A ceramic bond diamond grinding wheel for thinning silicon carbide wafers and a preparation method thereof
By using a combination of high-concentration, low-strength diamond abrasives and low-strength, high-fluidity ceramic binders, combined with polymer microsphere hole-making and full-ring grooving cutting structures, the efficiency and quality problems in silicon carbide wafer thinning processing are solved. , achieving efficient and stable silicon carbide wafer thinning effect.
Patent Information
- Application Number
- CN202210881499.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-07-26
AI Technical Summary
During silicon carbide wafer thinning processing, it is difficult for existing diamond grinding wheels to achieve high-efficiency and high-quality thinning, and it is easy to cause debris and flying pieces. Domestic products cannot meet the performance requirements.
Using high-concentration and low-strength diamond abrasives combined with low-strength and high-fluidity ceramic binders and polymer microspheres to create holes, a ceramic-bonded diamond grinding wheel is prepared. It adopts a whole-ring grooved cutting segmented structure, and through specific sintering and mechanical Processing technology to form a grinding wheel with efficient grinding performance.
It achieves high-efficiency thinning of silicon carbide wafers, avoids the problem of debris and flying chips, improves processing quality, meets customers' high surface quality requirements, and the grinding wheel is not easy to break during use.
Smart Images

Figure CN115091376B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of superhard abrasive tools and preparation thereof, in particular to a ceramic bond diamond grinding wheel for thinning silicon carbide wafers. Background Art
[0002] Silicon carbide material has the advantages of large bandgap, good thermal conductivity, and high carrier mobility. It is one of the representatives of the third-generation semiconductor materials and is particularly suitable for applications such as high power, high temperature, high frequency, and radiation resistance. With the continued drive of 5G, photovoltaic power generation, and new energy vehicle demand, the rapid development of the silicon carbide wafer market has accelerated. Although silicon carbide has excellent performance as a wafer material, compared with the first-generation semiconductor silicon material, its Mohs hardness can reach 9.5, second only to diamond, which greatly increases the difficulty of thinning processing. In addition to the common low efficiency and unstable processing quality, it is also prone to flying flakes and fragments, which affects the promotion and application of silicon carbide wafers.
[0003] The thinning process of silicon wafers has reached a mature stage. There are corresponding products for resin bond, ceramic bond, and metal bond grinding wheels with diamond as abrasive. However, the thinning process of silicon carbide wafers is still in the exploratory development stage. The performance of diamond grinding wheels with three types of bonds is being improved. The current best solution is the ceramic bond diamond grinding wheel imported from Japan. Domestic related products, whether resin bond, ceramic bond, or metal bond diamond grinding wheels, cannot meet the performance requirements. Summary of the invention
[0004] The purpose of the present invention is to provide a ceramic bond diamond grinding wheel for thinning silicon carbide wafers, so as to achieve high-efficiency and high-surface-quality thinning processing of silicon carbide wafers.
[0005] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:
[0006] A ceramic bond diamond grinding wheel for thinning silicon carbide wafers, the preparation method of which comprises the following steps:
[0007] (1) diamond abrasive, ceramic binder, pore-forming agent and phenolic resin powder are mixed to obtain an abrasive layer mixture; and the abrasive layer mixture is hot-pressed to obtain an abrasive layer blank;
[0008] (2) sintering the abrasive layer blank to obtain a ceramic bond diamond grinding wheel layer;
[0009] (3) The ceramic bond diamond grinding wheel layer is conventionally bonded to an aluminum substrate and then subjected to conventional mechanical processing to obtain a ceramic bond diamond grinding wheel for thinning silicon carbide wafers.
[0010] In the above technical solution, the mass ratio of the diamond abrasive, the ceramic binder, the pore-forming agent, and the phenolic resin powder is (50-70): (10-30): (10-25): (5-15), preferably (50-58): (18-24): (11-18): (8-13).
[0011] In the above technical scheme, the ceramic binder includes silicon dioxide, boric acid, sodium carbonate, lithium carbonate, and manganese oxide; preferably, the ceramic binder is prepared from silicon dioxide, boric acid, sodium carbonate, lithium carbonate, and manganese oxide. Further preferably, by mass percentage, silicon dioxide is 35% to 50%, boric acid is 30 to 40%, sodium carbonate is 2.5 to 5%, lithium carbonate is 8 to 15%, and the balance is manganese oxide. Preferably, silicon dioxide is 40% to 50%, boric acid is 33 to 38%, sodium carbonate is 2.5 to 4%, lithium carbonate is 11 to 15%, and the balance is manganese oxide.
[0012] In the above technical solution, the preparation process of the ceramic binder is as follows:
[0013] (1) Mix the raw materials uniformly according to the following mass percentages: 35% to 50% silicon dioxide, 30% to 40% boric acid, 2.5% to 5% sodium carbonate, 8% to 15% lithium carbonate, and 1% to 3% manganese oxide;
[0014] (2) The obtained mixture is melted in a frit furnace at 1350°C to 1500°C, and after cooling, it is ball-milled into powder, which passes through a 325-mesh standard sieve to obtain a ceramic binder.
[0015] In the above technical solution, the pore-forming agent is PS (polystyrene) resin balls with a particle size of 50 to 100 μm.
[0016] In the above technical solution, in step (1), mixing is carried out in a grinding mixer for 1 to 3 hours; the hot pressing pressure is 10 to 20 tons, the upper and lower plate temperatures of the press are 170 to 200° C., and the hot pressing time is 15 to 30 minutes.
[0017] In the above technical solution, in step (1), the abrasive layer blank is a grinding wheel grinding layer full ring structure; the grinding layer of the present invention is integrally formed and finally grooved, thereby improving the grinding wheel processing effect.
[0018] In the above technical scheme, in step (2), the sintering process is to increase the temperature from room temperature to 280-320°C over 1.5-3 hours, keep it warm for 1.5-2.5 hours, then increase the temperature to 480-520°C over 2.5-3.5 hours, keep it warm for 4.5-5.5 hours, then increase the temperature to 750-800°C over 1.5-2.5 hours, keep it warm for 2.5-3.5 hours, then cool it to 400-550°C over 1-3 hours, keep it warm for 0.5-1.5 hours, and finally cool it naturally with the furnace.
[0019] In the above technical solution, in step (3), the mechanical processing is conventional mechanical processing, such as turning, etc.; the processing order of the grinding wheel layer is: grinding the outer ring of the grinding wheel layer, grinding the inner ring of the grinding wheel layer, grinding the end surface of the grinding wheel layer, and the grinding wheel layer is divided into 32 grooves according to the angle, and the groove width is 2 mm (as a specific example).
[0020] The applicant found in the production test that the processing of silicon carbide wafers is different from that of silicon wafers. The silicon wafer thinning grinding wheel can improve self-sharpening by making a large number of holes and reducing the hardness of the grinding wheel, so as to realize the processing of silicon wafers with three kinds of binders: resin, ceramic and metal. However, in the processing of silicon carbide wafers, due to the high hardness of silicon carbide, this method causes the grinding wheel to be consumed too quickly, and it is impossible to remove the surplus of silicon carbide wafers. The common domestic solution is to increase the hardness of the grinding wheel or the strength of the binder. Although this method can initially thin silicon carbide, it is easy to cause wafer fragments and flying pieces as the thickness of the wafer decreases. The present invention redesigns the grinding wheel idea, adopts high-concentration and low-strength diamond abrasive combined with low-strength and high-fluidity ceramic binder, and polymer microsphere pore making, and the obtained grinding wheel unexpectedly realizes high-efficiency processing of silicon carbide wafers, and the processing quality is good, which meets customer requirements.
[0021] Due to the application of the above technical solution, the present invention has the following advantages compared with the existing silicon carbide wafer thinning grinding wheel technology:
[0022] 1. The grinding wheel of the present invention can effectively remove the excess in the process of thinning silicon carbide wafers. Practice has shown that resin and metal binders cannot produce high-concentration diamond grinding wheels due to their own characteristics, especially cannot be used to remove the excess of silicon carbide wafers.
[0023] 2. The technical solution of the present invention changes the existing design concept of the binder. The binder has good wettability to diamonds. During the cooling process after melting, the diamond particles are completely wrapped. Different from the usual diamond embedded in the binder, the contact points between the diamond particles are bonded together by a small amount of binder, and there are a large number of voids between the particles. The grinding wheel can present a "scattered beans to make soldiers" state in the microstructure; and the diamond particles fall off quickly after being blunted. At the same time, due to the high concentration formula (referring to the volume concentration after molding), there are more diamond particles, and the surrounding diamonds begin to participate in grinding, which does not affect the sharpness of the grinding wheel.
[0024] 3. The ceramic bond diamond grinding wheel for thinning silicon carbide wafers of the present invention adopts a full-ring slotted cutting segmented structure for the grinding wheel layer, and retains a non-cutting layer with a thickness of 1-1.5 mm. Compared with the existing thinning grinding wheel agglomerate inlaid bonding structure, the full-ring structure can adopt a mold self-rotating scraping mode during preparation, and the hardness uniformity of the entire grinding wheel is better, while the agglomerate type can only be scraped manually, and the agglomerate hardness is uneven; the slotted cutting segmented structure is adopted, which retains the advantage of easy chip removal. At the same time, the full-ring slotted cutting segmented structure grinding wheel has a smaller dynamic imbalance during processing and more stable processing.
[0025] In summary, the present invention develops a new grinding wheel for thinning silicon carbide wafers, avoiding the problems of wafer fragmentation and flying flakes caused by existing grinding wheels; retaining a certain thickness of non-cutting layer can increase the strength of the entire grinding wheel layer, and the grinding wheel layer is not easy to break during machining and use of the grinding wheel; unexpectedly achieves high-efficiency processing of silicon carbide wafers with good processing quality, meeting customer requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a physical picture of the grinding wheel of the present invention in the embodiment;
[0027] Figure 2 Schematic diagram of the grinding wheel layer of the full-ring slotting and cutting segmented structure of the present invention in the embodiment;
[0028] Among them: 1. Grinding wheel layer; 2. Matrix;
[0029] Figure 3 3 is a microstructure diagram of the grinding layer of the grinding wheel of the present invention in the embodiment. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0031] The ceramic bond diamond grinding wheel for silicon carbide wafer thinning prepared by the present invention is a grinding wheel layer with a full-ring slotted cutting segmented structure, retaining a non-cutting layer with a thickness of 1 to 1.5 mm, and is annular as a whole. The raw materials of the present invention are all commercially available products, and the specific preparation method and processing method are prior art. The mechanical processing is conventional mechanical processing, such as lathe processing, etc. As an example, the processing sequence of the grinding wheel layer is: grinding of the outer ring of the grinding wheel layer, grinding of the inner ring of the grinding wheel layer, grinding of the end face of the grinding wheel layer, and the grinding layer is grooved evenly at an angle, with a groove width of 2 mm, and a non-cutting layer with a thickness of 1 mm is retained.
[0032] The ceramic binder of the present invention is a low-strength, high-fluidity ceramic binder, and its preparation process is as follows: the raw materials are conventionally mixed according to the following mass percentages: 45% silicon dioxide, 36% boric acid, 3% sodium carbonate, 14% lithium carbonate, and 2% manganese oxide; the obtained mixture (10 kg) is smelted at 1450° C. in a frit furnace, ball-milled into powder after cooling, and passed through a 325-mesh standard sieve. The material under the sieve is the ceramic binder, which is used in the embodiments (unless otherwise specified).
[0033] Unless otherwise specified, in the following examples, the diamond abrasive is micron-sized particles, Eagle, EA-M19; the pore-forming agent is PS resin balls with a particle size of 50 to 100 μm.
[0034] Example 1: A ceramic bond diamond grinding wheel for thinning silicon carbide wafers, with specifications of 250×25×190×3×5 mm, is prepared as follows:
[0035] (1) diamond abrasive, ceramic binder, pore-forming agent and phenolic resin powder in a mass ratio of 55:20:15:10 are mixed in a grinding mixer for 2 hours to obtain an abrasive layer mixture; the abrasive layer mixture is hot-pressed to obtain an abrasive layer blank, which is a grinding wheel grinding layer full ring structure, and the specific hot-pressing process is a pressure of 15 tons, a temperature of the upper and lower plates of the press at 180° C., and a hot-pressing time of 20 minutes;
[0036] (2) Sintering the abrasive layer blank to obtain a ceramic bond diamond wheel layer. The specific sintering process is to heat the temperature from room temperature to 300°C over 2 hours, keep it at that temperature for 2 hours, then heat it to 500°C over 3 hours, keep it at that temperature for 5 hours, then heat it to 760°C over 2 hours, keep it at that temperature for 3 hours, then cool it down to 500°C over 2 hours, keep it at that temperature for 1 hour, and finally cool it naturally with the furnace;
[0037] (3) This step is a conventional technology. The ceramic bond diamond grinding wheel layer is conventionally bonded to the existing aluminum substrate, and then mechanically processed to obtain a ceramic bond diamond grinding wheel for silicon carbide wafer thinning. The grinding wheel is a grinding wheel layer with a full-ring slotted cutting segmented structure, and a non-cutting layer with a thickness of 1 mm is retained. The actual picture is shown in Figure 1 The processing sequence of the grinding wheel layer is: grinding of the outer ring of the grinding wheel layer, grinding of the inner ring of the grinding wheel layer, grinding of the end surface of the grinding wheel layer, and the grinding wheel layer is grooved evenly according to the angle, with a groove width of 2mm, see Figure 2 The grinding wheel layer is bonded to the substrate, and the grooves are opened and the non-cutting layer is retained. It has the advantages of easy chip removal of the agglomerate type and the stability of whole ring preparation. At the same time, because the grooves can be evenly opened, the dynamic imbalance of the grinding wheel is smaller during use, and the processing is more stable. The non-cutting layer with retained thickness can increase the strength of the entire grinding wheel layer. The grinding wheel layer is not easy to break during machining and use.
[0038] Figure 3This is a microscopic photograph of the above-mentioned grinding wheel. It can be seen from the figure that the ceramic binder diamond grinding wheel for thinning silicon carbide wafers of the present invention is different from the existing diamond embedded in the binder. The contact points between the diamond particles are bonded together by a small amount of binder. There are a large number of voids between the particles. The grinding wheel can present a "scattered beans to make soldiers" state in the microstructure, and can achieve high-efficiency and high-surface quality thinning processing of silicon carbide wafers.
[0039] Processing Example
[0040] Table 1 is a comparison of the thinning grinding wheel of the present invention and the existing grinding wheel for processing silicon carbide wafers of the same specifications. It can be seen from the table that during the processing of the existing metal bond grinding wheel, the resistance is large, and the wafer is easy to fly out of the suction cup, resulting in damage to the wafer; the existing resin grinding wheel has poor sharpness and easily causes the edge of the wafer to break; therefore, these two types of grinding wheels are not used for silicon carbide wafer processing in industry. At present, the industry uses ceramic bond silicon wafer grinding wheels to process silicon carbide wafers. The commercially available ceramic bond silicon wafer grinding wheels with the best market response are used as a control. They consume quickly and have low processing efficiency. The silicon carbide wafer thinning grinding wheel of the present invention has greatly reduced self-loss and increased wafer thinning efficiency by about 4 times. Like the existing high-performance grinding wheels, the appearance and roughness of the silicon carbide wafers processed by the present invention are very good.
[0041]
[0042] Embodiment 2
[0043] On the basis of Example 1, the sintering process of step (2) was adjusted to increase the temperature from room temperature to 300°C over 2 hours, keep it at that temperature for 2 hours, then increase the temperature to 500°C over 3 hours, keep it at that temperature for 5 hours, then increase the temperature to 760°C over 2 hours, keep it at that temperature for 3 hours, and then naturally cool it with the furnace; the rest remained unchanged, and a ceramic bond diamond grinding wheel for thinning silicon carbide wafers was obtained. Experiments on processing silicon carbide wafers of the same specifications found that the wear ratio of the grinding wheel was relatively low, at 1:11.88.
[0044] Embodiment 3
[0045] The raw materials were mixed evenly according to the following mass percentages: 45% silicon dioxide, 36% boric acid, 3% sodium carbonate, 14% lithium carbonate, and 2% aluminum oxide; the resulting mixture (10 kg) was melted in a frit furnace at 1450°C, ball-milled into powder after cooling, and passed through a 325-mesh standard sieve, and the material under the sieve was the ceramic binder.
[0046] Only the ceramic binder was replaced, and the rest was prepared according to Example 1. A ceramic binder diamond grinding wheel was prepared. Experiments on processing silicon carbide wafers of the same specifications found that edge fragments were present.
[0047] Embodiment 4
[0048] Only the diamond was replaced with high-strength diamond (Eagle, EA-M60), and the rest was prepared according to Example 1 to obtain a ceramic bond diamond grinding wheel. Experiments on processing silicon carbide wafers of the same specification found that the surface of the product after processing by the grinding wheel had obvious scratches.
[0049] Embodiment 5 A ceramic bond diamond grinding wheel for thinning silicon carbide wafers is prepared as follows:
[0050] (1) diamond abrasive, ceramic binder, pore-forming agent and phenolic resin powder in a mass ratio of 60:25:8:7 are mixed in a grinding mixer for 2 hours to obtain an abrasive layer mixture; the abrasive layer mixture is hot-pressed to obtain an abrasive layer blank, which is a grinding wheel grinding layer full ring structure, and the specific hot-pressing process is a pressure of 15 tons, a temperature of the upper and lower plates of the press at 180° C., and a hot-pressing time of 30 minutes;
[0051] (2) Sintering the abrasive layer blank to obtain a ceramic bond diamond wheel layer. The specific sintering process is to heat the temperature from room temperature to 300°C over 2 hours, keep it at that temperature for 2 hours, then heat it to 500°C over 3 hours, keep it at that temperature for 5 hours, then heat it to 750°C over 2 hours, keep it at that temperature for 3 hours, then cool it to 500°C over 2 hours, keep it at that temperature for 1 hour, and finally cool it naturally with the furnace;
[0052] (3) This step is a conventional technique. Referring to Example 1, a ceramic bond diamond grinding wheel layer is conventionally bonded to an aluminum substrate, and then mechanically processed to obtain a ceramic bond diamond grinding wheel for thinning silicon carbide wafers.
[0053] Embodiment 6 A ceramic bond diamond grinding wheel for thinning silicon carbide wafers is prepared as follows:
[0054] (1) diamond abrasive, ceramic binder, pore-forming agent and phenolic resin powder in a mass ratio of 58:22:12:8 are mixed in a grinding mixer for 1.5 hours to obtain an abrasive layer mixture; the abrasive layer mixture is hot-pressed to obtain an abrasive layer blank, which is a grinding wheel grinding layer full ring structure, and the specific hot-pressing process is a pressure of 10 tons, a temperature of the upper and lower plates of the press at 170° C., and a hot-pressing time of 25 minutes;
[0055] (2) Sintering the abrasive layer blank to obtain a ceramic bond diamond wheel layer. The specific sintering process is to heat the temperature from room temperature to 300°C over 2 hours, keep it at that temperature for 2 hours, then heat it to 500°C over 3 hours, keep it at that temperature for 5 hours, then heat it to 780°C over 2 hours, keep it at that temperature for 3 hours, then cool it down to 500°C over 2 hours, keep it at that temperature for 1 hour, and finally cool it naturally with the furnace;
[0056] (3) This step is a conventional technique. Referring to Example 1, a ceramic bond diamond grinding wheel layer is conventionally bonded to an aluminum substrate, and then mechanically processed to obtain a ceramic bond diamond grinding wheel for thinning silicon carbide wafers.
[0057] The grinding wheel processing effects of the fifth and sixth embodiments are not as good as that of the first embodiment, but both can be used to process silicon carbide wafers.
[0058] The actual experiment found that the processing of silicon carbide wafers is different from that of silicon wafers. The silicon wafer thinning grinding wheel can improve self-sharpening by a large number of holes and reduce the hardness of the grinding wheel, and realize the processing of silicon wafers by three kinds of binders: resin, ceramic and metal. However, this method is not applicable in the processing of silicon carbide wafers, and the excess of silicon carbide wafers cannot be removed at all. The common domestic solution is to increase the hardness of the grinding wheel or increase the strength of the binder. Although this method can initially thin silicon carbide, it is easy to cause wafer fragments and flying pieces as the thickness of the wafer decreases. In particular, the resin grinding wheel and metal grinding wheel for processing silicon wafers cannot be used for processing silicon carbide wafers from experiments. In the present invention, the grinding wheel idea is redesigned, and high-concentration low-strength diamond, low-strength high-fluidity ceramic binder and high-volume content diamond micropowder particles are used to combine polymer holes to ensure that the excess can be effectively removed during the thinning process of silicon carbide wafers and the processing effect is good, while significantly improving efficiency and ensuring processing quality.
Claims
1. A ceramic bond diamond grinding wheel for thinning silicon carbide wafers, characterized in that: The preparation method comprises the following steps: (1) diamond abrasive, ceramic binder, pore-forming agent and phenolic resin powder are mixed to obtain an abrasive layer mixture; and the abrasive layer mixture is hot-pressed to obtain an abrasive layer blank; (2) sintering the abrasive layer blank to obtain a ceramic bond diamond grinding wheel layer; (3) conventionally bonding the ceramic bond diamond grinding wheel layer to an aluminum substrate, and then performing conventional mechanical processing to obtain a ceramic bond diamond grinding wheel for thinning silicon carbide wafers; The mass ratio of the diamond abrasive, ceramic binder, pore-forming agent and phenolic resin powder is (50-70): (10-30): (10-25): (5-15); the ceramic binder comprises silicon dioxide, boric acid, sodium carbonate, lithium carbonate and manganese oxide; the diamond abrasive is a low-strength diamond abrasive; in terms of mass percentage, silicon dioxide is 35%-50%, boric acid is 30-40%, sodium carbonate is 2.5-5%, lithium carbonate is 8-15%, and the balance is manganese oxide.
2. The ceramic bond diamond grinding wheel for thinning silicon carbide wafers according to claim 1, characterized in that: The pore-forming agent is PS resin balls with a particle size of 50 to 100 μm; the abrasive layer blank is a grinding wheel grinding layer full ring structure.
3. The ceramic bond diamond grinding wheel for thinning silicon carbide wafer according to claim 1, characterized in that: In step (1), mixing is carried out in a grinding mixer for 1 to 3 hours; the hot pressing pressure is 10 to 20 tons, the temperature of the upper and lower plates of the press is 170 to 200° C., and the hot pressing time is 15 to 30 minutes; in step (2), the sintering process is to heat the temperature from room temperature to 280 to 320° C. over 1.5 to 3 hours, keep the temperature for 1.5 to 2.5 hours, then heat the temperature to 480 to 520° C. over 2.5 to 3.5 hours, keep the temperature for 4.5 to 5.5 hours, then heat the temperature to 750 to 800° C. over 1.5 to 2.5 hours, keep the temperature for 2.5 to 3.5 hours, then cool the temperature to 400 to 550° C. over 1 to 3 hours, keep the temperature for 0.5 to 1.5 hours, and finally cool naturally with the furnace.
4. A ceramic bond diamond grinding wheel for thinning a silicon carbide wafer prepared according to the ceramic bond diamond grinding wheel for thinning a silicon carbide wafer according to claim 1.
5. Use of the ceramic bond diamond grinding wheel for silicon carbide wafer thinning as claimed in claim 4 in wafer thinning.
6. A method for thinning a silicon carbide wafer using the ceramic bond diamond grinding wheel for thinning a silicon carbide wafer as claimed in claim 4.
7. The method according to claim 6, characterized in that The wafer is a silicon carbide wafer.
Citation Information
Patent Citations
Grinding block for grinding disc for processing alloy materials, preparation method of grinding block and grinding disc