A high entropy layered metal oxide and its preparation method and application

Through the preparation of high-entropy layered metal oxides, the problem of limited performance of the cathode material of sodium ion battery is solved, and high cycle stability and electrochemical performance are improved, which is suitable for the application of sodium ion battery.

CN115064657BActive Publication Date: 2024-11-08SHENZHEN JINGONG ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210727547.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-24
Publication Date
2024-11-08
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

The specific capacity, energy density and rate performance of the positive electrode material of sodium ion battery are limited, especially the irreversible phase change of layered oxides and air sensitivity limit their development.

Method used

Using high-entropy layered metal oxides, including at least 5 metal elements such as Li+, Cu2+, Ni2+, Ni3+, Co3+, Fe3+, Al3+, Mn3+, Mn4+, Ti4+, Sn4+, Sb5+, etc., O3 or P2 phase is prepared by high-temperature sintering. Metal oxides of structures are used as the positive electrode material for sodium ion batteries, combined with ball milling and pressing processes to improve structural stability.

Benefits of technology

It significantly improves the cycle stability and electrochemical performance of sodium ion batteries, improves specific capacity and energy density, reduces voltage hysteresis, and is suitable for fields such as 3C products and electric vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115064657B_ABST
    Figure CN115064657B_ABST
Patent Text Reader

Abstract

The present invention provides a high entropy layered metal oxide and a preparation method and application thereof. The metal oxide comprises Li + , Cu 2+ 、Ni 2+ 、Ni 3+ 、Co 3+ , Fe 3+ 、Al 3+ , Mn 3+ , Mn 4+ 、Ti 4+ Sn 4+ , Sb 5+ At least 5 of the above, the molecular formula of the metal oxide is: Na x Li y Cu z Ni a Co b Fe c Al d Mn e Ti f Sn g Sb k , wherein 0.5≤x≤1, 0≤y, z, a, b, c, d, e, f, g, k≤0.2, and the number of atoms of each metal element accounts for 5-35% of the total number of metal atoms, and the metal oxide is an O3 or P2 phase oxide. When used as a positive electrode material in a sodium ion battery, it can provide a higher specific capacity and energy density, and has excellent cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of positive electrode materials, and more specifically, to a high-entropy layered metal oxide and a preparation method and application thereof. Background Art

[0002] With the rapid development of information technology, the production and utilization of energy plays a vital role in maintaining the normal operation of modern society. With the continuous consumption of fossil fuels and the increasing environmental problems, people's demand for renewable clean energy such as wind energy, solar energy and tidal energy is growing rapidly. In order to integrate these intermittent and regional energy sources into large-scale power grids that can be applied in practice, cheap and efficient energy storage systems are extremely important in fully storing peak and valley energy and releasing it during peak periods. Since being commercialized by Sony in 1991, lithium-ion batteries have achieved great success in the portable electronics and electric vehicle markets, and have also attracted attention for their sustainable development characteristics in the scale of power grids. However, limited lithium resources, especially my country's current lack of lithium resources and extreme dependence on imports, have restricted the further development of lithium-ion batteries. Compared with lithium, the abundant reserves of sodium resources in the earth's crust lead to low prices for sodium-based raw materials (the cost of Na2CO3 is about 25-30 times lower than that of Li2CO3); the similar physical and chemical properties to lithium and the "rocking chair" working principle similar to lithium-ion batteries enable sodium-ion batteries to fully learn from the mature methods and processes of lithium-ion batteries for development. The specific capacity, energy density and rate performance of current sodium-ion batteries are mainly limited by the positive electrode material. How to prepare a low-cost, high-energy-density and high-power-density sodium-ion positive electrode material is the main problem currently faced.

[0003] Among all the cathode materials for sodium-ion batteries, layered oxides have become one of the most promising cathode materials due to their high specific capacity, simple synthesis method and strong plasticity. However, their irreversible phase transition, rapid capacity decay and air sensitivity limit their development and application. Summary of the invention

[0004] Based on the above technical problems existing in the prior art, one of the purposes of the present invention is to provide a high entropy layered metal oxide, which is an O3 or P2 phase layered oxide, and the space groups correspond to Or P63 / mmc type structure, it can be used as a positive electrode material for sodium ion batteries and has excellent cycle stability.

[0005] In order to achieve the above object, the technical solution of the present invention is:

[0006] A sodium ion high entropy layered metal oxide comprising Li + , Cu 2+ 、Ni 2+、Ni 3+ 、Co 3+ , Fe 3+ 、Al 3+ , Mn 3+ , Mn 4+ 、Ti 4+ Sn 4+ , Sb 5+ At least 5 of the above, the molecular formula of the metal oxide is: Na x Li y Cu z Ni a Co b Fe c Al d Mn e Ti f Sn g Sb k , wherein 0.5≤x≤1, 0≤y,z,a,b,c,d,e,f,g,k≤0.2, and the number of atoms of each metal element accounts for 5-35% of the total number of metal atoms, and the metal oxide is an O3 or P2 phase oxide.

[0007] Among them, the 0≤y, z, a, b, c, d, e, f, g, k≤0.2 specifically refers to 0≤y≤0.2, 0≤z≤0.2, 0≤a≤0.2, 0≤b≤0.2, 0≤c≤0.2, 0≤d≤0.2, 0≤e≤0.2, 0≤f≤0.2, 0≤g≤0.2, and 0≤k≤0.2.

[0008] In some embodiments, the metal oxide has the molecular formula: Na 0.73 (CuNiFeMnTiSb) 1 / 6 O2、Na 0.76 (Ni 0.12 Cu 0.12 Fe 0.18 Co 0.18 Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 )O2、Na 0.88 (Ni 0.18 Cu 0.18 Fe 0.12 Al 0.12 Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 )O2、Na(LiNiCoMnTiSn) 1 / 6 O2、Na 0.6 (CuNiMnTiSb) 0.2 O2、Na0.6 (LiCoMnTiSb) 0.2 O2 or Na 0.6 (LiNiMnTiSb) 0.2 O2.

[0009] The second object of the present invention is to provide a method for preparing the sodium ion high entropy layered metal oxide according to any of the above embodiments, the preparation method comprising the following steps:

[0010] S1, mixing at least five metal compounds and a sodium source in a stoichiometric ratio in a volatile organic solvent by ball milling, and drying to obtain a precursor powder;

[0011] S2, sintering the precursor powder at high temperature in air, then cooling and grinding to obtain the metal oxide;

[0012] Wherein, the metal compound is Li + , Cu 2+ 、Ni 2+ 、Ni 3+ 、Co 3+ , Fe 3+ 、Al 3+ , Mn 3+ , Mn 4+ 、Ti 4+ Sn 4+ , Sb 5+ of compounds.

[0013] In some embodiments, in step S1, a sodium source with a desired stoichiometric amount of 100 wt% to 110 wt% is mixed with the metal compound; if the metal compound contains Li + , then add 100wt% to 110wt% of a lithium-containing compound.

[0014] In some embodiments, the metal compound includes at least one of metal oxides, chlorides, nitrates, sulfates, and carbonates; and the sodium source is at least one of sodium carbonate, sodium nitrate, sodium oxide, sodium chloride, and sodium sulfate.

[0015] In some embodiments, the volatile organic solvent is an alcohol organic solvent, including but not limited to ethanol, isopropanol, etc.

[0016] In some embodiments, in step S2, sintering is performed at 800-1000°C for 6-24 hours. Specifically, the temperature is increased to 800-1000°C at a heating rate of 3°C / min.

[0017] In some embodiments, before sintering, the method further includes pressing the precursor powder into a round piece under a pressure of 10 MPa.

[0018] A third object of the present invention is to provide a positive electrode material, wherein the positive electrode material comprises the sodium ion high entropy layered metal oxide described in any of the above embodiments.

[0019] A fourth object of the present invention is to provide a positive electrode plate, wherein the positive electrode plate comprises the above-mentioned positive electrode material.

[0020] A fifth object of the present invention is to provide a sodium ion battery, which comprises the above-mentioned positive electrode plate.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention will Li + , Cu 2+ 、Ni 2+ 、Ni 3+ 、Co 3+ , Fe 3+ 、Al 3+ , Mn 3+ , Mn 4+ 、Ti 4+ Sn 4+ , Sb 5+ A compound of at least five metal elements of equal or similar molar mass and a sodium source are treated at high temperature to obtain a high-entropy layered metal oxide, in which the number of atoms of each metal accounts for 5 to 35% of the total number of metal atoms and the total number of anions and cations is balanced. In the high-entropy metal oxide, the inert elements can stabilize the structure, and the active elements can serve as redox centers to provide charge compensation in electrochemical reactions. The high-entropy structure design can effectively increase the disorder of cations, increase short-range order, and avoid the formation of Na+ in the process of sodium insertion and extraction. + The long-range order formed by the vacancies reduces voltage hysteresis and improves rate performance; it can also significantly improve structural stability, delay phase change, and improve cycle stability. The metal oxide of the present invention is used as a positive electrode material in sodium ion batteries, which can provide higher specific capacity and energy density as well as excellent cycle performance, and can be used in 3C products and electric vehicles and other fields, with good commercial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The O3-type high entropy layered oxide Na obtained in Example 1 0.73 (CuNiFeMnTiSb) 1 / 6 XRD pattern of O2;

[0024] Figure 2 and 3 The O3-type high entropy layered oxide Na obtained in Example 1 is 0.73 (CuNiFeMnTiSb) 1 / 6O2 current density is 0.2C (1C = 120mAh g -1 )'s charge and discharge curves and cycle performance diagrams;

[0025] Figure 4 The O3-type high entropy layered oxide Na obtained in Example 2 0.76 (Ni 0.12 Cu 0.12 Fe 0.18 Co 0.18 Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 )XRD pattern of O2;

[0026] Figure 5 and 6 The O3-type high entropy layered oxide Na obtained in Example 2 is 0.76 (Ni 0.12 Cu 0.12 Fe 0.18 Co 0.1 8Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 ) Charge and discharge curves and cycle performance diagrams of O2 with a current density of 0.2C;

[0027] Figure 7 The O3 type high entropy layered oxide Na obtained in Example 3 0.88 (Ni 0.18 Cu 0.18 Fe 0.12 Al 0.12 Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 )XRD pattern of O2;

[0028] Figure 8 and 9 They are respectively the O3 type high entropy layered oxide Na obtained in Example 3 0.88 (Ni 0.18 Cu 0.18 Fe 0.12 Al 0.1 2Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 ) Charge and discharge curves and cycle performance diagrams of O2 with a current density of 0.2C;

[0029] Fig.10The O3-type high entropy layered oxide Na(LiNiCoMnTiSn) obtained in Example 4 1 / 6 XRD pattern of O2;

[0030] Fig.11 and 12 They are respectively the O3-type high entropy layered oxide Na(LiNiCoMnTiSn) obtained in Example 4 1 / 6 The charge and discharge curve and cycle performance diagram of O2 with a current density of 0.1C;

[0031] Fig.13 The P2-type high entropy layered oxide Na obtained in Example 5 0.6 (CuNiMnTiSb) 0.2 XRD pattern of O2;

[0032] Fig.14 and 15 The P2-type high entropy layered oxide Na obtained in Example 5 is 0.6 (CuNiMnTiSb) 0.2 The charge and discharge curve and cycle performance diagram of O2 with a current density of 0.2C;

[0033] Fig.16 The P2-type high entropy layered oxide Na obtained in Example 6 0.6 (LiCoMnTiSb) 0.2 XRD pattern of O2;

[0034] Fig.17 The P2-type high entropy layered oxide Na obtained in Example 6 0.6 (LiCoMnTiSb) 0.2 The charge and discharge curve of O2 with a current density of 0.1C;

[0035] Fig.18 The P2-type high entropy layered oxide Na obtained in Example 7 0.8 (LiNiMnTiSb) 0.2 XRD pattern of O2;

[0036] Fig.19 The P2-type high entropy layered oxide Na obtained in Example 7 0.8 (LiNiMnTiSb) 0.2 The charge and discharge curve of O2 with a current density of 0.1C. DETAILED DESCRIPTION

[0037] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0039] Example 1

[0040] A high entropy layered metal oxide, the preparation method of which is as follows:

[0041] According to the stoichiometric ratio, Na2CO3, CuO, NiO, Fe2O3, MnO2, TiO2 and Sb2O5 were weighed and placed in a ball mill, wherein Na2CO3 was 5% in excess to prevent volatilization loss during high-temperature calcination, and then 20 mL of isopropanol was added; the ball mill was placed on a planetary ball mill and ball milled at 400 rpm for 12 h; the ball mill was taken out and placed in an 80°C blast drying oven for 6 h to evaporate the isopropanol; the ball mill was then placed on a planetary ball mill and ball milled at 300 rpm for 5 min to separate the balls and powder to obtain a precursor powder; 2 g of the obtained precursor powder was weighed and pressed into a disc at a pressure of 10 MPa and placed in a crucible, and the temperature was raised to 900°C at a rate of 3°C / min in a muffle furnace and kept warm for 15 h, cooled to 150°C with the furnace and moved to a glove box for cooling; finally, the disc was ground into powder to obtain O3-type layered metal oxide Na 0.73 (CuNiFeMnTiSb) 1 / 6 O2, its XRD test results are as follows Figure 1 shown.

[0042] Example 2

[0043] A high entropy layered metal oxide, the preparation method of which is as follows:

[0044] According to the stoichiometric ratio, weigh Na2CO3, NiO, CuO, Fe2O3, Co2O3, MnO2, TiO2, SnO2 and Sb2O5 respectively and place them in a ball mill, wherein Na2CO3 is 5% in excess to prevent volatilization loss during high-temperature calcination. Then add 20 mL of isopropanol; place the ball mill on a planetary ball mill and mill at 400 rpm for 12 h; take out the ball mill and place it in an 80°C forced air drying oven for 6 h to evaporate the isopropanol. alcohol; then the ball mill is placed on a planetary ball mill at a speed of 300 rpm for 5 minutes to separate the balls and powder to obtain a precursor powder; 2 g of the obtained precursor powder is weighed and pressed into a disc at a pressure of 10 MPa and placed in a crucible, and the temperature is increased to 900 ° C at a rate of 3 ° C / min in a muffle furnace and kept for 15 hours, and then cooled to 150 ° C in the furnace and moved to a glove box for cooling; finally, the disc is ground into powder to obtain O3-type layered metal oxide Na 0.76 (Ni 0.12 Cu 0.12 Fe 0.18 Co 0.18 Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 )O2, its XRD test results are as follows Figure 4 shown.

[0045] Example 3

[0046] A high entropy layered metal oxide, the preparation method of which is as follows:

[0047] According to the stoichiometric ratio, weigh Na2CO3, NiO, CuO, Fe2O3, Al2O3, MnO2, TiO2, SnO2 and Sb2O5 respectively and place them in a ball mill, wherein Na2CO3 is 5% in excess to prevent volatilization loss during high-temperature calcination. Then add 20 mL of isopropanol; place the ball mill on a planetary ball mill and mill at 400 rpm for 12 h; take out the ball mill and place it in an 80°C forced air drying oven for 6 h to evaporate the isopropanol. alcohol; then the ball mill is placed on a planetary ball mill at a speed of 300 rpm for 5 minutes to separate the balls and powder to obtain a precursor powder; 2 g of the obtained precursor powder is weighed and pressed into a disc at a pressure of 10 MPa and placed in a crucible, and the temperature is increased to 900 ° C at a rate of 3 ° C / min in a muffle furnace and kept for 15 hours, and then cooled to 150 ° C in the furnace and moved to a glove box for cooling; finally, the disc is ground into powder to obtain O3-type layered metal oxide Na 0.88 (Ni 0.12 Cu 0.12 Fe 0.18 Al 0.18 Mn 0.1 Ti 0.1Sn 0.1 Sb 0.1 )O2, its XRD test results are as follows Figure 7 shown.

[0048] Example 4

[0049] A high entropy layered metal oxide, the preparation method of which is as follows:

[0050] According to the stoichiometric ratio, weigh Na2CO3, Li2CO3, NiO, Co2O3, MnO2, TiO2 and SnO2 respectively and place them in a ball mill, wherein Na2CO3 is in excess of 5% and Li2CO3 is in excess of 2% to prevent volatilization loss during high-temperature calcination. Then add 20 mL of isopropanol; place the ball mill on a planetary ball mill and mill at 400 rpm for 12 h; take out the ball mill and place it in an 80°C forced air drying oven for 6 h to evaporate the isopropanol; then grind the ball mill again. The jar was placed on a planetary ball mill and ball-milled at a speed of 300 rpm for 5 minutes to separate the balls and powders, thereby obtaining a precursor powder; 2 g of the obtained precursor powder was weighed and pressed into a disc at a pressure of 10 MPa and placed in a crucible, and the temperature was raised to 1000°C at a rate of 3°C / min in a muffle furnace and kept for 15 hours, and then cooled to 150°C with the furnace and moved to a glove box for cooling; finally, the disc was ground into powder to obtain an O3-type layered metal oxide Na(LiNiCoMnTiSn) 1 / 6 O2, its XRD test results are as follows Fig.10 shown.

[0051] Example 5

[0052] A high entropy layered metal oxide, the preparation method of which is as follows:

[0053] According to the stoichiometric ratio, Na2CO3, CuO, NiO, MnO2, TiO2 and Sb2O5 were weighed and placed in a ball mill, wherein Na2CO3 was 5% in excess to prevent volatilization loss during high-temperature calcination, and then 20 mL of isopropanol was added; the ball mill was placed on a planetary ball mill and ball milled at 400 rpm for 12 h; the ball mill was taken out and placed in an 80°C blast drying oven for 6 h to evaporate the isopropanol; the ball mill was then placed on a planetary ball mill and ball milled at 300 rpm for 5 min to separate the balls and powder to obtain a precursor powder; 2 g of the obtained precursor powder was weighed and pressed into a disc at a pressure of 10 MPa and placed in a crucible, and the temperature was raised to 900°C at a rate of 3°C / min in a muffle furnace and kept warm for 15 h, cooled to 150°C with the furnace and moved to a glove box for cooling; finally, the disc was ground into powder to obtain P2-type layered metal oxide Na 0.6 (CuNiMnTiSb) 0.2 O2, its XRD test results are as follows Fig.13shown.

[0054] Example 6

[0055] A high entropy layered metal oxide, the preparation method of which is as follows:

[0056] According to the stoichiometric ratio, Na2CO3, Li2CO3, Co2O3, MnO2, TiO2 and Sb2O5 were weighed and placed in a ball mill, wherein Na2CO3 was 5% in excess and Li2CO3 was 2% in excess to prevent volatilization loss during high-temperature calcination, and then 20 mL of isopropanol was added thereto; the ball mill was placed on a planetary ball mill and ball milled at 400 rpm for 12 h; the ball mill was taken out and placed in an 80°C blast drying oven for 6 h to evaporate the isopropanol; the ball mill was then placed on a planetary ball mill and ball milled at 300 rpm for 5 min to separate the balls and powder to obtain a precursor powder; 2 g of the obtained precursor powder was weighed and pressed into a disc at a pressure of 10 MPa and placed in a crucible, and the temperature was raised to 800°C at a rate of 3°C / min in a muffle furnace and kept warm for 15 h, cooled to 150°C with the furnace and moved to a glove box for cooling; finally, the disc was ground into powder to obtain P2-type layered metal oxide Na 0.6 (LiCoMnTiSb) 0.2 O2, its XRD test results are as follows Fig.16 shown.

[0057] Example 7

[0058] A high entropy layered metal oxide, the preparation method of which is as follows:

[0059] According to the stoichiometric ratio, Na2CO3, Li2CO3, NiO, MnO2, TiO2 and Sb2O5 were weighed and placed in a ball mill, wherein Na2CO3 was 5% in excess and Li2CO3 was 2% in excess to prevent volatilization loss during high-temperature calcination, and then 20 mL of isopropanol was added thereto; the ball mill was placed on a planetary ball mill and ball milled at 400 rpm for 12 h; the ball mill was taken out and placed in an 80°C blast drying oven for 6 h to evaporate the isopropanol; the ball mill was then placed on a planetary ball mill and ball milled at 300 rpm for 5 min to separate the balls and powder to obtain a precursor; 2 g of the obtained precursor powder was weighed and pressed into a disc at a pressure of 10 MPa and placed in a crucible, and the temperature was raised to 800°C at a rate of 3°C / min in a muffle furnace and kept warm for 15 h, cooled to 150°C with the furnace and moved to a glove box for cooling; finally, the disc was ground into powder to obtain P2-type layered metal oxide Na 0.6 (LiNiMnTiSb) 0.2 O2, its XRD test results are as follows Fig.18 shown.

[0060] Example 8

[0061] The metal oxides obtained in Examples 1-5 were mixed with Super P and PVDF at a mass ratio of 8:1:1, respectively, ball-milled for 30 min with 1-methyl-2-pyrrolidone (NMP) as a solvent to prepare a slurry, which was then coated on aluminum foil and placed in a vacuum drying oven and dried at 120° C. for 10 h; thereafter, the slurry was cut into circular positive electrode sheets with a diameter of 14 mm using a cutting machine.

[0062] Metallic sodium was punched into a 19 mm diameter disc as the negative electrode, 1.0 M sodium perchlorate (NaClO4) / ethylene carbonate (EC): dimethyl carbonate (DMC): methyl ethyl carbonate (EMC) (volume fraction = 1:1:1 Vol%) / 5.0% FEC solution was used as the electrolyte, and 19 mm diameter glass fiber was used as the separator. CR2016 button cells were assembled in a glove box filled with high-purity argon.

[0063] The electrochemical properties of metal oxide materials were tested in different voltage ranges. The test results are as follows: Figure 2 and 3 , Figure 5 and 6 , Figure 8 and 9 , Fig.11 and 12 , Fig.14 and 15 , Fig.17 , Fig.19 And as shown in Table 1.

[0064] Table 1 Electrochemical performance test results of metal oxides of Examples 1-7

[0065]

[0066] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0067] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A high entropy layered metal oxide, characterized in that The molecular formula of the metal oxide is: Na 0.76 (Ni 0.12 Cu 0.12 Fe 0.18 Co 0.18 Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 )O2 or Na(LiNiCoMnTiSn) 1 / 6 O2, the metal oxide is an O3 type layered oxide; When the molecular formula of the high entropy layered metal oxide is: Na 0.76 (Ni 0.12 Cu 0.12 Fe 0.18 Co 0.18 Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 )O2, and its preparation method is: Na2CO3, NiO, CuO, Fe2O3, Al2O3, MnO2, TiO2, SnO2 and Sb2O5 were weighed in a ball mill according to the stoichiometric ratio, wherein Na2CO3 was in excess of 5% to prevent volatilization loss during high-temperature calcination, and then 20 mL of isopropanol was added thereto; the ball mill was placed on a planetary ball mill and ball milled at 400 rpm for 12 h; the ball mill was taken out and placed in an 80°C forced air drying oven for 6 h to evaporate the isopropanol; the ball mill was then placed on a planetary ball mill and ball milled at 300 rpm for 5 min to separate the balls and powder to obtain a precursor powder; 2 g of the obtained precursor powder was weighed, pressed into a disc at a pressure of 10 MPa, and placed in a crucible, heated to 900°C at a rate of 3°C / min in a muffle furnace and kept warm for 15 h, cooled to 150°C with the furnace, and then moved to a glove box for cooling; When the molecular formula of the high entropy layered metal oxide is: Na(LiNiCoMnTiSn) 1 / 6 O2, the preparation method thereof is: Na2CO3, Li2CO3, NiO, Co2O3, MnO2, TiO2 and SnO2 were weighed respectively according to the stoichiometric ratio and placed in a ball mill, wherein Na2CO3 was in excess of 5% and Li2CO3 was in excess of 2% to prevent volatilization loss during high-temperature calcination, and then 20 mL of isopropanol was added thereto; the ball mill was placed on a planetary ball mill and ball milled at 400 rpm for 12 h; the ball mill was taken out and placed in an 80°C forced air drying oven for 6 h to evaporate the isopropanol; the ball mill was then placed on a planetary ball mill and ball milled at 300 rpm for 5 min to separate the balls and powder to obtain a precursor powder; 2 g of the obtained precursor powder was weighed, pressed into a disc at a pressure of 10 MPa, and placed in a crucible, heated to 1000°C at a rate of 3°C / min in a muffle furnace and kept warm for 15 h, cooled to 150°C with the furnace and moved to a glove box for cooling.

2. The method for preparing the high entropy layered metal oxide according to claim 1, characterized in that: When the molecular formula of the high entropy layered metal oxide is: Na 0.76 (Ni 0.12 Cu 0.12 Fe 0.18 Co 0.18 Mn 0.1 Ti 0.1 Sn 0.1 Sb 0.1 )O2, and its preparation method is: Na2CO3, NiO, CuO, Fe2O3, Al2O3, MnO2, TiO2, SnO2 and Sb2O5 were weighed in a ball mill according to the stoichiometric ratio, wherein Na2CO3 was in excess of 5% to prevent volatilization loss during high-temperature calcination, and then 20 mL of isopropanol was added thereto; the ball mill was placed on a planetary ball mill and ball milled at 400 rpm for 12 h; the ball mill was taken out and placed in an 80°C forced air drying oven for 6 h to evaporate the isopropanol; the ball mill was then placed on a planetary ball mill and ball milled at 300 rpm for 5 min to separate the balls and powder to obtain a precursor powder; 2 g of the obtained precursor powder was weighed, pressed into a disc at a pressure of 10 MPa, and placed in a crucible, heated to 900°C at a rate of 3°C / min in a muffle furnace and kept warm for 15 h, cooled to 150°C with the furnace, and then moved to a glove box for cooling; When the molecular formula of the high entropy layered metal oxide is: Na(LiNiCoMnTiSn) 1 / 6 O2, the preparation method thereof is: Na2CO3, Li2CO3, NiO, Co2O3, MnO2, TiO2 and SnO2 were weighed respectively according to the stoichiometric ratio and placed in a ball mill, wherein Na2CO3 was in excess of 5% and Li2CO3 was in excess of 2% to prevent volatilization loss during high-temperature calcination, and then 20 mL of isopropanol was added thereto; the ball mill was placed on a planetary ball mill and ball milled at 400 rpm for 12 h; the ball mill was taken out and placed in an 80°C forced air drying oven for 6 h to evaporate the isopropanol; the ball mill was then placed on a planetary ball mill and ball milled at 300 rpm for 5 min to separate the balls and powder to obtain a precursor powder; 2 g of the obtained precursor powder was weighed, pressed into a disc at a pressure of 10 MPa, and placed in a crucible, heated to 1000°C at a rate of 3°C / min in a muffle furnace and kept warm for 15 h, cooled to 150°C with the furnace and moved to a glove box for cooling.

3. A positive electrode material, characterized in that: Comprising the metal oxide according to claim 1.

4. A positive electrode sheet, characterized in that: Comprising the positive electrode material as claimed in claim 3.

5. A sodium ion battery, characterized in that Including the positive electrode sheet as described in claim 4.