A two-dimensional Ti 3 C 2 T x Gas sensor of MOS composite material and preparation method thereof

By depositing MOS nanoparticles on the surface of the Ti3C2Tx film, the Ti3C2Tx/MOS composite material is prepared, which solves the problems of high temperature stability and slow response of MXene materials of existing MOS sensors, and realizes a gas sensor with high sensitivity and stability at room temperature, which is suitable for large-scale applications. scale production.

CN115096953BActive Publication Date: 2024-10-22SHANGHAI MARITIME UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210646831.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-08
Publication Date
2024-10-22
Estimated Expiration
2042-06-08

AI Technical Summary

Technical Problem

Existing metal oxide semiconductor (MOS) gas sensors show high sensitivity at high temperatures, but have stability issues and are not suitable for flammable and explosive gas detection. MXene materials such as Ti3C2Tx have low response values, slow speeds and resistance values ​​at room temperature. It is difficult to recover and cannot meet actual application requirements.

Method used

Magnetron sputtering technology is used to uniformly deposit MOS nanoparticles on the surface of the Ti3C2Tx film to prepare Ti3C2Tx/MOS composite materials. The synergy is used to improve the gas-sensing performance. The preparation process is simple and suitable for large-scale production.

Benefits of technology

A gas sensor with excellent sensitivity, selectivity and stability at room temperature has been realized, which solves the high power consumption and safety problems of traditional MOS sensors. The process is simple and reliable, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115096953B_ABST
    Figure CN115096953B_ABST
Patent Text Reader

Abstract

The invention discloses a two-dimensional Ti3C2T x / MOS composite material gas sensor and preparation method thereof, the preparation method comprises the following steps: providing a planar electrode substrate; weighing a multilayer Ti3C2T x The material was intercalated and ultrasonically dispersed to obtain a few-layer Ti3C2T x dispersion; the few-layer Ti3C2T x The dispersed liquid is dropwise applied to the upper surface of the planar electrode substrate and dried to form a Ti3C2T x Thin film; Provide MOS target material, through magnetron sputtering on Ti3C2T x A MOS film is deposited on the surface of the film to obtain a planar electrode substrate with a double-layer gas-sensitive material film, and then assembled to complete the two-dimensional Ti3C2T x Preparation of gas sensors of MOS composite materials. The sensor prepared by the preparation method of the present invention has excellent sensitivity, selectivity, cycle stability and recoverability, and the preparation method is simple and reliable, with high repeatability, and is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of gas sensors and specifically relates to a two-dimensional Ti3C2T x / MOS composite material gas sensor and preparation method thereof. Background Art

[0002] A gas sensor is a device that can detect harmful gas pollutants and convert gas concentrations into electrical signals. Gas sensing equipment has been used in military and public security, industrial and agricultural production, and environmental monitoring. Humans need to use gas sensors to detect these pollutants sensitively, accurately, and quickly to overcome the limitations of human perception. Among the various types of gas sensors, metal oxide semiconductor (MOS) gas sensors have attracted widespread attention due to their simple structure, high sensitivity, low cost, and long life. However, MOS gas sensing materials only show high sensitivity and good selectivity at high temperatures, such as SnO2 (400°C), ZnO (400°C), and W 18 O 49 (300°C). High temperature environment will affect the stability of the sensor and pose a safety risk to the detection of flammable and explosive gases, which greatly limits the development prospects of MOS sensing materials.

[0003] MXene is a new type of two-dimensional transition metal carbon / nitride, generally represented by M n +1X n T x (n=1-3), where M is a transition metal element (such as Ti, V, Nb, Ta, Cr, Mo, Hf, etc.), X is carbon or nitrogen, T x Indicates surface functional groups (-OH, -O or -F). Currently discovered MXenes mainly include Ti3C2T x 、Ti2CT x 、V2CT x 、Nb2CT x 、Mo2CT x 、Ti4N3T x etc. Ti3C2T x As the most representative MXene material, it has been applied in the field of gas sensors because its abundant oxygen-containing functional groups on the surface can effectively adsorb gas molecules, making it have good gas sensitivity at room temperature. xThe sensor has the disadvantages of low response value (about 0.001-0.06), slow response and recovery speed, and its resistance value is difficult to restore to the initial state, which cannot meet the needs of practical applications. Although researchers have made some efforts to improve the gas sensing performance of MXene, there are still problems such as complex preparation, uneven or stable gas-sensitive materials, and poor binding, which affect the sensitivity and selectivity of gas sensors.

[0004] In summary, there is an urgent need in this field to develop a gas sensor that is simple to prepare, highly repeatable, and has excellent sensitivity, selectivity, and stability. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a two-dimensional Ti3C2T x / MOS composite material gas sensor and preparation method thereof, the method comprising: using magnetron sputtering technology to deposit Ti3C2T x MOS (SnO2, ZnO, WO3) nanoparticles are uniformly deposited on the film surface to prepare different types of Ti3C2T x / MOS composite materials use the synergistic effect between different materials to effectively improve the gas sensitive performance of the sensor. The prepared gas sensor has good response characteristics and excellent selectivity and stability, and the preparation process is simple and suitable for large-scale production.

[0006] In order to achieve the above object, the present invention first provides a two-dimensional Ti3C2T x A method for preparing a gas sensor of a MOS composite material comprises the following steps:

[0007] S1, providing a planar electrode substrate;

[0008] S2, weigh multilayer Ti3C2T x The material was intercalated and ultrasonically dispersed to obtain a few-layer Ti3C2T x Dispersion liquid;

[0009] S3, the few-layer Ti3C2T x The dispersed liquid droplets are applied to the upper surface of the planar electrode substrate and dried to form Ti3C2T x film;

[0010] S4, providing a MOS target material, and depositing it on the Ti3C2T x A MOS film is deposited on the surface of the film to obtain a planar electrode substrate with a double-layer gas-sensitive material film;

[0011] S5, the planar electrode substrate obtained in step S4 is subsequently assembled to complete the two-dimensional Ti3C2T x Preparation of gas sensors based on MOS composite materials.

[0012] Preferably, the MOS target material is selected from any one of SnO2, ZnO, and WO3.

[0013] Preferably, in step S4, the magnetron sputtering conditions are: the vacuum degree is 5×10 -4 Pa, the sputtering power is 100W, the sputtering pressure is 2Pa, and the sputtering time is 60-360s.

[0014] Furthermore, the sputtering time is 300 s.

[0015] Preferably, the specific operations of step S2 are:

[0016] S2.1, weigh multilayer Ti3C2T x The material was added to DMSO for intercalation treatment. After centrifugation, precipitation and washing, the precipitate was dispersed in deionized water again to form a multilayer Ti3C2T x Dispersion liquid;

[0017] S2.2, the multilayer Ti3C2T obtained in step S2.1 x The dispersion was subjected to ultrasonic exfoliation in an ice bath to obtain a few-layer Ti3C2T x Dispersion.

[0018] Preferably, the multilayer Ti3C2T x The thickness of the material is 100-200nm.

[0019] Preferably, in step S2.2, the conditions for the ultrasonic stripping treatment are: introducing nitrogen or argon, ultrasonic power of 50-1000 W, and ultrasonic time of 60-600 min.

[0020] Preferably, in step S2.1, the centrifugal conditions are: rotation speed 1000-8000 rpm, time 5-20 min.

[0021] On the other hand, the present invention also provides a two-dimensional Ti3C2T based on the preparation method according to any one of the above x / MOS composite material gas sensor, the gas sensor comprises from bottom to top: a planar electrode substrate, a Ti3C2T x film and MOS film, wherein the Ti3C2T x Together with the MOS film, it forms the gas-sensitive material layer.

[0022] Compared with the prior art, the beneficial effects of the present invention are:

[0023] 1. The present invention adopts a method of first drip coating and drying followed by magnetron sputtering deposition to prepare MXene (Ti3C2Tx ) / MOS composite materials, on the one hand, the obtained film has high purity, good density, uniform film formation, and good stability and bonding, overcoming the MXene (Ti3C2T x ) and the problem of uneven composite between MOS materials; on the other hand, the preparation process is simple and reliable, in which the sputtering process can control the coating thickness and the film particle size by changing the parameter conditions, with high repeatability and suitable for large-scale production.

[0024] 2. The present invention is based on MXene (Ti3C2T x ) film, which fully utilizes the advantages of the two types of sensitive components and produces a synergistic sensitization effect. The increase in active sites on the composite surface and the electron transfer of the heterojunction effectively improve the sensitivity, selectivity, cycle stability and recoverability of the sensor.

[0025] 3. The sensor prepared by the method of the present invention can work at room temperature, solving the problems of high power consumption and safety of use of traditional MOS gas sensors. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The present invention is based on two-dimensional Ti3C2T x Flow chart of the preparation method of gas sensor of / MOS composite material.

[0027] Figure 2 It is a schematic diagram of the structure of the planar electrode substrate in the gas sensor of the present invention.

[0028] Figure 3 The present invention is based on two-dimensional Ti3C2T x Schematic diagram of the structure of the gas sensor based on / MOS composite material.

[0029] Figure 4 The present invention is based on two-dimensional Ti3C2T x Schematic cross-sectional view of a gas sensor made of / MOS composite material.

[0030] Figure 5 This is the response recovery curve of the sensor prepared in the comparative example of the present invention to 5ppm-500ppm ammonia.

[0031] Figure 6 This is the response recovery curve of the sensor prepared in Example 1 of the present invention to 5ppm-500ppm ammonia.

[0032] Figure 7 This is the cyclic response curve of the sensor prepared in Example 1 of the present invention to 100 ppm ammonia.

[0033] Figure 8This is the response recovery curve of the sensor prepared in Example 2 of the present invention to 5ppm-500ppm ammonia.

[0034] Fig. 9 This is the cyclic response curve of the sensor prepared in Example 2 of the present invention to 100 ppm ammonia.

[0035] Fig.10 This is the response recovery curve of the sensor prepared in Example 3 of the present invention to 5ppm-500ppm ammonia.

[0036] Fig.11 This is the cyclic response curve of the sensor prepared in Example 3 of the present invention to 100 ppm ammonia.

[0037] Fig.12 The selectivity test graphs of the sensors prepared in Examples 1-3 of the present invention and the comparative example to 500 ppm formaldehyde, acetone, ethanol, isopropanol and ammonia are shown.

[0038] Figure ID

[0039] Planar electrode substrate 1; Au interdigital electrode 11; planar ceramic substrate 12; copper wire 3; Ti3C2T x Film 2; MOS film 3. DETAILED DESCRIPTION

[0040] To make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. The components of the embodiments of the present application usually described and shown in the drawings here can be arranged and designed in various configurations. Therefore, the following detailed description of the embodiments of the present application provided in the drawings is not intended to limit the scope of the application claimed for protection, but merely represents the selected embodiments of the present application. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application.

[0041] In the description of the present application, it should be noted that the terms "upper", "lower", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, or the orientations or positional relationships in which the inventive product is usually placed when in use. These are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0042] As mentioned above, in view of the shortcomings of the prior art, the applicant of the present invention, after long-term research and extensive practice, first provides a two-dimensional Ti3C2Tx Preparation method of gas sensor of / MOS composite material, such as Figure 1 As shown, the following steps are included:

[0043] S1, providing a planar electrode substrate;

[0044] S2, weigh multilayer Ti3C2T x The material was intercalated and ultrasonically dispersed to obtain a few-layer Ti3C2T x Dispersion liquid;

[0045] S3, the few-layer Ti3C2T x The dispersed liquid droplets are applied to the upper surface of the planar electrode substrate and dried to form Ti3C2T x Film; It should be noted that the upper surface mentioned here refers to the side of the planar electrode substrate with the electrode;

[0046] S4, providing a MOS target material, and depositing it on the Ti3C2T x A MOS film is deposited on the surface of the film to obtain a planar electrode substrate with a double-layer gas-sensitive material film;

[0047] S5, the planar electrode substrate obtained in step S4 is subsequently assembled to complete the two-dimensional Ti3C2T x Preparation of gas sensor of MOS composite material. In some embodiments, this step is: the planar electrode substrate loaded with gas sensitive material is welded to the hexagonal base, and the hexagonal base is used to connect the sensing substrate and the test cavity.

[0048] Preferably, the MOS target material is selected from any one of SnO2, ZnO, and WO3.

[0049] Preferably, in step S4, the magnetron sputtering conditions are: the vacuum degree is 5×10 -4 Pa, the sputtering power is 100W, the sputtering pressure is 2Pa, and the sputtering time is 60-360s.

[0050] Furthermore, in some embodiments, the sputtering time is 300 s.

[0051] Preferably, the specific operations of step S2 are:

[0052] S2.1, weigh multilayer Ti3C2T x The material was added to DMSO for intercalation treatment. After centrifugation, precipitation and washing, the precipitate was dispersed in deionized water again to form a multilayer Ti3C2T x Dispersion liquid;

[0053] S2.2, the multilayer Ti3C2T obtained in step S2.1 xThe dispersion was subjected to ultrasonic exfoliation in an ice bath to obtain a few-layer Ti3C2T x Dispersion.

[0054] Preferably, the multilayer Ti3C2T x The thickness of the material is 100-200nm.

[0055] Preferably, the conditions for the ultrasonic stripping treatment are: introducing nitrogen or argon, ultrasonic power of 50-1000W, and ultrasonic time of 60-600min.

[0056] Preferably, in step S2.1, the centrifugal conditions are: rotation speed 1000-8000 rpm, time 5-20 min.

[0057] On the other hand, the present invention also provides a two-dimensional Ti3C2T based on the preparation method according to any one of the above x / MOS composite gas sensors, such as Figure 3 and Figure 4 As shown, the gas sensor comprises, from bottom to top, a planar electrode substrate 1, a Ti3C2T x Film 2 and MOS film 3, wherein the Ti3C2T x Together with the MOS film, it forms the gas-sensitive material layer.

[0058] The technical features of the present invention are described in detail below through examples and drawings. Unless otherwise specified, the instruments and materials described in the following examples can be obtained from commercial channels.

[0059] like Figure 2 As shown, the planar electrode substrate used in the embodiment of the present invention refers to a planar ceramic substrate with Au interdigital electrodes 11, with a size of 3×3 mm and a pair of interdigital electrodes. The Au interdigital electrodes 11 are fixed to the surface of the planar ceramic substrate 12, and the gas-sensitive material is coated on the surface of the Au interdigital electrodes 11. It should be noted that other embodiments may also use multiple pairs of ceramic interdigital electrodes or flexible PI / PET interdigital electrodes.

[0060] Example 1

[0061] A two-dimensional MXene (Ti3C2T x ) / SnO2 composite material gas sensor preparation method, comprising the following steps:

[0062] (1) 45 mg of multilayer Ti3C2T x The powder was added to 20 ml of dimethyl sulfoxide (DMSO) and stirred at room temperature for 18 h. The mixture was then centrifuged at 4000 rpm for 10 min to separate the solid and liquid to obtain a precipitate, which was the intercalated multilayer Ti3C2Tx The obtained precipitate was washed with deionized water, and the process was repeated at least twice; finally, the washed precipitate was dispersed in 30 ml of deionized water and ultrasonicated in an ice bath in flowing argon for 8 h at an ultrasonic power of 300 W to obtain a few-layer Ti3C2T x Dispersion liquid;

[0063] (2) Use a pipette to absorb the few-layer Ti3C2T prepared in step (1) x The dispersion is drop-coated on the planar electrode substrate, and then the substrate coated with a few layers of Ti3C2T x The flat electrode substrate of the dispersion was placed in a drying oven at 30°C to form Ti3C2T x film;

[0064] (3) The Ti3C2T x The flat electrode substrate of the film was pasted on a glass sheet and fixed on the base of the vacuum chamber of the JCP200 high vacuum magnetron sputtering coating machine. SnO2 was used as the target material. When the vacuum degree was drawn to 5×10 -4 Pa, high-purity argon gas was introduced, and SnO2 thin film was deposited under the conditions of sputtering power of 100 W, sputtering pressure of 2 Pa, sputtering time of 300 s, and sputtering temperature of room temperature to obtain Ti3C2T x / SnO2 double-layer gas-sensitive material film planar electrode substrate;

[0065] (4) The Ti3C2T x The planar electrode substrate of the / SnO2 composite material was welded on the hexagonal base to obtain a two-dimensional Ti3C2T x Room temperature gas sensor with SnO2 as sensitive material.

[0066] Example 2

[0067] A two-dimensional Ti3C2T x A method for preparing a gas sensor of a ZnO / ZnO composite material comprises the following steps:

[0068] (1) 45 mg of multilayer Ti3C2T x The powder was added to 20 ml of dimethyl sulfoxide (DMSO) and stirred at room temperature for 18 h. The mixture was then centrifuged at 4000 rpm for 10 min to separate the solid and liquid to obtain a precipitate, which was the intercalated multilayer Ti3C2T x The obtained precipitate was washed with deionized water, and the process was repeated at least twice; finally, the washed precipitate was dispersed in 30 ml of deionized water and ultrasonicated in an ice bath in flowing argon for 8 h at an ultrasonic power of 300 W to obtain a few-layer Ti3C2T x Dispersion liquid;

[0069] (2) Use a pipette to absorb the few-layer Ti3C2T prepared in step (1) x The dispersion is drop-coated on the planar electrode substrate, and then the substrate coated with a few layers of Ti3C2T x The flat electrode substrate of the dispersion was placed in a drying oven at 30°C to form Ti3C2T x film;

[0070] (3) The Ti3C2T x The flat electrode substrate of the film was pasted on a glass sheet and fixed on the base of the vacuum chamber of a JCP200 high vacuum magnetron sputtering coating machine. ZnO was used as the target material. When the vacuum degree was drawn to 5×10 -4 Pa, high-purity argon gas was introduced, and ZnO thin film was deposited under the conditions of sputtering power of 100 W, sputtering pressure of 2 Pa, sputtering time of 300 s, and sputtering temperature of room temperature to obtain Ti3C2T x / ZnO double-layer gas-sensitive material film planar electrode substrate;

[0071] (4) The Ti3C2T x The planar electrode substrate of the / ZnO composite material is welded on the hexagonal base to obtain a two-dimensional Ti3C2T x Room temperature gas sensor with ZnO as sensitive material.

[0072] Example 3

[0073] A two-dimensional Ti3C2T x A method for preparing a gas sensor of a / WO3 composite material comprises the following steps:

[0074] (1) 45 mg of multilayer Ti3C2T x The powder was added to 20 ml of dimethyl sulfoxide (DMSO) and stirred at room temperature for 18 h. The mixture was then centrifuged at 4000 rpm for 10 min to separate the solid and liquid to obtain a precipitate, which was the intercalated multilayer Ti3C2T x The obtained precipitate was washed with deionized water, and the process was repeated at least twice. Finally, the washed precipitate was dispersed in 30 ml of deionized water and ultrasonicated in an ice bath in flowing argon for 8 h at an ultrasonic power of 300 W to obtain a few-layer Ti3C2T x Dispersion liquid;

[0075] (2) Use a pipette to absorb the few-layer Ti3C2T prepared in step (1) x The dispersion is drop-coated on the planar electrode substrate, and then the substrate coated with a few layers of Ti3C2T xThe flat electrode substrate of the dispersion was placed in a drying oven at 30°C to form Ti3C2T x film;

[0076] (3) The Ti3C2T x The flat electrode substrate of the film was pasted on a glass sheet and fixed on the base of the vacuum chamber of the JCP200 high vacuum magnetron sputtering coating machine. WO3 was used as the target material. When the vacuum degree was drawn to 5×10 -4 Pa, high-purity argon gas was introduced, and WO3 thin film was deposited under the conditions of sputtering power of 100 W, sputtering pressure of 2 Pa, sputtering time of 300 s, and sputtering temperature of room temperature to obtain Ti3C2T x / WO3 double-layer gas-sensitive material film planar electrode substrate;

[0077] (4) The Ti3C2T x The planar electrode substrate of the / WO3 composite material is welded on the hexagonal base to obtain a two-dimensional Ti3C2T x Room temperature gas sensor with / WO3 as sensitive material.

[0078] Comparative Example

[0079] Two-dimensional Ti3C2T x Nanomaterials are used as gas-sensitive materials to make room temperature gas sensors. The specific steps are as follows:

[0080] Weigh 7.5 mg of multilayer Ti3C2T x The powder was added to 5 ml of deionized water and then placed in an ultrasonic machine for 5 min to disperse it evenly. The Ti3C2T x The dispersion is drop-coated on the flat electrode substrate, and then the Ti3C2T x The flat electrode substrate of the dispersion was placed in a drying oven at 30°C to form Ti3C2T x The film will be coated with Ti3C2T x The flat electrode substrate of the gas-sensitive material is welded on the hexagonal base to obtain a two-dimensional Ti3C2T x Room temperature gas sensor with nanomaterials as sensitive materials.

[0081] Sensor performance test

[0082] The gas sensors prepared in the above-mentioned Examples 1-3 and the comparative example were placed in a test chamber, and the target gas was introduced by static gas distribution at room temperature. The resistance change of the sensor in the air and in different concentrations of the target gas environment was detected by the CGS-8 intelligent gas sensitive analysis system. The resistance difference of the device in the air and in the target gas and the resistance ratio in the air (|Ra -R g | / R a ×100%) is the device's response value to the target gas at this concentration. The results are as follows:

[0083] like Figure 5 As shown, the two-dimensional Ti3C2T prepared in the comparative example of the present invention was tested at room temperature. x The response of the nanomaterial sensor to 5ppm-500ppm ammonia. As can be seen from the figure, the stability of the sensor is poor, and the device resistance is difficult to return to the initial state after the gas response. The sensitivity to 100ppm ammonia is only 4.6%.

[0084] like Figure 6 As shown, the two-dimensional Ti3C2T prepared in Example 1 of the present invention was tested at room temperature. x The response of the sensor of Ti3C2T / SnO2 composite material to 5ppm-500ppm ammonia. In the figure, the horizontal axis is the acquisition time and the vertical axis is the device sensitivity. x The response value of the SnO2-based sensor to 100ppm ammonia can reach 15.6%, which is the highest of pure Ti3C2T x The sensitivity of the composite material to ammonia is 3.3 times that of the base sensor (comparative example), indicating that the sensitivity of the composite material to ammonia is greatly improved.

[0085] Furthermore, the cyclic response performance of the sensor of Example 1 to 100 ppm ammonia was tested at room temperature. Figure 7 As shown in the figure, the horizontal axis is the acquisition time, and the vertical axis is the device resistance value. After five response-recovery cycles, the sensor resistance value remains basically unchanged, indicating that the sensor prepared in Example 1 has good cycle stability.

[0086] like Figure 8 As shown, the two-dimensional Ti3C2T prepared in Example 2 of the present invention was tested at room temperature. x The response of the sensor of Ti3C2T / ZnO composite material to 5ppm-500ppm ammonia. x The lowest ammonia concentration that the ZnO-based sensor can detect is 5ppm, and the corresponding response value is 2.0%. As the ammonia concentration increases, the sensor's response value to the gas also increases, and the response values ​​to 10, 30, 50, 100 and 500ppm ammonia are 3.9, 6.3, 7.1, 11.0 and 17.5% respectively.

[0087] Furthermore, the cyclic response performance of the sensor of Example 2 to 100 ppm ammonia was tested at room temperature. Fig. 9As shown in Figure 2, in the five response-recovery cycles, the resistance of the device can basically recover to the initial state, indicating that the Ti3C2T x / ZnO-based sensors have good cycling stability.

[0088] like Fig.10 As shown, the two-dimensional Ti3C2T prepared in Example 3 of the present invention was tested at room temperature. x The response of the sensor made of Ti3C2T / WO3 composite material to 5ppm-500ppm ammonia. As shown in the figure, the response value of the sensor made in Example 3 to 100ppm ammonia is 10.5%, which is higher than that of the pure Ti3C2T / WO3 composite material at the same concentration. x 2.3 times of the base sensor (comparative example). x Compared with Ti3C2T based sensors x The response value and recovery of WO3-based sensors to various ammonia concentrations are significantly improved.

[0089] Furthermore, the cyclic response performance of the sensor of Example 3 to 100 ppm ammonia was tested at room temperature. Fig.11 As shown, the Ti3C2T prepared in Example 3 x In the five test cycles, the device resistance of the Ti3C2T x / WO3 composite sensor has ideal repeatability and cycle stability.

[0090] Fig.12 The selectivity test diagram of the sensor prepared in Examples 1 to 3 of the present invention and the comparative example to 500ppm formaldehyde, acetone, ethanol, isopropanol and ammonia is shown. The results show that compared with the pure Ti3C2T x Compared with Ti3C2T based sensors x / MOS composite material sensor has higher sensitivity and selectivity for ammonia, and in the present invention, based on Ti3C2T x The gas sensor based on SnO2 composite material has the best gas sensing performance.

[0091] In summary, the present invention adopts a method of first drop coating and drying followed by magnetron sputtering to sequentially prepare Ti3C2T x The gas sensor of the composite gas-sensitive material with controllable thickness and strong binding force is finally obtained conveniently and quickly. The increase of active sites on the surface of the composite gas-sensitive material and the electron transfer of the heterojunction effectively improve the sensitivity, selectivity, cycle stability and recoverability of the sensor of the present invention. In addition, the preparation method of the present invention is simple and reliable, with high repeatability, and is suitable for large-scale production.

[0092] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A two-dimensional Ti 3 C 2 T x Preparation method of gas sensor of MOS composite material, It is characterized in that The following steps are involved: S1, providing a planar electrode substrate; S2, weigh multilayer Ti 3 C 2 T x The material was intercalated and ultrasonically dispersed to obtain a few-layer Ti 3 C 2 T x Dispersion liquid; S3, the few-layer Ti 3 C 2 T x The dispersed liquid is dropwise applied to the upper surface of the planar electrode substrate and dried to form a Ti 3 C 2 T x film; S4, providing a MOS target material, and depositing it on the Ti 3 C 2 T x A MOS film is deposited on the surface of the film to obtain a planar electrode substrate with a double-layer gas-sensitive material film; S5, the planar electrode substrate obtained in step S4 is subsequently assembled to complete the two-dimensional Ti 3 C 2 T x Preparation of gas sensors based on / MOS composite materials; Wherein, the MOS target material is selected from SnO 2 、ZnO、WO 3 Any of the following: The detection gas of the gas sensor is ammonia.

2. The preparation method according to claim 1, It is characterized in that In step S4, the magnetron sputtering conditions are: vacuum degree is 5×10 -4 Pa, the sputtering power is 100W, the sputtering pressure is 2Pa, and the sputtering time is 60-360s.

3. The preparation method according to claim 2, It is characterized in that The sputtering time was 300 s.

4. The preparation method according to claim 1, It is characterized in that The specific operations of step S2 are: S2.1, weigh the multilayer Ti 3 C 2 T x The material was added to DMSO for intercalation treatment. After centrifugation, precipitation and washing, the precipitate was dispersed in deionized water again to form a multilayer Ti 3 C 2 T x Dispersion liquid; S2.2, the multilayer Ti obtained in step S2.1 3 C 2 T x The dispersion was subjected to ultrasonic exfoliation in an ice bath to obtain a few-layer Ti 3 C 2 T x Dispersion.

5. The preparation method according to claim 1, It is characterized in that The multilayer Ti 3 C 2 T x The thickness of the material is 100-200nm.

6. The preparation method according to claim 4, It is characterized in that In step S2.2, the conditions for the ultrasonic stripping treatment are: introducing nitrogen or argon, ultrasonic power of 50-1000 W, and ultrasonic time of 60-600 min.

7. The preparation method according to claim 4, It is characterized in that In step S2.1, the centrifugal conditions are: rotation speed 1000-8000 rpm, time 5-20 min.

8. A two-dimensional Ti-based 3 C 2 T x / MOS composite gas sensor, It is characterized in that The gas sensor comprises, from bottom to top, a planar electrode substrate, a Ti 3 C 2 T x film and MOS film, wherein the Ti 3 C 2 T x Together with the MOS film, it forms the gas-sensitive material layer.