Epitaxial wafer, semiconductor device, and method for manufacturing epitaxial wafer

By doping Si in the lower layer of the channel layer of the epitaxial wafer, the current collapse problem caused by C impurities capturing 2DEG electrons due to In detachment is solved, and semiconductor device performance with high output and low leakage current is achieved.

CN115088058BActive Publication Date: 2024-10-25MITSUBISHI ELECTRIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202080096401.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-02-17
Publication Date
2024-10-25
Estimated Expiration
2040-02-17

AI Technical Summary

Technical Problem

When existing epitaxial wafers are grown at low temperatures, In detaches from the back barrier layer, resulting in the presence of a large amount of impurity C in the channel layer, capturing 2DEG electrons, and causing current collapse problems.

Method used

Doping Si in the lower layer of the channel layer is lower than the growth temperature of the upper layer of the channel layer on the electron supply layer side, forming a Si-rich lower layer of the channel layer to compensate for the electron trap of C, suppress current collapse, and adjust the temperature in the furnace and pressure control C and Si concentrations.

Benefits of technology

It effectively suppresses the capture of 2DEG electrons, improves carrier mobility, reduces current collapse and leakage current, and improves the output performance of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115088058B_ABST
    Figure CN115088058B_ABST
Patent Text Reader

Abstract

The epitaxial wafer of the present disclosure comprises: a substrate; a buffer layer containing a composition formula of Al x Ga y In z N (x+y+z=1, y>0) represented by a crystal, and disposed on a substrate; a back barrier layer, containing a composition formula Al x Ga y In z N (x+y+z=1, y>0, z>0) represented by a crystal, and is disposed on the buffer layer; the channel layer contains a crystal having a composition formula of Al x Ga y In z N (x+y+z=1, y>0) and is disposed on the back barrier layer; and an electron supply layer having a composition formula of Al x Ga y In z The epitaxial wafer is characterized in that the channel layer is composed of an upper channel layer on the electron supply layer side and a lower channel layer on the back barrier layer side, the concentration of C in the lower channel layer is higher than that in the upper channel layer, and the lower channel layer contains Si.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an epitaxial wafer and a method for manufacturing the same, and the present disclosure relates to a semiconductor device including the epitaxial wafer. Background Art

[0002] There is a semiconductor device including an epitaxial wafer containing Al x Ga y In z N (x+y+z=1, y>0, Aluminum Gallium Indium Nitride) crystal. The epitaxial wafer has a composition of Al x Ga y In z A channel layer composed of a crystal represented by N (x+y+z=1, y>0), and a channel layer composed of a crystal having a composition formula of Al x Ga y In z The electron supply layer is composed of a crystal represented by N (x+y+z=1, x>0). Since these layers are heterojunctioned, a high-concentration two-dimensional electron gas (2DEG) is generated at the interface between these layers. By using this 2DEG as a carrier, the semiconductor device can perform high-output operation.

[0003] On the other hand, since the electron density of 2DEG is high, the semiconductor device described above may cause leakage current to flow through the buffer layer provided under the channel layer, and may reduce the high frequency characteristics. This leakage current is more significant when the gate is shortened to obtain a high current gain cutoff frequency.

[0004] In contrast, in the following Patent Document 1, a layer having a composition formula of Al is provided between the channel layer and the buffer layer. x Ga y In z The back barrier layer composed of crystals represented by N (x+y+z=1, y>0, z>0) increases the energy of the conduction band of the buffer layer, thereby suppressing the leakage current from flowing through the buffer layer.

[0005] Patent Document 1: Japanese Patent Application Publication No. 2019-21704

[0006] However, the epitaxial wafer of the above-mentioned Patent Document 1 is formed by a composition formula of Al x Ga y In zThe back barrier layer composed of the crystal represented by N (x+y+z=1, y>0, z>0) is separated and the resulting surface roughness causes the lower layer of the channel layer located on the back barrier layer side in the channel layer to grow at a low temperature. Therefore, a large amount of C (Carbon) as an impurity is contained in the lower layer of the channel layer. Since C is an acceptor-type trap, the electrons of 2DEG are captured by C, and there is a problem of current collapse. Summary of the invention

[0007] The present disclosure has been made to solve the above-mentioned problems, and an object of the present disclosure is to provide an epitaxial wafer capable of suppressing the occurrence of current collapse, a semiconductor device including the epitaxial wafer, and a method for manufacturing the epitaxial wafer.

[0008] The epitaxial wafer of the present disclosure comprises: a substrate; a buffer layer containing a composition formula of Al x Ga y In z N (x+y+z=1, y>0) represented by a crystal, and disposed on a substrate; a back barrier layer, containing a composition formula Al x Ga y In z N (x+y+z=1, y>0, z>0) represented by a crystal, and is disposed on the buffer layer; the channel layer contains a crystal having a composition formula of Al x Ga y In z N (x+y+z=1, y>0) and is disposed on the back barrier layer; and an electron supply layer having a composition formula of Al x Ga y In z A crystal represented by N(x+y+z=1, x>0) is provided on a channel layer. The channel layer is characterized in that the channel layer is composed of an upper channel layer on the electron supply layer side and a lower channel layer on the back barrier layer side, the concentration of C in the lower channel layer is higher than that in the upper channel layer, and the lower channel layer contains Si.

[0009] Furthermore, the semiconductor device according to the present disclosure includes: the epitaxial wafer described above; a source electrode and a drain electrode spaced apart and arranged on an electron supply layer of the epitaxial wafer; and a gate electrode arranged between the source electrode and the drain electrode on the electron supply layer.

[0010] In addition, the method for manufacturing an epitaxial wafer according to the present disclosure comprises the following steps: a placement step of placing a substrate in a furnace; a buffer layer formation step of forming a buffer layer having a composition formula of Al on the substrate; x Ga y In zA buffer layer of a crystal represented by N (x+y+z=1, y>0); a back barrier layer forming step, forming a crystal having a composition formula Al on the buffer layer x Ga y In z A back barrier layer of a crystal represented by N (x+y+z=1, y>0, z>0); a channel layer forming step, growing a crystal having a composition formula Al on the back barrier layer x Ga y In z N (x+y+z=1, y>0) represented by a channel layer; and an electron supply layer forming step, growing an electron supply layer having a composition formula Al x Ga y In z The electron supply layer of the crystal represented by N (x+y+z=1, x>0) is characterized in that, in the channel layer forming step, the temperature in the furnace when forming the channel layer lower layer on the back barrier layer side of the channel layer is lower than the temperature when forming the channel layer upper layer on the electron supply layer side of the channel layer, and in the channel layer forming step, Si is doped into the channel layer lower layer when forming the channel layer lower layer.

[0011] The epitaxial wafer and the semiconductor device according to the present disclosure contain Si in the lower layer of the channel layer, so that electrons are supplied from Si to C, and Si compensates for C. Therefore, current collapse can be suppressed.

[0012] In addition, the epitaxial wafer manufacturing method according to the present disclosure dopes Si into the channel layer lower layer when forming the channel layer lower layer, so that electrons are supplied from Si to C in the channel layer lower layer, and Si compensates for C. Therefore, an epitaxial wafer capable of suppressing current collapse can be manufactured. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a conceptual cross-sectional view of an epitaxial wafer according to Embodiment 1 of the present disclosure.

[0014] Figure 2 This is a graph showing the relationship between the C concentration and the Si concentration of the epitaxial wafer according to the first embodiment of the present disclosure and the depth from the surface.

[0015] Figure 3 This is a conceptual cross-sectional view of the semiconductor device according to the first embodiment of the present disclosure.

[0016] Figure 4 This is a flowchart showing the method for manufacturing an epitaxial wafer according to the first embodiment of the present disclosure.

[0017] Figure 5 This is a graph showing the relationship between the furnace temperature and the growth time in the channel layer forming step of the method for manufacturing an epitaxial wafer according to the first embodiment of the present disclosure.

[0018] Figure 6 This is a graph showing the relationship between the furnace temperature and the furnace pressure and the growth time in the channel layer forming step of the method for manufacturing an epitaxial wafer according to the second embodiment of the present disclosure.

[0019] Figure 7 This is a graph showing the relationship between the furnace temperature and the V / III ratio and the growth time in the channel layer forming step of the method for manufacturing an epitaxial wafer according to the third embodiment of the present disclosure.

[0020] Figure 8 This is a graph showing the relationship between the C concentration and the Si concentration of the epitaxial wafer according to the third embodiment of the present disclosure and the depth from the surface. DETAILED DESCRIPTION

[0021] Hereinafter, embodiments of the present disclosure will be described using the drawings. The same reference numerals in the drawings represent the same or corresponding parts.

[0022] Implementation Method 1

[0023] use Figure 1 , the structure of the epitaxial wafer 10 (hereinafter, simply referred to as the wafer 10 ) according to the first embodiment of the present disclosure will be described.

[0024] The wafer 10 includes a substrate 12 and a semiconductor layer disposed on the substrate 12. The semiconductor layer includes a nucleation layer 13, a buffer layer 14, a back barrier layer 15, a channel layer 16, and an electron supply layer 17 in order from the substrate 12 side. The wafer 10 is a III-V nitride semiconductor epitaxial wafer in which the semiconductor layer contains a III-group element and a V-group element. More specifically, at least a portion of the semiconductor layer contains a composition formula of Al x Ga y In z The wafer 10 is a gallium nitride crystal represented by N (x+y+z=1, y>0). In addition, the wafer 10 is used for a GaN-HEMT (Gallium Nitride-High Electron Mobility Transistor) as a high electron mobility transistor.

[0025] The substrate 12 constituting the wafer 10 is used to form a substrate 12 having a composition formula of Al x Ga y In z The crystal growth represented by N (x+y+z=1) is composed of SiC (Silicon Carbide).

[0026] A nucleus formation layer 13 containing crystals represented by a composition formula of AlN is disposed on the substrate 12. The nucleus formation layer 13 is used to form a crystal represented by a composition formula of AlN on the substrate 12. x Ga y In z A layer of crystal represented by N (x+y+z=1, y>0).

[0027] The thickness of the nucleation layer 13 from the interface with the substrate 12 to the interface with the buffer layer 14 was 50 nm.

[0028] A buffer layer 14 containing crystals expressed by the composition formula GaN is disposed on the nucleation layer 13. The buffer layer 14 is a layer for reducing dislocations (crystal defects) in a region where 2DEG occurs (interface between the channel layer 16 and the electron supply layer 17).

[0029] Although the thickness of the buffer layer 14 from the interface with the nucleation layer 13 to the interface with the back barrier layer 15 is 1 μm, any thickness may be sufficient to achieve the effect of reducing dislocations.

[0030] A back barrier layer 15 is disposed on the buffer layer 14. The back barrier layer 15 is used to generate a back barrier effect that increases the energy of the conduction band of the buffer layer 14 and raises the band. In order to generate the back barrier effect, the back barrier layer 15 contains GaN crystals with a smaller band gap than the GaN crystals contained in the buffer layer 14 and a composition formula of GaN. y In z It is known that when a back barrier layer 15 having a small band gap is arranged on the buffer layer 14, the energy of the conduction band of the buffer layer 14 rises toward the interface with the back barrier layer 15 due to the polarization effect.

[0031] If the composition of In in the back barrier layer 15 is too low, the band gap difference with the buffer layer 14 becomes small, and the above-mentioned back barrier effect cannot be fully generated. In addition, if the composition of In is too high, the strain in the crystal becomes too large, and the crystal quality deteriorates. That is, the number of dislocations in the region where 2DEG is generated increases, resulting in negative effects such as reduced mobility of electrons in 2DEG. Therefore, the composition of In in the InGaN crystal contained in the back barrier layer 15 is preferably in the range of 3% to 15%, and is 5% in Embodiment 1.

[0032] In addition, if the thickness of the back barrier layer 15 from the interface with the buffer layer 14 to the interface with the channel layer 16 is too thin, the above-mentioned back barrier effect cannot be fully produced. On the contrary, if the thickness of the back barrier layer 15 is too thick, the crystal quality deteriorates. In this way, there is also a trade-off relationship between the back barrier effect and the crystal quality regarding the thickness. Therefore, the thickness of the back barrier layer 15 is preferably in the range of 1nm to 2nm, and in embodiment 1, the thickness is 1nm.

[0033] As described later, the back barrier layer 15 is formed by epitaxially growing InGaN crystals while making the temperature in the furnace lower than that of the buffer layer 14, the channel layer upper layer 16b located on the electron supply layer 17 side of the channel layer 16, and the electron supply layer 17. This is because In is not easily separated from the back barrier layer 15 by growing at a low temperature. In addition, under this growth condition, C (carbon) in the furnace is introduced into the back barrier layer 15 and is not easily separated thereafter, so the back barrier layer 15 contains C. Specifically, in Embodiment 1, the back barrier layer 15 contains 3×10 16 atoms / cm 3 or more carbon.

[0034] Among them, C in the furnace is supplied by TMGa (Tri-Methyl Gallium, Ga(CH3)3) which is a raw material of Ga.

[0035] A channel layer 16 is disposed on the back barrier layer 15. The channel layer 16 is a layer for carriers to move, and is composed of a crystal represented by a composition formula of GaN. The reason why GaN crystal is used is that high-quality crystals can be grown.

[0036] Here, the channel layer 16 is composed of a channel layer lower layer 16a on the back barrier layer 15 side and a channel layer upper layer 16b on the electron supply layer 17 side. The channel layer lower layer 16a and the channel layer upper layer 16b have different epitaxial growth conditions.

[0037] The lower channel layer 16a is used to cover the back barrier layer 15 so that In contained in the back barrier layer 15 or N combined with In does not separate. If In or N separates from the back barrier layer 15, the surface will be rough and the crystal quality will be reduced, which is not preferred. Since In or N also separates when growing the lower channel layer 16a, the lower channel layer 16a is grown at a lower temperature than when growing the upper channel layer 16b. Therefore, a large amount of C is introduced into the lower channel layer 16a, and the concentration of C is higher than that of the upper channel layer 16b. Specifically, in embodiment 1, the concentration of C in the lower channel layer 16a is 7×10 16 atoms / cm 3 In addition, although the concentration of C varies depending on the growth conditions, the concentration of C is at least 5×10 16 atoms / cm3 or above.

[0038] Here, since the lower layer 16a of the channel layer is located near the region where 2DEG that becomes a carrier is generated, that is, the upper layer 16b of the channel layer, the C contained in the lower layer 16a of the channel layer captures the electrons of the 2DEG at its acceptor level, reduces the electron concentration of the 2DEG, and produces a deterioration of the transient response such as a temporary decrease in the output of the transistor having the chip 10. Such a phenomenon is called current collapse, which hinders the high output of the transistor. In addition, the transistor that produces current collapse has the property that the output varies depending on the power input in the past, that is, it has a memory effect. This is particularly a problem when the transistor is used for wireless communication purposes. For example, in the communication of mobile phone base stations, etc., distortion compensation technology is used to ensure the communication quality, but when the transistor has a memory effect caused by current collapse, the distortion of the signal cannot be fully compensated, resulting in deterioration of the communication quality and power release outside the specified frequency band. In addition, in order to reduce this effect, the output must be limited, and in this case the efficiency deteriorates. In order to suppress the occurrence of current collapse that causes such a problem, the lower layer 16a of the channel layer of embodiment 1 is doped with Si during growth and contains Si. Si is an n-type dopant and supplies electrons to the trap level formed by C. Therefore, it is possible to suppress the trapping of electrons in 2DEG caused by C and suppress the current collapse. In order to fully suppress the current collapse, in the first embodiment, the concentration of Si contained in the lower layer 16a of the channel layer is higher than the concentration of C in the lower layer 16a of the channel layer. Specifically, in the first embodiment, the concentration of Si is 8×10 16 atoms / cm 3 or above.

[0039] The lower layer 16a of the channel layer needs to reliably cover the back barrier layer 15 and cannot be too thin so that In or N does not detach from the back barrier layer 15. On the other hand, if the concentration of electrons moving in the lower layer 16a of the channel layer cannot be ignored relative to the electron concentration of 2DEG, the output of the transistor is reduced. This is because, as described later, the upper layer 16b of the channel layer contains undoped GaN crystals, while the lower layer 16a of the channel layer contains a large amount of Si and C. In comparison, the mobility of carriers in the lower layer 16a of the channel layer is low, which lowers the average value of the mobility. Therefore, it is necessary to make the lower layer 16a of the channel layer not too thick. Based on the above, the thickness of the lower layer 16a of the channel layer from the interface with the back barrier layer 15 to the interface with the upper layer 16b of the channel layer is preferably in the range of 1nm to 20nm. In embodiment 1, the thickness of the lower layer 16a of the channel layer is 5nm.

[0040] The upper channel layer 16b is used for carrier movement and contains undoped GaN crystals to prevent electron mobility from being reduced. In addition, when C is introduced, electron mobility is reduced or current collapse is easily generated, so the upper channel layer 16b is grown at a higher temperature than the lower channel layer 16a.

[0041] Although 2DEG is generated near the interface between the channel layer upper layer 16b and the electron supply layer 17, in order to make most of the 2DEG exist in the channel layer upper layer 16b with high mobility, the channel layer upper layer 16b must be thickened to a certain extent. Specifically, the layer thickness of the channel layer upper layer 16b from the interface with the channel layer lower layer to the interface with the electron supply layer 17 is preferably 5nm or more. In embodiment 1, the layer thickness of the channel layer upper layer 16b is 50nm.

[0042] If the thickness of the channel layer 16 composed of the lower channel layer 16a and the upper channel layer 16b is too thick, the back barrier layer 15 is formed from the gate electrode 23 (see the following description) provided above the channel layer 16. Figure 3 ) is too separated, and control based on the gate electrode 23 cannot be performed, and the electrons moving in the back barrier layer 15 where the conduction band becomes low act as leakage current, which brings a significant negative impact. Therefore, the layer thickness of the channel layer 16 from the interface between the back barrier layer to the interface between the electron supply layer 17 is preferably less than 100nm. By setting the layer thickness to less than 100nm, the back barrier layer 15 and the gate electrode 23 become closer, and even if a leakage current flows slightly near the pinch-off, as long as the voltage involved in the gate electrode is set to a closed state, the back barrier layer 15 is immediately depleted, and the leakage current is suppressed. Therefore, the influence of the leakage current becomes smaller, and it will not be a problem in practical use. In embodiment 1, the layer thickness of the channel layer 16 is 55nm.

[0043] Here, the thickness of the channel layer 16 can be made less than 100 nm because the channel layer lower layer 16 a contains Si, and even if the channel layer lower layer 16 a is close to the region where 2DEG is generated, the current collapse can be suppressed. On the contrary, when Si is not doped in the channel layer lower layer 16 a, if the thickness of the channel layer 16 is set to less than 100 nm, the electrons of 2DEG are easily captured by C, so that the current collapse is easily generated, and it is difficult to reduce the thickness.

[0044] In summary, it is preferred that the channel layer 16 has a thickness of 100 nm or less, the channel layer lower layer 16 a has a thickness of 1 nm to 20 nm, and the channel layer upper layer 16 b has a thickness of 5 nm to 80 nm.

[0045] An electron supply layer 17 is disposed on the channel layer upper layer 16 b of the channel layer 16 . The electron supply layer 17 contains a composition formula of Al x Ga yThe electron supply layer 17 is used to generate a high concentration of 2DEG at the interface between the electron supply layer 17 and the channel layer upper layer 16b, and contains an AlGaN crystal having a larger band gap than the GaN crystal contained in the channel layer 16. The AlGaN crystal generates 2DEG near the interface between the electron supply layer 17 and the channel layer 16 by the polarization effect.

[0046] The composition ratio of Al to Ga in the AlGaN crystal contained in the electron supply layer 17 and the thickness of the electron supply layer 17 can be appropriately selected according to the concentration of 2DEG to be generated. Here, although the concentration of 2DEG increases as the Al content and the thickness of the electron supply layer 17 increase, when these are large, dislocations caused by strain are more likely to occur, and there is a trade-off relationship. In embodiment 1, the composition is x=0.25, y=0.75, and the thickness of the electron supply layer 17 is 20nm.

[0047] The wafer 10 is configured as described above. Here, as described above, the wafer 10 contains C and Si. Figure 2 The concentrations of these in the channel layer 16 will be described. Figure 2 The vertical axis represents the concentration of C and Si, and the horizontal axis represents the depth from the surface. The portion of the horizontal axis to the left (origin side) of the dotted line represents the depth at which the upper channel layer 16b is arranged, and the portion to the right represents the depth at which the lower channel layer 16a is arranged. In addition, the concentration of C is represented by a solid line, and the concentration of Si is represented by a single-point dashed line.

[0048] Since the channel layer upper layer 16b is grown at a higher temperature than the channel layer lower layer 16a, even if C is introduced during growth, it is easy to be separated, such as Figure 2 As shown, the concentration of C becomes lower than that of the channel layer lower layer 16a. On the contrary, the channel layer lower layer 16a is grown at a low temperature, so the concentration of C becomes higher than that of the channel layer upper layer 16b.

[0049] In addition, the channel layer lower layer 16a is doped with Si, such as Figure 2 As shown in FIG. 1 , the concentration of Si is higher than that of C. The channel layer upper layer 16 b is not doped with Si, but only slightly contains Si diffused from the channel layer lower layer 16 a. Therefore, although Figure 2 The position corresponding to the depth of the channel layer upper layer 16b does not show the Si concentration (single-dot chain line), but the Si concentration of the channel layer upper layer 16b is lower than the Si concentration of the channel layer lower layer 16a.

[0050] Next, use Figure 3The structure of the semiconductor device 20 including the above-mentioned wafer 10 will be described. Specifically, the semiconductor device 20 is a semiconductor element used in GaN-HEMT (High Electron Mobility Transistor) and the like.

[0051] The semiconductor device 20 includes a wafer 10 , a source electrode 21 , a drain electrode 22 , and a gate electrode 23 .

[0052] On the upper surface of the wafer 10, i.e., the surface of the electron supply layer 17 opposite to the substrate 12 side, a source electrode 21 and a drain electrode 22 are arranged at intervals. In the source electrode 21 and the drain electrode 22, the lower layer on the electron supply layer 17 side is composed of Ti (Titanium), and the upper layer on the opposite side of the electron supply layer 17 is composed of Al, the thickness of the lower layer is about 20nm, and the thickness of the upper layer is about 200nm. The source electrode 21 and the drain electrode 22 are in ohmic contact with the electron supply layer 17.

[0053] In addition, a gate electrode 23 in contact with the electron supply layer 17 is arranged between the source electrode 21 and the drain electrode 22. In the gate electrode 23, the lower layer on the electron supply layer 17 side is composed of Ni (Nickel), and the upper layer on the opposite side of the electron supply layer 17 is composed of Au, the thickness of the lower layer is about 30nm, and the thickness of the upper layer is about 400nm.

[0054] In addition, although Figure 3 Although omitted in the figure, in the semiconductor device 20, wiring is also connected to the source electrode 21, the drain electrode 22, and the gate electrode 23. In addition, Ar (Argon) or the like is injected into the side surface of the wafer 10, that is, the surface of the wafer 10 parallel to the arrangement direction from the substrate 12 to the electron supply layer 17, to form an inactive region.

[0055] Next, follow Figure 4 The manufacturing method of the above-mentioned wafer 10 is described with reference to the flowchart of FIG. 1 . Here, each layer of the wafer 10 is formed by a metal organic chemical vapor deposition (MOCVD) method.

[0056] (Configuration steps)

[0057] First, the substrate 12 is placed in a furnace for epitaxially growing the wafer 10 (step S101 ).

[0058] (Nucleation layer formation step)

[0059] Next, a mixed gas of TMA (Tri-Methyl Aluminum, Al(CH 3 ) 3 ) gas and ammonia gas is introduced into the furnace to grow 50 nm AlN crystals on the substrate 12 , thereby forming a nucleation layer 13 on the substrate 12 (step S102 ).

[0060] (Buffer layer formation step)

[0061] Next, a mixed gas of TMGa gas and ammonia gas is introduced into the furnace to grow a 1 μm GaN crystal on the nucleation layer 13, and an undoped buffer layer 14 is formed on the nucleation layer 13 (step S103). At this time, the temperature in the furnace is set to 1100°C, the pressure is set to 200 mbar, and the V / III ratio of the mixed gas (V / III ratio: the value obtained by dividing the molar flow rate of the V group raw material supplied to the furnace by the molar flow rate of the III group raw material supplied to the furnace) is set to 500. In addition, hydrogen is used as a carrier gas.

[0062] (Back Barrier Layer Formation Step)

[0063] Next, a mixed gas of TMI (Tri-Methyl Indium, In(CH3)3) gas, TMGa gas, and ammonia gas is introduced into the furnace to grow a 1 nm InGaN crystal on the buffer layer 14, and to form a back barrier layer 15 on the buffer layer 14 (step S104). At this time, the temperature in the furnace is set to 800°C, the pressure is set to 400 mbar, and the V / III ratio is set to 50000. In addition, nitrogen gas is used as a carrier gas.

[0064] The back barrier layer 15 is grown under growth conditions of lower temperature, higher pressure and higher V / III ratio than the nucleation layer 13 , the channel layer upper layer 16 b described later and the electron supply layer 17 . This is to introduce In into the back barrier layer 15 to prevent it from being easily separated.

[0065] (Channel layer lower layer formation step)

[0066] Next, a mixed gas of TMGa gas, monosilane gas and ammonia gas is introduced into the furnace to grow a 5 nm Si-doped GaN crystal on the back barrier layer 15, and to form a channel layer lower layer 16a on the back barrier layer 15 (step S105). At this time, the temperature in the furnace is set to 800°C, the pressure is set to 200 mbar, and the V / III ratio is set to 500. In addition, hydrogen gas is used as a carrier gas.

[0067] If the temperature in the furnace is set to a high temperature in the channel layer lower layer formation step, there is a possibility that In or N will be separated from the surface of the back barrier layer 15, causing the surface roughness. Therefore, the channel layer lower layer is grown under growth conditions at a temperature lower than that of the nucleation layer 13, the channel layer upper layer 16b described later, and the electron supply layer 17. Generally speaking, after the InGaN crystal is grown, the temperature cannot be increased until the InGaN crystal is protected by a material that does not contain In, such as GaN. However, if the growth conditions are set to a low temperature, when the GaN crystal is grown, a large amount of C contained in the TMGa gas is introduced into the channel layer lower layer and is not easy to separate. Since this C becomes an acceptor and captures electrons of 2DEG, it becomes a cause of the deterioration of the transition response, but in the channel layer lower layer formation step of embodiment 1, the channel layer lower layer 16a is doped with Si. By making the concentration of doped Si higher than the concentration of C contained in the lower layer 16a of the channel layer, Si can fill the trap energy level of C with electrons. Therefore, the amount of monosilane gas in the mixed gas is adjusted in such a way that the concentration of Si is higher than the concentration of C in the lower layer 16a of the channel layer.

[0068] (Channel layer upper layer formation step)

[0069] Next, a mixed gas of TMGa gas and ammonia gas is introduced into the furnace to grow a 50nm undoped GaN crystal on the channel layer lower layer 16a, and to form a channel layer upper layer 16b on the channel layer lower layer 16a (step S106). At this time, the temperature in the furnace is set to 1100°C, the pressure is set to 200mbar, and the V / III ratio is set to 500. In addition, hydrogen is used as a carrier gas.

[0070] When the channel layer upper layer 16b is formed, the surface of the back barrier layer 15 is covered by the channel layer lower layer 16a. Therefore, even if the growth condition is set to a temperature higher than that when the channel layer lower layer 16a is formed, the problem of In or N separation is not easy to occur. In addition, since it is not easy to include C in the channel layer upper layer 16b when the growth condition is set to a high temperature, it is preferable from the viewpoint of improving the mobility of carriers. Therefore, in the channel layer upper layer formation step, the furnace temperature is made higher than that in the channel layer lower layer formation step.

[0071] Here, the channel layer lower layer forming step and the channel layer upper layer forming step are collectively referred to as the channel layer forming step. Figure 5 , the relationship between the growth time and the furnace temperature in the channel layer formation step and the timing of doping Si are explained.

[0072] exist Figure 5In the graph, the vertical axis represents the furnace temperature, the horizontal axis represents the growth time, and the origin of the horizontal axis represents the time when the growth of the channel layer lower layer 16a is started. In addition, the portion between the left dotted line and the origin corresponds to the time when the channel layer lower layer formation step is performed, and the portion to the right of the right dotted line corresponds to the time when the channel layer upper layer formation step is performed.

[0073] like Figure 5 As shown in FIG. 1 , the temperature in the furnace when forming the lower channel layer 16a is different from the temperature in the furnace when forming the upper channel layer 16b. As described above, the temperature in the furnace when forming the lower channel layer 16a is lower than the temperature in the furnace when forming the upper channel layer 16b. In addition, although monosilane, which is a raw material of Si, is supplied in the step of forming the lower channel layer, it is not supplied after the step of forming the lower channel layer is completed.

[0074] In addition, if Figure 5 As shown, a period (between the dotted line on the left and the dotted line on the right) for interrupting the growth is provided between the channel layer lower layer forming step and the channel layer upper layer forming step, and the temperature in the furnace is increased during this period, but the channel layer 16 (referred to as the intermediate layer) may also be grown during this period. In this case, the intermediate layer grown without the temperature in the furnace being sufficiently increased contains C, and the concentration of C gradually decreases as the temperature rises. For this reason, the supply of monosilane, which is the raw material of Si supplied in the channel layer lower layer forming step, is continued, and the supply amount of monosilane is gradually reduced, thereby being able to compensate for C with Si.

[0075] Back to Figure 4 , the electron supply layer forming step which is the next step of the channel layer upper layer forming step (step S106) is described.

[0076] (Electron Supply Layer Formation Step)

[0077] A mixed gas of TMA gas, TMG gas and ammonia gas is introduced into the furnace to grow a 20 nm AlGaN crystal on the channel layer upper layer 16 b, and an electron supply layer 17 is formed on the channel layer upper layer 16 b (step S107). At this time, the temperature in the furnace is set to 1100° C., the pressure is set to 50 mbar, and the V / III ratio is set to 1000. In addition, hydrogen gas is used as a carrier gas.

[0078] In the above-described manner, the wafer 10 is manufactured.

[0079] Next, a method of manufacturing the semiconductor device 20 from the wafer 10 manufactured as described above will be described.

[0080] First, a resist mask for forming a source electrode 21 and a drain electrode 22 is formed on the electron supply layer 17 of the wafer 10. Specifically, a resist is applied on the electron supply layer 17, and an opening is formed in the portion of the resist where the electrode is to be formed. Next, 20 nm of Ti and 200 nm of Al are deposited on the resist including the opening by evaporation in such a manner that Ti becomes the lower layer and Al becomes the upper layer, and the resist mask and the Ti and Al deposited thereon are removed by a stripping method. Thereafter, the wafer 10 is heat treated at 600° C. in, for example, a nitrogen atmosphere, so that Ti and Al are in ohmic contact with the electron supply layer 17. In this way, the source electrode 21 and the drain electrode 22 are formed.

[0081] In addition, a resist mask for forming the gate electrode 23 is formed on the electron supply layer 17 of the wafer 10. Specifically, a resist is applied on the electron supply layer 17, and processed by photolithography to form an opening for forming the gate electrode 23 between the source electrode 21 and the drain electrode 22 in the resist. Next, 30 nm of Ni and 400 nm of Au are deposited on the resist including the opening by evaporation in such a way that Ni becomes the lower layer and Au becomes the upper layer, and the resist mask and the Ni and Au deposited thereon are removed by a lift-off method. In this way, the gate electrode 23 is formed between the source electrode 21 and the drain electrode 22.

[0082] Furthermore, connection of wirings to the electrodes and formation of inactive regions are also performed by known methods.

[0083] The wafer 10 , the semiconductor device 20 , and the method for manufacturing the wafer 10 according to the first embodiment of the present disclosure are configured as described above, and provide the following effects.

[0084] The chip 10 and the semiconductor device 20 involved in the embodiment 1 of the present disclosure are doped with Si as an n-type dopant in the lower layer 16a of the channel layer near the area where C exists at a high concentration and 2DEG exists. Si supplies electrons to the trap energy level of C so that the electrons of 2DEG are not easily captured. Therefore, the chip 10 and the semiconductor device 20 can suppress the situation where the electrons of 2DEG are captured by C and the carrier density is reduced. That is, the occurrence of current collapse can be suppressed. In addition, since the current collapse can be suppressed, the chip 10 and the semiconductor device 20 can suppress the deterioration of the transient response characteristics, and the semiconductor device 20 can be used at a high output (near the saturation output).

[0085] Si functions as a donor that supplies one electron, and C contained therein functions as an acceptor that receives one electron. Therefore, if the concentration of Si contained in the channel lower layer 16a is lower than that of C, electrons cannot be supplied to all Cs.

[0086] In the wafer 10 and the semiconductor device 20 according to the first embodiment of the present disclosure, the concentration of Si contained in the channel lower layer 16a is higher than the concentration of C contained in the channel lower layer 16a. Therefore, electrons supplied to all C can be prepared, and the occurrence of current collapse can be suppressed more reliably.

[0087] The wafer 10 and the semiconductor device 20 according to the first embodiment of the present disclosure suppress the generation of current collapse by doping Si in the lower layer 16a of the channel layer, and suppress the generation of leakage current by setting the layer thickness of the channel layer to 100 nm or less so as to bring the back barrier layer 15 and the gate electrode 23 closer. Therefore, the generation of leakage current and the generation of current collapse can be suppressed at the same time.

[0088] The channel layer upper layer 16b is a layer through which 2DEG as carriers move. If there are many impurities in the channel layer upper layer 16b, the mobility of carriers decreases, so it is preferable that the concentration of impurities in the channel layer upper layer 16b is low.

[0089] In the wafer 10 and the semiconductor device 20 according to the first embodiment of the present disclosure, the channel layer upper layer 16b is grown at a higher temperature than the channel layer lower layer 16a, so the C concentration of the channel layer upper layer 16b is lower than that of the channel layer lower layer. Therefore, the carrier mobility can be improved.

[0090] Furthermore, the method for manufacturing the wafer 10 according to the first embodiment of the present disclosure can manufacture the wafer 10 that exhibits the above-described effects.

[0091] Here, modifications of the wafer 10 , the semiconductor device 20 , and the method for manufacturing the wafer 10 according to the first embodiment of the present disclosure will be described and supplemented.

[0092] In the first embodiment of the present disclosure, although the wafer 10 includes the substrate 12, the nucleus formation layer 13, the buffer layer 14, the back barrier layer 15, the channel layer 16, and the electron supply layer 17 in order from the bottom, another layer may be added between these layers as long as the above-mentioned effect and the function as the GaN-HEMT can be exerted. In the description of the first embodiment, for example, it is shown that the nucleus formation layer 13 is arranged and grown on the substrate 12 and the buffer layer 14 is arranged and grown on the nucleus formation layer 13, but in the case of adding another layer, it can be replaced by arranging and growing the nucleus formation layer 13 via another layer on the substrate 12 and arranging and growing the buffer layer 14 via another layer on the nucleus formation layer 13. In addition, it can also be shown that the layer located in the middle is omitted. For example, it can also be shown that the nucleus formation layer 13 is omitted and only the buffer layer is arranged and grown on the substrate 12.

[0093] As an example of adding another layer, a nucleation layer 13 may be grown after a material such as SiN is arranged on the substrate 12. In addition, a layer containing high-resistance GaN crystals doped with Fe (Ferrum) or C may be provided between the buffer layer 14 and the nucleation layer 13. In this case, the thickness of the buffer layer 14 and the layer containing high-resistance GaN crystals can be appropriately adjusted. In addition, in the case of doping with Fe, ferrocene can be used as its raw material. In addition, a cap layer containing GaN crystals may be provided between the electron supply layer 17 and each electrode.

[0094] In the first embodiment, the substrate 12 is made of SiC, but it may be made of Si (Silicon), sapphire, GaAs (Garium Arsenide), or ZnO (Zinc Oxide) instead of SiC.

[0095] In the first embodiment, although the nucleation layer 13 contains AlN crystals, as long as a layer having a composition formula of Al x Ga y In z N (x+y+z=1, y>0), it may also contain crystals other than AlN. For example, it may also contain crystals with a composition formula of Al x Ga y In z N(x+y+z=1) is a crystal. In addition, the nucleation layer 13 may be composed of multiple layers with different compositions. In this case, the composition of each layer can be expressed by the composition formula Al x Ga y In z N(x+y+z=1) represents the thickness of the nucleus formation layer 13. Although the thickness of the nucleus formation layer 13 is 50 nm, any thickness may be used as long as the crystals of the upper layer of the nucleus formation layer 13 can be grown with high quality.

[0096] In the first embodiment, the buffer layer 14 contains GaN crystals, but may be crystals other than GaN as long as the dislocations in the region where 2DEG is generated can be reduced. x Ga y In z A crystal represented by N(x+y+z=1, y>0).

[0097] In the first embodiment, the back barrier layer 15 contains InGaN crystals, but as long as the back barrier effect can be produced, crystals other than InGaN may be used. For example, a crystal having a composition formula of Al x Ga y In z A crystal represented by N(x+y+z=1, y>0, z>0).

[0098] In the first embodiment, the channel layer 16 contains GaN crystals, but as long as 2DEG can be generated, it may be a crystal other than GaN. For example, it may contain a crystal having a composition formula of Al x Ga y In z A crystal represented by N(x+y+z=1, y>0).

[0099] In the first embodiment, the electron supply layer 17 contains AlGaN crystals, but the channel layer 16 may contain crystals other than AlGaN as long as it can generate 2DEG. x Ga y In z N (x+y+z=1, x>0) is a crystal. More specifically, Al x In z N (x+z=1, x>0, z>0), Al x Ga y In z N(x+y+z=1, x>0, y>0, z>0), etc.

[0100] In Embodiment 1, nitrogen gas is used as a carrier gas when growing the back barrier layer 15 , and hydrogen gas is used as a carrier gas when growing other layers. However, other carrier gases may be used.

[0101] In Embodiment 1, an example is described in which the concentration of Si contained in the channel layer lower layer 16a is higher than the concentration of C contained in the channel layer lower layer 16a. However, even if the concentration of Si is lower than that of C, Si can compensate for a part of C, thereby suppressing the occurrence of current collapse.

[0102] In the first embodiment, the source electrode 21 and the drain electrode 22 are made of Ti and Al, and the gate electrode 23 is made of Ni and Au, but the materials are not limited to these and known materials can be used. In addition, the structure and layer thickness of the electrodes can be appropriately selected.

[0103] Implementation Method 2

[0104] Next, Embodiment 2 of the present disclosure will be described. The description of the same parts as those of the structure and manufacturing method described in Embodiment 1 will be omitted, and the following will describe the parts that are different from Embodiment 1. In addition, the wafer 10, the semiconductor device 20, and the manufacturing method of the wafer 10 of Embodiment 2 can be implemented by combining with the modified example of Embodiment 1.

[0105] In Embodiment 1, the pressure in the furnace when growing the GaN crystal of the lower channel layer 16a is set to 200 mbar, similarly to the upper channel layer 16b. In contrast, in Embodiment 2, the pressure in the furnace when growing the GaN crystal of the lower channel layer 16a is set to be lower than the pressure in the furnace when growing the GaN crystal of the upper channel layer 16b.

[0106] The wafer 10 and the semiconductor device 20 of the second embodiment include a channel layer lower layer 16a containing GaN crystal grown under low pressure. If the pressure is low when growing GaN crystal, the amount of C introduced increases, so the C concentration of the channel layer lower layer 16a is higher than that of the first embodiment. Specifically, the C concentration is 1.1×10 17 atoms / cm 3 or more. In a manner corresponding to the C concentration, Si is also doped more than in Embodiment 1, and the Si concentration is also higher than in Embodiment 1. Specifically, it is 1.2×10 17 atoms / cm 3 or above.

[0107] In the channel layer lower layer forming step in the manufacturing method of the wafer 10 of the second embodiment, the temperature in the furnace is set to 800°C, the pressure is set to 50 mbar, and the V / III ratio is set to 500 to grow GaN crystal. That is, in the channel layer lower layer forming step, the pressure in the furnace when forming the channel layer lower layer 16a is lower than the pressure in the furnace when forming the channel layer upper layer 16b. The pressure in the furnace when forming the channel layer upper layer 16b is 200 mbar.

[0108] Here, use Figure 6 , which explains how to change the temperature and pressure in the furnace when growing the channel layer 16. Figure 6 In the graph, the vertical axis represents the temperature and pressure in the furnace, the horizontal axis represents the growth time, and the origin of the horizontal axis represents the time when the growth of the channel layer lower layer 16a is started. In addition, the portion between the left dotted line and the origin corresponds to the time when the channel layer lower layer formation step is performed, and the portion to the right of the right dotted line corresponds to the time when the channel layer upper layer formation step is performed.

[0109] like Figure 6 As shown, the temperature and pressure in the furnace when forming the lower layer 16a of the channel layer are different from the temperature and pressure in the furnace when forming the upper layer 16b of the channel layer. As mentioned above, the temperature and pressure when forming the lower layer 16a of the channel layer are lower than the temperature and pressure when forming the upper layer 16b of the channel layer.

[0110] In addition, if Figure 6As shown in FIG. 1 , a period (between the left dotted line and the right dotted line) for interrupting the growth is provided between the channel layer lower layer forming step and the channel layer upper layer forming step, and the temperature and pressure in the furnace are increased during this period, but the channel layer 16 (referred to as an intermediate layer) may also be grown during this period as in Embodiment 1. In this case, the supply of monosilane, which is a raw material of Si supplied in the channel layer lower layer forming step, is continued, and the supply amount of monosilane is gradually reduced, thereby being able to compensate for C with Si.

[0111] The wafer 10 , the semiconductor device 20 , and the method for manufacturing the wafer 10 according to the second embodiment of the present disclosure are configured as described above, and provide the following effects.

[0112] Generally speaking, if GaN crystals are grown at low temperatures, there is a problem of introducing a large amount of C, and the surface migration length of Ga becomes shorter, and the flatness of the lower layer 16a of the channel layer deteriorates. If the flatness of the lower layer 16a of the channel layer deteriorates, the upper layer 16b of the channel layer has a layer thickness of only tens of nanometers, so the flatness cannot be fully restored. As a result, the flatness of the interface between the upper layer 16b of the channel layer and the electron supply layer 17 deteriorates, and the mobility of 2DEG decreases.

[0113] In the manufacturing method of the chip 10 of the second embodiment of the present disclosure, in the step of forming the lower layer of the channel layer, the GaN crystal is grown at a pressure lower than that in the step of forming the upper layer of the channel layer. If the pressure is set to low when growing the GaN crystal, the amount of C introduced becomes more, but Si is doped in the lower layer 16a of the channel layer, and the generation of current collapse can be suppressed. In addition, by reducing the pressure in the step of forming the lower layer of the channel layer, the surface migration length of Ga can be lengthened, and the deterioration of flatness can be suppressed. Therefore, in the second embodiment, the generation of current collapse and the deterioration of flatness (reduction in mobility) can be suppressed at the same time.

[0114] Furthermore, since the wafer 10 and the semiconductor device 20 according to the second embodiment of the present disclosure are manufactured as described above, the occurrence of current collapse can be suppressed, and the flatness is high, and a decrease in the output of the semiconductor device 20 due to a decrease in the mobility of 2DEG is suppressed.

[0115] Implementation 3

[0116] Next, Embodiment 3 of the present disclosure will be described. The description of the same parts as those of the structure and manufacturing method described in Embodiment 1 will be omitted, and the following will describe the parts that are different from Embodiment 1. In addition, the wafer 10, the semiconductor device 20, and the manufacturing method of the wafer 10 of Embodiment 3 can be implemented by combining with the modified example of Embodiment 1 or Embodiment 2.

[0117] In the first embodiment, the V / III ratio in the furnace when growing the GaN crystal of the lower channel layer 16a is set to 500, similarly to the upper channel layer 16b. In contrast, in the third embodiment, the V / III ratio in the furnace when growing the GaN crystal of the lower channel layer 16a is set to be lower than the V / III ratio in the furnace when growing the GaN crystal of the upper channel layer 16b.

[0118] The wafer 10 and the semiconductor device 20 of the third embodiment include a channel layer lower layer 16a containing GaN crystals grown at a low V / III ratio. If the V / III ratio is reduced when growing GaN crystals, the amount of C introduced increases, so the C concentration of the channel layer lower layer 16a is higher than that of the first embodiment. Specifically, the C concentration is 1.1×10 17 atoms / cm 3 or more. In a manner corresponding to the C concentration, Si is also doped more than in Embodiment 1, and the Si concentration is also higher than in Embodiment 1. Specifically, it is 1.2×10 17 atoms / cm 3 or above.

[0119] In the channel layer lower layer forming step in the manufacturing method of the wafer 10 of the third embodiment, the temperature in the furnace is set to 800°C, the pressure is set to 200 mbar, and the V / III ratio is set to 200 to grow GaN. That is, in the channel layer lower layer forming step, the V / III ratio in the furnace when forming the channel layer lower layer 16a is lower than the V / III ratio in the furnace when forming the channel layer upper layer 16b. The V / III ratio in the furnace when forming the channel layer upper layer 16b is 500.

[0120] Here, use Figure 7 , which explains how to change the temperature and V / III ratio in the furnace when growing the channel layer 16. Figure 7 In the graph, the vertical axis represents the temperature in the furnace and the V / III ratio, the horizontal axis represents the growth time, and the origin of the horizontal axis represents the time when the growth of the channel layer lower layer 16a is started. In addition, the portion between the left dotted line and the origin corresponds to the time when the channel layer lower layer formation step is performed, and the portion to the right of the right dotted line corresponds to the time when the channel layer upper layer formation step is performed.

[0121] like Figure 7 As shown, the temperature and V / III ratio in the furnace when forming the lower layer 16a of the channel layer are different from the temperature and V / III ratio in the furnace when forming the upper layer 16b of the channel layer. As mentioned above, the temperature and V / III ratio when forming the lower layer 16a of the channel layer are lower than the temperature and V / III ratio when forming the upper layer 16b of the channel layer.

[0122] In addition, if Figure 7As shown, a period for interrupting the growth is provided between the channel layer lower layer forming step and the channel layer upper layer forming step (between the dotted line on the left and the dotted line on the right), and the temperature in the furnace is increased during this period. In addition, since GaN crystal is not grown during this period, raw materials are not supplied. Therefore, since the V / III ratio cannot be defined, it is not shown. In embodiment 3, as in embodiment 1, the channel layer 16 (referred to as an intermediate layer) may also be grown during the period in which the growth is interrupted. In this case, the V / III ratio is gradually increased, while the supply of the raw material of Si supplied in the channel layer lower layer forming step, that is, monosilane, is continued, and the supply amount of monosilane is gradually reduced, thereby being able to compensate for C with Si.

[0123] The wafer 10 , the semiconductor device 20 , and the method for manufacturing the wafer 10 according to the third embodiment of the present disclosure are configured as described above, and provide the following effects.

[0124] As described in Embodiment 2, when a GaN crystal is grown at a low temperature, the amount of C introduced increases, and the surface migration length of Ga becomes shorter, resulting in deterioration of flatness and a decrease in the mobility of 2DEG.

[0125] In the manufacturing method of the chip 10 of the third embodiment of the present disclosure, in the step of forming the lower layer of the channel layer, the GaN crystal is grown at a V / III ratio lower than that in the step of forming the upper layer of the channel layer. If the V / III ratio is lowered when growing the GaN crystal, the amount of C introduced becomes larger, but Si is doped in the lower layer 16a of the channel layer, and the generation of current collapse can be suppressed. In addition, by lowering the V / III ratio, the surface migration length of Ga can be lengthened, and the deterioration of flatness can be suppressed. Therefore, in the third embodiment, the generation of current collapse and the deterioration of flatness (reduction in mobility) can be suppressed at the same time.

[0126] Furthermore, since the wafer 10 and the semiconductor device 20 according to the third embodiment of the present disclosure are manufactured as described above, the occurrence of current collapse can be suppressed, and the flatness is high, and a decrease in the output of the semiconductor device 20 due to a decrease in the mobility of 2DEG is suppressed.

[0127] As described above, in the manufacturing method of the third embodiment, the channel lower layer forming step is performed under high pressure like the pressure in the first embodiment, but may be performed under low pressure like the second embodiment.

[0128] Implementation 4

[0129] Next, Embodiment 4 of the present disclosure will be described. The description of the same parts as those of the structure and manufacturing method described in Embodiment 1 will be omitted, and the following will describe the parts that are different from Embodiment 1. In addition, the wafer 10, the semiconductor device 20, and the manufacturing method of the wafer 10 of Embodiment 4 can be implemented by combining with the modified example of Embodiment 1, Embodiment 2, or Embodiment 3.

[0130] In the fourth embodiment, Si is doped not only in the channel lower layer 16 a but also in the back barrier layer 15 .

[0131] The wafer 10 and the semiconductor device 20 of the fourth embodiment include a back barrier layer 15 containing Si. The back barrier layer 15 is also formed at a low temperature like the lower channel layer 16a, and C is introduced into the layer and is not easily separated, so it contains C. Moreover, the concentration of Si contained in the back barrier layer 15 is higher than the concentration of C in the back barrier layer 15. Specifically, the concentration of C is 5×10 16 atoms / cm 3 or above, the concentration of Si is 6×10 16 atoms / cm 3 or above.

[0132] The manufacturing method of the chip 10 of embodiment 3 is different from that of embodiment 1. In the back barrier layer formation step, TMI (Tri-Methyl Indium, In(CH3)3) gas, TMGa gas, and a mixed gas of monosilane added to ammonia gas are introduced into the furnace, and 1nm of InGaN crystal constituting the back barrier layer 15 is grown on the buffer layer 14, and a back barrier layer 15 doped with Si is formed on the buffer layer 14.

[0133] Here, use Figure 8 , the concentration of C and the concentration of Si in the back barrier layer 15 and the channel layer 16 are described. Figure 8 In the graph, the vertical axis represents the concentration, and the horizontal axis represents the depth from the surface. The portion from the origin to the dotted line on the left is the depth corresponding to the upper channel layer 16b, the portion from the dotted line on the left to the dotted line on the right is the depth corresponding to the lower channel layer 16a, and the portion to the right of the dotted line on the right is the depth corresponding to the back barrier layer 15. The concentration of C is represented by the solid line, and the concentration of Si is represented by the single-point dashed line.

[0134] like Figure 8As shown, since a large amount of C is introduced into the channel layer lower layer 16a and the back barrier layer 15 of the GaN and InGaN crystals grown at low temperature, the concentration of C is higher than that of the channel layer upper layer 16b. In addition, since the back barrier layer 15 is formed at a higher pressure and a higher V / III ratio than the channel layer lower layer 16a, the concentration of C is lower than that of the channel layer lower layer 16a. The concentration of Si is higher than the concentration of C in each of the channel layer lower layer 16a and the back barrier layer 15. In addition, in Figure 8 In the embodiment, the C and Si concentrations of the channel lower layer 16 a are respectively higher than the C and Si concentrations of the back barrier layer 15 , but the C and Si concentrations of the back barrier layer 15 may be higher.

[0135] The wafer 10 , the semiconductor device 20 , and the method for manufacturing the wafer 10 according to the fourth embodiment of the present disclosure are configured as described above, and have the following effects.

[0136] Since the back barrier layer 15 is formed at a low temperature, the concentration of C is high. Therefore, C may capture electrons of 2DEG and cause current collapse. In addition, when current collapse occurs, the transient response characteristics deteriorate.

[0137] Since the wafer 10 and the semiconductor device 20 of the fourth embodiment of the present disclosure also contain Si in the back barrier layer 15, Si compensates for C, and can suppress the generation of current collapse and the deterioration of transient response characteristics caused by C in the back barrier layer 15. In addition, the generation of current collapse and the deterioration of transient response characteristics can be suppressed more reliably than in the case of the first embodiment in which Si is doped in the lower layer 16a of the channel layer.

[0138] Here, the growth conditions of the back barrier layer 15 are low temperature, high pressure, and high V / III ratio, which become conditions that deteriorate the flatness. However, since In has a surface activation effect (surfactant effect), it can lengthen the surface migration length of Ga, so the flatness will not be significantly deteriorated. However, by combining with embodiment 2 or embodiment 3, the back barrier layer 15 is formed at low pressure and low V / III ratio, thereby further improving the flatness.

[0139] In Embodiment 4, an example is described in which the concentration of Si contained in the back barrier layer 15 is higher than the concentration of C contained in the back barrier layer 15 . However, even if the concentration of Si is lower than that of C, Si can compensate for a part of C, thereby suppressing the occurrence of current collapse.

[0140] Industrial Applicability

[0141] The epitaxial wafer, the semiconductor device, and the method for manufacturing the epitaxial wafer disclosed in the present invention can be used as a high electron mobility transistor or in manufacturing a high electron mobility transistor.

[0142] Description of Reference Numerals

[0143] 10...epitaxial wafer (wafer); 12...substrate; 13...nucleation layer; 14...buffer layer; 15...back barrier layer; 16a...lower layer of channel layer; 16b...upper layer of channel layer; 17...electron supply layer; 20...semiconductor device; 21...source electrode; 22...drain electrode; 23...gate electrode.

Claims

1. An epitaxial wafer, characterized in that: The epitaxial wafer has: substrate; The buffer layer contains Al x Ga y In z A crystal represented by N is disposed on the substrate, wherein x+y+z=1, y>0; The back barrier layer contains Al x Ga y In z A crystal represented by N is disposed on the buffer layer, wherein x+y+z=1, y>0, z>0; The channel layer contains a composition of Al x Ga y In z A crystal represented by N is disposed on the back barrier layer, wherein x+y+z=1, y>0; and The electron supply layer contains Al x Ga y In z A crystal represented by N is disposed on the channel layer, wherein x+y+z=1, x>0, The channel layer is composed of an upper channel layer layer on the electron supply layer side and a lower channel layer layer on the back barrier layer side, The concentration of C in the lower layer of the channel layer is higher than the concentration of C in the upper layer of the channel layer. The lower layer of the channel layer comprises Si, The concentration of Si in the lower layer of the channel layer is higher than the concentration of C in the lower layer of the channel layer.

2. The epitaxial wafer according to claim 1, characterized in that The back barrier layer includes Si.

3. The epitaxial wafer according to claim 1 or 2, characterized in that: The channel layer has a thickness of 100 nm or less from an interface with the back barrier layer to an interface with the electron supply layer.

4. The epitaxial wafer according to any one of claims 1 to 3, characterized in that The buffer layer contains crystals represented by a composition formula of GaN, The back barrier layer contains a composition of Ga y In z A crystal represented by N, wherein y+z=1, y>0, z>0, The channel layer contains crystals represented by a composition formula of GaN.

5. A semiconductor device, characterized in that: The semiconductor device comprises: The epitaxial wafer according to any one of claims 1 to 4; A source electrode and a drain electrode are disposed on the electron supply layer of the epitaxial wafer with a gap therebetween; as well as The gate electrode is disposed between the source electrode and the drain electrode on the electron supply layer.

6. An epitaxial wafer, characterized in that: The epitaxial wafer has: substrate; The buffer layer contains Al x Ga y In z A crystal represented by N is disposed on the substrate, wherein x+y+z=1, y>0; The back barrier layer contains Al x Ga y In z A crystal represented by N is disposed on the buffer layer, wherein x+y+z=1, y>0, z>0; The channel layer contains a composition of Al x Ga y In z A crystal represented by N is disposed on the back barrier layer, wherein x+y+z=1, y>0; and The electron supply layer contains Al x Ga y In z A crystal represented by N is disposed on the channel layer, wherein x+y+z=1, x>0, The channel layer is composed of an upper channel layer layer on the electron supply layer side and a lower channel layer layer on the back barrier layer side, The concentration of C in the lower layer of the channel layer is higher than the concentration of C in the upper layer of the channel layer. The lower layer of the channel layer comprises Si, The back barrier layer comprises Si and C, The Si concentration of the back barrier layer is higher than the C concentration of the back barrier layer.

7. The epitaxial wafer according to claim 6, characterized in that The channel layer has a thickness of 100 nm or less from an interface with the back barrier layer to an interface with the electron supply layer.

8. The epitaxial wafer according to claim 6 or 7, characterized in that: The buffer layer contains crystals represented by a composition formula of GaN, The back barrier layer contains a composition of Ga y In z A crystal represented by N, wherein y+z=1, y>0, z>0, The channel layer contains crystals represented by a composition formula of GaN.

9. A semiconductor device, characterized in that: The semiconductor device comprises: The epitaxial wafer according to any one of claims 6 to 8; A source electrode and a drain electrode are disposed on the electron supply layer of the epitaxial wafer with a gap therebetween; as well as The gate electrode is disposed between the source electrode and the drain electrode on the electron supply layer.

10. A method for manufacturing an epitaxial wafer, characterized in that: The method for manufacturing the epitaxial wafer comprises the following steps: a configuration step of configuring the substrate in the furnace; The buffer layer forming step is to form a buffer layer having a composition formula of Al on the substrate. x Ga y In z N represents a buffer layer of a crystal, wherein x+y+z=1, y>0; The back barrier layer forming step is to form a layer having a composition formula of Al on the buffer layer. x Ga y In z N represents a back barrier layer of the crystal, wherein x+y+z=1, y>0, z>0; The channel layer forming step is to grow a layer having a composition formula of Al on the back barrier layer. x Ga y In z N represents a channel layer of a crystal, wherein x+y+z=1, y>0; and The electron supply layer forming step is to grow a layer containing a composition formula Al on the channel layer. x Ga y In z N represents a crystalline electron supply layer, wherein x+y+z=1, x>0, In the channel layer forming step, the temperature in the furnace when forming the channel layer lower layer on the back barrier layer side of the channel layer is lower than the temperature when forming the channel layer upper layer on the electron supply layer side of the channel layer, In the channel layer forming step, Si is doped into the channel layer lower layer when the channel layer lower layer is formed so that a concentration of Si becomes higher than a concentration of C in the channel layer lower layer.

11. The method for manufacturing an epitaxial wafer according to claim 10, characterized in that: In the channel layer forming step, the pressure in the furnace when forming the lower layer of the channel layer is made lower than the pressure in the furnace when forming the upper layer of the channel layer.

12. The method for manufacturing an epitaxial wafer according to claim 10 or 11, characterized in that: In the channel layer forming step, the V / III ratio, which is a value obtained by dividing the molar flow rate of the group V raw material supplied into the furnace when forming the lower layer of the channel layer by the molar flow rate of the group III raw material supplied into the furnace, is lower than the V / III ratio when forming the upper layer of the channel layer.

13. The method for producing an epitaxial wafer according to any one of claims 10 to 12, characterized in that: In the back barrier layer forming step, Si is doped into the back barrier layer when the back barrier layer is formed.

14. The method for manufacturing an epitaxial wafer according to claim 13, characterized in that: In the back barrier layer forming step, Si is doped into the back barrier layer when the back barrier layer is formed so that a concentration of Si becomes higher than a concentration of C in the back barrier layer.

15. The method for producing an epitaxial wafer according to any one of claims 10 to 14, characterized in that: The buffer layer contains crystals represented by a composition formula of GaN, The back barrier layer contains a composition of Ga y In z A crystal represented by N, wherein y+z=1, y>0, z>0, The channel layer contains a crystal represented by a composition formula of GaN, The electron supply layer contains Al x Ga y N represents a crystal, wherein x+y=1, x>0, y>0.

Citation Information

Patent Citations

  • High-electronic-mobility-rate transistor

    CN102856373A

  • High electron mobility transistor with n-p-n structure back barrier and manufacturing method thereof

    CN109638074A

  • Epitaxial substrate for electronic device and manufacturing method therefor

    JP2011040766A

  • Compound semiconductor device and manufacturing method of the same

    JP2019021704A

  • Nitride semiconductor device

    JP2019134153A