm; the second barrier layer is NiCrMo layer, the film thickness is 1.3nm; the third dielectric layer is SiNx layer, the film thickness is 66nm; the third seed layer is ZnOx layer, the film thickness is 7nm; the third functional layer is Ag layer, the film thickness is 12.6nm; the third barrier layer is NiCrMo layer, the film thickness is 2.1nm; the top protective layer is SiNx layer, the film thickness is 28.6nm.

[0061] The standard hollow outdoor reflectivity and transmittance color data of the coated glass products provided in this example are as follows:

[0062] Outdoor reflectivity Light transmittance Transmittance color a* Transmittance b* Standard hollow 7% 49% -1.1 -0.8

[0063] The present invention also provides a method for preparing neutral color low-reflection LOW-E coated glass, which comprises the following steps:

[0064] An anti-reflection film layer, a composite film layer, and a top protective layer are sequentially plated on the inner surface of a glass substrate by magnetron sputtering coating, wherein the composite film layer comprises a dielectric layer, a seed layer, a functional layer, and a barrier layer which are sequentially arranged, and two or three composite film layers are arranged. When coating the composite layer, the anti-reflection film layer is adjacent to the dielectric layer of the composite film layer adjacent thereto, the functional layer of the composite film layer adjacent to the anti-reflection film layer is adjacent to the barrier layer of the composite film layer adjacent thereto, and the top protective layer is adjacent to the barrier layer of the composite film layer adjacent thereto.

[0065] Taking the preparation of the neutral color low-reflection LOW-E coated glass of Example 1 as an example, the preparation method is specifically described, which includes the following steps:

[0066] 1. Clean and dry the glass substrate to be coated;

[0067] 2. Vacuum transition;

[0068] 3. The following sputtering layers are formed in sequence by vacuum magnetron sputtering from the glass substrate outwards. The specific sputtering method is as follows:

[0069] S1: The anti-reflection film layer is a NiCr layer, which is sputtered by magnetron sputtering technology, and the film thickness ranges from 0 to 2nm;

[0070] S2: The first dielectric layer is a SiNx layer, which is sputtered by a magnetron sputtering process, and the film thickness ranges from 28 to 35 nm;

[0071] S3: The first seed layer is a ZnOx layer, which is sputtered by a magnetron sputtering process, and the film thickness ranges from 5 to 8 nm;

[0072] S4: The first functional layer is an Ag+Cu layer (filmed in sequence), which is sputtered by a magnetron sputtering process, and the total film thickness ranges from 7 to 16 nm, wherein the thickness range of the Cu layer is from 5 to 7 nm;

[0073] S5: The first barrier layer is a NiCrMo layer, which is sputtered by a magnetron sputtering process, and the film thickness ranges from 0 to 2 nm;

[0074] S6: The second dielectric layer is a SiNx layer, which is sputtered by a magnetron sputtering process, and the film thickness ranges from 43 to 70 nm;

[0075] S7: The second seed layer is a ZnOx layer, which is sputtered by a magnetron sputtering process, and the film thickness ranges from 5 to 10 nm;

[0076] S8: The second functional layer is an Ag layer, which is sputtered by magnetron sputtering process, and the film thickness ranges from 10 to 15 nm;

[0077] S9: The second barrier layer is a NiCrMo layer, which is sputtered by a magnetron sputtering process, and the film thickness ranges from 0 to 4 nm;

[0078] S10: The top protective layer is a SiNx layer, which is sputtered using a magnetron sputtering process, and the film thickness ranges from 25 to 43 nm;

[0079] The sputtering method of the anti-reflection film layer in step S1 is: using a direct current power supply, using a NiCr target material with a target material purity greater than 99.99%, and performing sputtering in pure argon working gas.

[0080] The sputtering methods of the first dielectric layer, the second dielectric layer, and the top protective layer in steps S2, S6, and S10 all adopt: using an AC medium frequency power supply, using a target material of SiAl target or a pure Si target, and the target purity is greater than 99.7% (if a SiAl target is used, the Al content in the SiAl target is 8 to 15wt%, and the main function of the Al doped in the SiAl material is to increase the conductivity of the film material), and sputtering in a mixed gas of argon and nitrogen.

[0081] The sputtering method of the first seed layer and the second seed layer in steps S3 and S7 is: using an AC medium frequency power supply, using a ZnAl target with a target purity greater than 99.8% and an Al content of 1.5-2.5wt%, and sputtering in a mixed gas of argon and oxygen.

[0082] The sputtering method of the first functional layer and the second functional layer in steps S4 and S8 is: using a DC power supply, using a target material of Ag+Cu target or Ag target, the purity of the target material is greater than 99.99%, and sputtering is performed in pure argon working gas.

[0083] The sputtering method of the first barrier layer and the second barrier layer in steps S5 and S9 is: using a direct current power supply, using a NiCrMo target with a target purity greater than 99.9%, and performing sputtering in pure argon working gas. The thickness of at least one of the first barrier layer and the second barrier layer is greater than or equal to 1 nm.

[0084] If the first barrier layer and the second barrier layer are NiCr layers, a NiCr target is used, the target purity is greater than 99.9%, and sputtering is performed in pure argon working gas.

[0085] In the neutral color low-reflection LOW-E coated glass provided by the present invention, NiCrMo is used as a barrier layer of the low-radiation glass, and the produced product has the advantage of a wide range of perspective color adjustment, and can even achieve the purpose of neutrality of the perspective color without using Cu with slightly poor processing resistance, so as to obtain a more realistic viewing experience when observing outdoor scenery from indoors; NiCr is used as an anti-reflection film layer, and the material has a relatively high visible light absorption capacity, high hardness, strong wear resistance and chemical stability, and provides a relatively strong anti-reflection capacity while having a relatively strong protective effect on the film layer, and NiCr can have good adhesion to the glass and the dielectric layer used.

[0086] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A neutral color low-reflective LOW-E coated glass, characterized by: The neutral color low-reflection LOW-E coated glass comprises a glass substrate and an anti-reflection film layer, two or three composite film layers, and a top protective layer which are sequentially coated on the surface of one side of the glass substrate from the inside to the outside, each of the composite film layers comprises a dielectric layer, a seed layer, a functional layer, and a barrier layer which are sequentially arranged, the anti-reflection film layer is adjacent to the dielectric layer of the composite film layer adjacent thereto, the barrier layer of the composite film layer adjacent to the anti-reflection film layer is adjacent to the dielectric layer of the composite film layer adjacent thereto, the top protective layer is adjacent to the barrier layer of the composite film layer adjacent thereto, the barrier layer is a NiCrMo layer; the anti-reflection film layer is a NiCr layer; The functional layer is an Ag layer or an Ag+Cu layer; if the functional layer is an Ag+Cu layer, the Ag layer is adjacent to the seed layer of the adjacent composite film layer, and the Cu layer is adjacent to the barrier layer of the adjacent composite film layer; The dielectric layer and the top protective layer are a combination of one or more layers of a SiNx layer, a SiOx layer, a SiNxOy layer, and a TiOx layer; The seed layer is one layer of a ZnOx layer or a ZnSnOx layer or a combination of two layers; In each of the composite film layers, the thickness of the functional layer is greater than or equal to 7 and less than or equal to 16 nm; if the functional layer is an Ag+Cu layer, the thickness of the Cu layer is greater than or equal to 5 and less than 7 nm; the thickness of the anti-reflection film layer is greater than 1.3 and less than or equal to 3 nm; the thickness of the dielectric layer ranges from 28 to 70 nm; the thickness of the seed layer ranges from 5 to 10 nm; the thickness of the barrier layer is greater than or equal to 1 and less than or equal to 4 nm; the thickness of the top protective layer ranges from 25 to 43 nm.

2. The neutral color low-reflection LOW-E coated glass according to claim 1, characterized in that: The composite film layer is provided with two, the composite film layer adjacent to the anti-reflection film layer includes a first dielectric layer, a first seed layer, a first functional layer, and a first barrier layer, and the composite film layer adjacent to the top protective layer includes a second dielectric layer, a second seed layer, a second functional layer, and a second barrier layer. The anti-reflection film layer, the first dielectric layer, the first seed layer, the first functional layer, the first barrier layer, the second dielectric layer, the second seed layer, the second functional layer, the second barrier layer, and the top protective layer are deposited in sequence from the inside to the outside on the surface of one side of the glass substrate.

3. The neutral color low-reflective LOW-E coated glass according to claim 1, characterized in that: The number of the composite film layers is three, the composite film layer adjacent to the anti-reflection film layer includes a first dielectric layer, a first seed layer, a first functional layer, and a first barrier layer, the middle composite film layer between the two composite film layers includes a second dielectric layer, a second seed layer, a second functional layer, and a second barrier layer, the composite film layer adjacent to the top protective layer includes a third dielectric layer, a third seed layer, a third functional layer, and a third barrier layer, the anti-reflection film layer, the first dielectric layer, the first seed layer, the first functional layer, the first barrier layer, the second dielectric layer, the second seed layer, the second functional layer, the second barrier layer, the third dielectric layer, the third seed layer, the third functional layer, the third barrier layer, and the top protective layer are sequentially deposited on the surface of one side of the glass substrate from the inside to the outside.

4. A method for preparing the neutral color low-reflection LOW-E coated glass according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: adopting a magnetron sputtering coating method to sequentially coat an anti-reflection film layer, a composite film layer, and a top protective layer on one side surface of a glass substrate, wherein two or three composite film layers are arranged, and the composite film layers comprise a dielectric layer, a seed layer, a functional layer, and a barrier layer arranged in sequence; when coating the composite layer, the anti-reflection film layer is adjacent to the dielectric layer of the composite film layer adjacent to it, the functional layer of the composite film layer adjacent to the anti-reflection film layer is adjacent to the barrier layer of the composite film layer adjacent to it, and the top protective layer is adjacent to the barrier layer of the composite film layer adjacent to it.