Method for producing stretched film
By using longitudinally oriented variable-pitch clamps in the manufacturing of circularly polarizing plates to manufacture diagonally stretched films, the problems of film relaxation and wrinkles are solved, and the flatness of the film and manufacturing efficiency are improved.
Patent Information
- Application Number
- CN202210304954.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-03-25
AI Technical Summary
In the existing technology, the diagonally stretched film is prone to relaxation or wrinkles during the production process, which affects the quality of the circular polarizing plate.
The longitudinally variable spacing left and right clamps are used to extend the long strip of film diagonally. By changing the spacing and movement of the clamps, the film is transported at an angle during the transportation process, thereby reducing the tension on the slack side and thereby improving the flatness of the film.
It effectively reduces the relaxation amount of the film, improves the flatness of the stretched film, reduces the possibility of wrinkles, and improves the manufacturing efficiency and quality of circularly polarizing plates.
Smart Images

Figure CN115122621B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a stretched film and a method for producing an optical layered body. Background Art
[0002] In image display devices such as liquid crystal display devices (LCDs) and organic electroluminescent display devices (OLEDs), circular polarizers are used to improve display characteristics or prevent reflection. Circular polarizers typically laminate polarizers and phase difference films (typically λ / 4 plates) in such a way that the absorption axis of the polarizer forms an angle of 45° with the slow axis of the phase difference film. Phase difference films have been typically made by uniaxial stretching or biaxial stretching in the longitudinal and / or transverse directions, so their slow axes are mostly presented in the transverse direction (width direction) or longitudinal direction (length direction) of the roll of the long film. As a result, when making a circular polarizer, it is necessary to cut the phase difference film at an angle of 45° to the width direction or the length direction and stick them together one by one.
[0003] In addition, in order to ensure the wide bandwidth of the circular polarizer, there is also a case where two phase difference films of a λ / 4 plate and a λ / 2 plate are stacked. In this case, it is necessary to stack the λ / 2 plate at an angle of 75° relative to the absorption axis of the polarizer, and to stack the λ / 4 plate at an angle of 15° relative to the absorption axis of the polarizer. In this case, when making a circular polarizer, it is necessary to cut the phase difference film at an angle of 15° and 75° relative to the width direction or the length direction, and stick them one by one.
[0004] Furthermore, in other embodiments, in order to prevent the light from the laptop from being reflected into the keyboard, etc., a λ / 2 plate is sometimes used on the visible side of the polarizer for the purpose of rotating the direction of the linear polarized light from the polarizer by 90°. In this case, it is necessary to cut the phase difference film at an angle of 45° with respect to the width direction or the length direction and laminate them one by one.
[0005] In order to solve this problem, a technique has been proposed in which the left and right ends of the long strip film in the width direction are held by using left and right clamps of variable spacing type with varying clamp spacing in the longitudinal direction, the clamp spacing of at least one of the left and right clamps is varied, and the slow axis of the phase difference film is presented in the oblique direction by stretching the film in the oblique direction relative to the longitudinal direction (hereinafter also referred to as "oblique stretching") (e.g. Patent Document 1). However, the obliquely stretched film obtained by this technique sometimes sags (droops) or wrinkles.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 4845619 Summary of the invention
[0009] Technical problem to be solved by the invention
[0010] The present invention has been made to solve the above-mentioned technical problems, and its main object is to reduce the slack generated in the obliquely stretched film.
[0011] Means for solving technical problems
[0012] According to one aspect of the present invention, there is provided a method for manufacturing a stretched film, comprising: gripping the left and right ends in the width direction of a continuously conveyed long strip of film using left and right clamps of a variable spacing type in which the clamp spacing in the longitudinal direction changes; moving the left and right clamps while changing the clamp spacing of at least one clamp to obliquely stretch the film; and releasing the film from the left and right clamps, wherein the conveying direction of the film before being gripped by the left and right clamps is obliquely inclined relative to the conveying direction of the film during the oblique stretching, and the line connecting the left and right clamps when gripping the film is obliquely inclined relative to the conveying direction of the film during the oblique stretching.
[0013] In one embodiment, the conveyance direction of the film before being gripped by the left and right clamps is inclined with respect to the conveyance direction of the film during the oblique stretching so that the unrelaxed end of the film becomes a concave side.
[0014] In one embodiment, the conveyance direction of the film before being gripped by the left and right clamps forms an angle of 10° to 40° with respect to the conveyance direction of the film during the oblique stretching.
[0015] In one embodiment, the oblique extension includes: (i) increasing the clamp spacing of one of the left and right clamps from P1 to P2, while reducing the clamp spacing of the other clamp from P1 to P3; and (ii) changing the clamp spacing of each clamp in such a manner that the reduced clamp spacing and the increased clamp spacing become a specified equal spacing.
[0016] In one embodiment, P2 / P1 is 1.25 to 1.75, and P3 / P1 is 0.50 or more and less than 1.
[0017] According to another aspect of the present invention, there is provided a method for producing an optical laminate, comprising: obtaining a long-length stretched film by the above-mentioned production method; and continuously bonding the long-length optical film and the long-length stretched film while conveying them in the same longitudinal direction.
[0018] In one embodiment, the optical film is a polarizing plate, and the stretched film is a λ / 4 plate or a λ / 2 plate.
[0019] Effects of the Invention
[0020] In the method for manufacturing a stretched film of the present invention, the conveying direction of the film before being gripped by the clamp is set in a manner that is oblique relative to the conveying direction of the film during oblique stretching. By conveying the film in an oblique direction relative to the conveying direction during oblique stretching, the travel path length (path length) of the left and right ends of the film from the time of being sent out from the roller to the time of being released from the clamp can be made different. As a result, tension is applied to the slack side of the film, and the film becomes flat as a whole, so that a long strip of stretched film with reduced slack can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic plan view for explaining the overall structure of an example of a stretching device that can be used in the method for producing a stretched film of the present invention.
[0022] Figure 2 For the purpose of explaining Figure 1 A schematic top view of the main parts of the linkage mechanism for changing the distance between the clamps in the extension device.
[0023] Figure 3 To illustrate the Figure 1 A schematic top view of the main parts of the linkage mechanism for changing the distance between the clamps in the extension device.
[0024] Figure 4 A schematic top view for explaining the holding process.
[0025] Figure 5A It is a schematic diagram showing the outline of the clamp spacing in one embodiment of the oblique extension.
[0026] Figure 5B It is a schematic diagram showing the outline of the clamp spacing in one embodiment of the oblique extension.
[0027] Figure 6 This is a schematic cross-sectional view of a circularly polarizing plate using a retardation film obtained by the production method of the present invention.
[0028] Figure 7 This is a schematic diagram for explaining the method of measuring the relaxation amount.
[0029] Explanation of symbols
[0030] 1. Stretch film
[0031] 10L Endless Ring
[0032] 10R Endless Ring
[0033] 20 Clamp
[0034] 50 Transport roller
[0035] 100 Extension device
[0036] 500 Circular Polarizer DETAILED DESCRIPTION
[0037] The preferred embodiments of the present invention are described below, but the present invention is not limited to these embodiments. In addition, in this specification, "the clamp spacing in the longitudinal direction" refers to the distance between the centers of adjacent clamps in the longitudinal direction in the travel direction. In addition, the left-right relationship in the width direction of the long film refers to the left-right relationship facing the conveying direction of the film unless otherwise specified.
[0038] A. Method for producing stretched film
[0039] The manufacturing method of the stretched film of the embodiment of the present invention includes the following steps: holding the left and right ends in the width direction of the continuously conveyed long strip film with left and right clamps of variable spacing type in which the clamp spacing in the longitudinal direction changes (holding step); moving the left and right clamps while changing the clamp spacing of at least one clamp to stretch the film obliquely (oblique stretching step); and releasing the film from the left and right clamps (releasing step).
[0040] In the manufacturing method of the embodiment of the present invention, the conveying direction of the film before being held by the left and right clamps is inclined obliquely relative to the conveying direction of the film during the oblique stretching, and the line connecting the left and right clamps when holding the film is inclined obliquely relative to the conveying direction of the film during the oblique stretching. Typically, the manufacturing method of the stretched film of the embodiment of the present invention further includes a preheating step. Specifically, the film held by the left and right clamps is preheated and then supplied to the oblique stretching.
[0041] The film holding, preheating, oblique stretching and release by the clamps can be performed, for example, using a tentering machine-type simultaneous biaxial stretching device having left and right clamps that hold the left and right ends of the long film in the width direction and can move at different speeds.
[0042] Figure 1The present invention is a schematic top view of the overall structure of an example of a stretching device that can be used in the manufacturing method of the present invention. The stretching device 100, in a top view, has an endless ring 10L and an endless ring 10R with a plurality of clamps 20 for holding the film symmetrically on the left and right sides. In addition, in this specification, when observed from the inlet side of the film, the endless ring on the left is referred to as the endless ring 10L on the left, and the endless ring on the right is referred to as the endless ring 10R on the right. The clamps 20 of the endless rings 10L and 10R on the left and right are respectively guided to the standard track 70 and move in a circular manner. The clamps 20 of the endless ring 10L on the left are moved in a counterclockwise direction, and the clamps 20 of the endless ring 10R on the right are moved in a clockwise direction. In the stretching device, from the inlet side to the outlet side of the sheet, the holding area A, the preheating area B, the stretching area C and the release area D are arranged in sequence. The conveying direction of the film does not change from the preheating area B to the release area D, and the film is conveyed in a straight line during this period. In addition, these respective areas refer to the areas where the film to be stretched is actually held, preheated, obliquely stretched and released, and do not refer to mechanically and structurally independent partitions. It should also be noted that Figure 1 The length ratio of each region in the extension device is different from the actual length ratio.
[0043] Figure 1 Although not shown in the figure, an area for performing any appropriate treatment may be provided between the stretching area C and the release area D as required. Such treatment may include a lateral shrinking treatment. In addition, although not shown in the figure, the stretching device typically includes a heating device (e.g., various ovens such as hot air type, near infrared type, and far infrared type) for making the preheating area B to the release area D a heating environment.
[0044] In the holding area A of the stretching device 100, the left endless ring 10L is longer than the right endless ring 10R, and the distance between the left and right endless rings 10L and 10R is maintained to correspond to the distance of the initial width of the film to be stretched. From the stretching area B to the release area D, the left and right endless rings 10L and 10R are symmetrically formed in a top view. Specifically, in the preheating area B, the left and right endless rings 10L and 10R are roughly parallel to each other with a distance corresponding to the initial width of the film to be stretched. The stretching area C is formed as the distance between the left and right endless rings 10L and 10R gradually expands to the width corresponding to the stretched width of the above-mentioned film from one side of the preheating area B toward the release area D. In the release area D, the left and right endless rings 10L and 10R are formed in a manner that they are roughly parallel to each other with a distance corresponding to the width of the above-mentioned film after stretching. However, the structure of the left and right endless rings 10L and 10R is not limited to the above-mentioned example. For example, the left and right endless loops 10L and 10R may be configured to be substantially parallel to each other at a spacing distance corresponding to the initial width of the film to be stretched from the preheating area B to the release area D. In addition, with respect to the holding area A, in the example shown in the figure, the left endless loop 10L is configured to be longer than the right endless loop 10R, but it is also possible to configure one of the left and right endless loops to be longer corresponding to the location where slack occurs.
[0045] The clamp (clamp on the left side) 20 of the endless ring 10L on the left side and the clamp (clamp on the right side) 20 of the endless ring 10R on the right side can be moved in a circular motion independently. For example, the driving sprockets 11 and 12 of the endless ring 10L on the left side are driven to rotate in the counterclockwise direction by the motors 13 and 14, and the driving sprockets 11 and 12 of the endless ring 10R on the right side are driven to rotate in the clockwise direction by the motors 13 and 14. As a result, the clamp holding member (not shown) of the driving roller (not shown) meshing with these driving sprockets 11 and 12 is given a walking force. As a result, the endless ring 10L on the left side is moved in a circular motion in the counterclockwise direction, and the endless ring 10R on the right side is moved in a circular motion in the clockwise direction. By driving the left motor and the right motor independently, the endless ring 10L on the left side and the endless ring 10R on the right side can be moved in a circular motion independently.
[0046] Furthermore, the clamp 20 of the left endless ring 10L (the clamp on the left) and the clamp 20 of the right endless ring 10R (the clamp on the right) are of variable pitch type. That is, the left and right clamps 20, 20 are independent of each other, and the clamp pitch in the longitudinal direction can be changed as they move. The variable pitch type structure can be realized by adopting a driving method such as a pantograph method, a linear motor method, a motor chain method, etc. The following is an example of a link mechanism (pantograph mechanism).
[0047] Figure 2 and Figure 3 For illustration Figure 1 A schematic top view of the main part of the link mechanism for changing the distance between the clamps in the extension device. Figure 2 Indicates that the distance between the fixtures is the smallest. Figure 3 Indicates the state where the distance between the fixtures is at the maximum.
[0048] like Figure 2 and Figure 3 As shown in the figure, a slender rectangular clamp holding member 30 is provided in the horizontal direction of each holding clamp 20 when viewed from above. Although not shown in the figure, the clamp holding member 30 is closed by an upper beam, a lower beam, a front wall (the wall on the clamp side) and a rear wall (the wall on the opposite side of the clamp), forming a frame structure with a strong cross section. The clamp holding member 30 is arranged in such a way that it rotates on the running surfaces 81 and 82 using the running wheels 38 at both ends. In addition, Figure 2 and Figure 3 In the figure, the running wheels on the front wall side (the running wheels on the rotating running surface 81) are not shown. The running surfaces 81 and 82 are parallel to the standard track 70 in the entire area. On the rear side of the upper beam and the lower beam of the clamp holding member 30 (the opposite side of the clamp side (hereinafter referred to as the anti-clamp side)), a long hole 31 is formed along the length direction of the clamp holding member, and the slider 32 can be slidably engaged in the length direction of the long hole 31. Near the end of the clamp 20 side of the clamp holding member 30, a first shaft member 33 is vertically provided through the upper beam and the lower beam. On the other hand, a second shaft member 34 is vertically provided on the slider 32 of the clamp holding member 30. One end of the main connecting rod member 35 is pivotally connected to the first shaft member 33 of each clamp holding member 30. The main connecting rod member 35 is pivotally connected to the second shaft member 34 of the clamp holding member 30 at the other adjacent end. In addition to the main link member 35, one end of a secondary link member 36 is also pivotally connected to the first shaft member 33 of each clamp holding member 30. The other end of the secondary link member 36 is pivotally connected to the middle part of the main link member 35 through a pivot 37. The link mechanism obtained by the main link member 35 and the secondary link member 36 is as follows: Figure 2 As shown in FIG. 1 , the slider 32 moves toward the rear side (anti-clamp side) of the clamp holding member 30, and the longitudinal distance between the clamp holding members 30 (resulting in the clamp distance) becomes smaller, as shown in FIG. Figure 3 As shown in FIG. 1 , the more the slider 32 moves toward the front side (the clamp side) of the clamp holding member 30, the larger the longitudinal distance between the clamp holding members 30 (resulting in the clamp distance). The slider 32 is positioned by the distance setting rail 90. Figure 2 and Figure 3 As shown, the smaller the spacing distance between the standard rail 70 and the spacing setting rail 90 is, the larger the clamp spacing becomes.
[0049] By using the stretching device to stretch the film obliquely, an oblique stretched film, for example, a phase difference film having a slow axis in an oblique direction can be produced. In addition, a specific embodiment of the stretching device is described in, for example, Japanese Patent Application Publication No. 2008-44339, which is incorporated herein by reference in its entirety. Each step is described in detail below.
[0050] A-1. Holding process
[0051] The film can be held at the film receiving entrance of the stretching device. Figure 4 The holding process is specifically described. The film 1 before being held by the left and right clamps 20 is transported obliquely relative to the conveying direction X of the film 1 during oblique stretching (in other words, the conveying direction of the film 1 in the stretching device 100). Specifically, the conveying direction Y of the film 1 before being held is inclined at an angle θ relative to the conveying direction X of the film 1 during oblique stretching. The film 1 thus conveyed from the oblique direction is typically held at its left and right ends by the left and right clamps 20 at the same time and at a certain clamp spacing equal to each other in the holding area A of the stretching device 100. As described above, the stretching device 100 is constructed in such a way that one endless loop in the holding area (the left endless loop 10L in the example shown) is longer than the other endless loop (the right endless loop 10R in the example shown). By means of this stretching device 100, the film 1 can be gripped in such a manner that the line Z connecting the left and right clamps 20 (more specifically, the line connecting the centers of the conveying direction of the left and right clamps 20) becomes inclined relative to the conveying direction X of the film 1 during oblique stretching, and the subsequent conveying direction is changed to direction X. As a result, the conveying path length of the film 1 from the time of being gripped by the clamp 20 to the time of being released can be made to have different distances at the left and right ends. In one embodiment, the line Z connecting the centers of the left and right clamps 20 when gripping can be approximately orthogonal to the conveying direction Y of the film 1 before gripping. In addition, in this specification, approximately orthogonal includes a range of 87.0° to 93.0°, for example, includes a range of 89.0° to 91.0°, preferably includes a range of 89.7° to 90.3°, more preferably includes a range of 89.9° to 90.1°, and further preferably includes 90.0°.
[0052] The film 1 before being gripped by the left and right clamps is preferably conveyed obliquely relative to the conveying direction X in such a manner that the unrelaxed side end (the right end in the example in the figure) becomes the concave side (inside) after the oblique stretching. By bending the conveying direction of the film in such a manner that the unrelaxed side end becomes the concave side, the walking path length (path length) of the film from the time it is sent out from the roller to the time it is released from the clamp is longer at the relaxed side end (the left end in the example in the figure) than at the unrelaxed side end. Thus, tension is added to the relaxed side end and the film is flattened as a whole, resulting in appropriate reduction in relaxation. In addition, in the stretched film obtained by oblique stretching, the stretching processes (timing, number of times, sequence, thermal process, etc. of stretching or contraction) of the left and right ends of the film are different from each other during the oblique stretching, resulting in that the deformation at the two ends caused by the residual stress after the clamp is released becomes uneven, and thus relaxation can occur at either end. In one embodiment, in an obliquely stretched film in which the left and right ends are stretched at different stretching ratios, the side with a lower stretching ratio during the oblique stretching is the relaxed side, and the film before being grasped is conveyed at an angle relative to the conveying direction X in such a manner that the end on the side with a higher stretching ratio (unrelaxed side) becomes a concave side.
[0053] Angle θ can be any appropriate value as long as the effect of the present invention is obtained. Angle θ is, for example, 5° to 50°, preferably 7° to 45°, and more preferably 10° to 40°. When angle θ is within this range, the relaxation reduction effect can be preferably obtained while maintaining the target in-plane phase difference and axis angle. In addition, angle θ can be adjusted to a desired value by changing the shape of the left and right endless rings 10L and 10R, applying various technologies for changing the conveying direction of the sheet to change the conveying direction Y, etc. The technology for changing the conveying direction of the sheet is recorded in, for example, Japanese Patent Publication No. 2000-351506, Japanese Patent Publication No. 2009-046285, etc.
[0054] In the holding area, the clamp spacing can be adjusted in a manner that slack or wrinkles do not occur at the end of the concave side due to changes in the conveying direction of the film. In one embodiment, the occurrence of slack or wrinkles is prevented by slightly increasing the clamp spacing of the clamp holding the concave side end. At this time, the clamp spacing of the clamp holding the convex side end is also preferably adjusted. By adjusting the clamp spacing of the two clamps, slack or wrinkles can be prevented from occurring at the end of the concave side, while a pair of left and right clamps are moved to the preheating area with the same clamp spacing and at the same time. In addition, a pair of left and right clamps that are transferred to the preheating area at the same time can be a combination that is different from a pair of left and right clamps that hold the film at the same time.
[0055] The film 1 gripped by the left and right clamps 20 is sent to the preheating area B by the movement of the left and right clamps 20 (substantially, the movement of the clamp holding members introduced into the standard rail 70 ).
[0056] A-2. Preheating process
[0057] In the preheating area B, the left and right endless rings 10L and 10R are configured as described above to be approximately parallel to each other at a distance corresponding to the initial width of the film to be stretched, so that the film is heated without basically stretching it horizontally or vertically. However, since the preheating may cause the film to warp, in order to avoid contact with the nozzle in the oven, etc., the distance between the left and right clamps (the distance in the width direction) may be slightly widened.
[0058] In the preheating step, the film is heated to a temperature T1 (°C). The temperature T1 is preferably above the glass transition temperature (Tg) of the film, more preferably above Tg+2°C, and further preferably above Tg+5°C. On the other hand, the heating temperature T1 is preferably below Tg+40°C, and more preferably below Tg+30°C. The temperature T1 varies depending on the film used, and is, for example, 70°C to 190°C, and preferably 80°C to 180°C.
[0059] The heating time to reach the temperature T1 and the holding time at the temperature T1 can be appropriately set according to the constituent material of the film or the manufacturing conditions (e.g., the conveying speed of the film). The heating time and the holding time can be controlled by adjusting the moving speed of the clamp 20, the length of the preheating zone, the temperature of the preheating zone, etc.
[0060] A-3. Oblique stretching process
[0061] In the stretching area C, the film is stretched obliquely by changing the clamp spacing in the longitudinal direction of at least one of them and moving the left and right clamps 20. More specifically, the film is stretched obliquely by increasing or decreasing the clamp spacing at different positions while moving the left and right clamps, changing (increasing and / or decreasing) the clamp spacing at different speeds while moving the left and right clamps, etc. The result of moving the left and right clamps while changing the clamp spacing in this way is that, in a pair of left and right clamps that move to the stretching area at the same time, one clamp reaches the terminal of the stretching area before the other clamp. Through this oblique stretching, the side end of the leading clamp is stretched at a higher stretching ratio than the side end of the trailing clamp, and as a result, a slow axis can be presented in the desired direction of the long film (for example, a direction of 45° relative to the length direction).
[0062] The oblique extension may also include lateral extension. In this case, the oblique extension may be performed while increasing the distance between the left and right clamps (the distance in the width direction), as shown in the example in the figure. Alternatively, unlike the example in the figure, the oblique extension may not include lateral extension and may be performed while maintaining the distance between the left and right clamps.
[0063] When the oblique stretching includes the transverse stretching, the stretching ratio in the transverse direction (TD) (the width W of the film after the oblique stretching) final The initial width W of the film initial The ratio (W final / W initial )) is preferably 1.05 to 6.00, more preferably 1.10 to 5.00.
[0064] In one embodiment, the oblique extension can be performed by increasing or decreasing the clamp spacing of each clamp to a predetermined spacing while making the position where the clamp spacing of one of the left and right clamps starts to increase or decrease different from the position where the clamp spacing of the other clamp starts to increase or decrease in the longitudinal direction. For the oblique extension of this embodiment, for example, the description of Patent Document 1, Japanese Patent Application Publication No. 2014-238524, etc. can be referred to.
[0065] In other embodiments, the oblique extension can be performed by increasing or decreasing the clamp spacing of the other clamp to a predetermined spacing while fixing the clamp spacing of one of the left and right clamps, and then returning to the initial clamp spacing. For the oblique extension of this embodiment, for example, reference can be made to the records of Japanese Patent Publication No. 2013-54338, Japanese Patent Publication No. 2014-194482, etc.
[0066] In other embodiments, the oblique extension can be performed by: (i) increasing the clamp spacing of one of the left and right clamps from P1 to P2, while reducing the clamp spacing of the other clamp from P1 to P3; and (ii) changing the clamp spacing of each clamp in such a way that the reduced clamp spacing and the increased clamp spacing become a predetermined equal spacing. For the oblique extension of this embodiment, for example, reference can be made to the records of Japanese Patent Publication No. 2014-194484. The oblique extension of this embodiment may also include: extending the distance between the left and right clamps while increasing the clamp spacing of one clamp from P1 to P2 and reducing the clamp spacing of the other clamp from P1 to P3, thereby extending the film obliquely (first oblique extension); and extending the distance between the left and right clamps while maintaining the clamp spacing of one clamp at P2 or reducing it to P4 in a manner that the clamp spacings of the left and right clamps become equal, and increasing the clamp spacing of the other clamp to P2 or P4, thereby extending the film obliquely (second oblique extension).
[0067] In the first oblique stretching, by stretching one end of the film in the longitudinal direction and shrinking the other end in the longitudinal direction while performing oblique stretching, a slow axis can be presented in a desired direction (for example, a direction at 45° relative to the longitudinal direction) with high uniaxiality and in-plane orientation. In addition, in the second oblique stretching, by narrowing the difference in the gap between the left and right clamps while performing oblique stretching, it is possible to fully stretch in the oblique direction while relieving excess stress.
[0068] In the oblique stretching of the above three embodiments, since the film can be released from the clamps while the moving speeds of the left and right clamps become equal, it is difficult for unevenness in the film conveying speed to occur when the left and right clamps are released, and the subsequent film winding can also be carried out appropriately.
[0069] Figure 5A and Figure 5B 1 and 2 are schematic diagrams showing an example of the outline of the clamp spacing in the oblique extension including the first oblique extension and the second oblique extension. The first oblique extension will be described in detail below with reference to these diagrams. Figure 5A and Figure 5B In the figure, the horizontal axis corresponds to the travel distance of the clamp. At the beginning of the first oblique extension, the left and right clamp spacings are both P1. P1 is representative of the clamp spacing in the preheating process. At the beginning of the first oblique extension, the clamp spacing of one clamp (hereinafter sometimes referred to as the first clamp) begins to increase and the clamp spacing of another clamp (hereinafter sometimes referred to as the second clamp) begins to decrease. In the first oblique extension, the clamp spacing of the first clamp is increased to P2, and the clamp spacing of the second clamp is reduced to P3. Therefore, at the end of the first oblique extension (when the second oblique extension begins), the second clamp moves with a clamp spacing of P3, and the first clamp moves with a clamp spacing of P2. In addition, the ratio of the clamp spacings can roughly correspond to the ratio of the moving speeds of the clamps.
[0070] Figure 5A and Figure 5BIn the embodiment, the timing of starting to increase the clamp spacing of the first clamp and the timing of starting to reduce the clamp spacing of the second clamp are both at the beginning of the first oblique extension. Unlike the illustrated example, the clamp spacing of the second clamp can be reduced after the clamp spacing of the first clamp is increased, and the clamp spacing of the first clamp can be increased after the clamp spacing of the second clamp is reduced. In a preferred embodiment, the clamp spacing of the second clamp can be reduced after the clamp spacing of the first clamp is increased. According to this embodiment, since the film has been extended to a certain extent (preferably about 1.2 times to 2.0 times) in the width direction, wrinkles are difficult to occur even if the clamp spacing of the second clamp is greatly reduced. Therefore, a more acute oblique extension can be performed, and a phase difference film with high uniaxiality and in-plane orientation can be preferably obtained.
[0071] Likewise, in Figure 5A and Figure 5B In the figure, the increase in the clamp spacing of the first clamp and the decrease in the clamp spacing of the second clamp continue until the end of the first oblique extension (the beginning of the second oblique extension), but unlike the example shown in the figure, either the increase or the decrease in the clamp spacing may end earlier than the other, and the clamp spacing may remain the same until the other ends (until the end of the first oblique extension).
[0072] The rate of change of the clamp spacing of the first clamp (P2 / P1) is preferably 1.25 to 1.75, more preferably 1.30 to 1.70, and further preferably 1.35 to 1.65. In addition, the rate of change of the clamp spacing of the second clamp (P3 / P1) is, for example, greater than 0.50 and less than 1, preferably 0.50 to 0.95, more preferably 0.55 to 0.90, and further preferably 0.55 to 0.85. When the rate of change of the clamp spacing is within this range, a slow axis can be presented with high uniaxiality and in-plane orientation in a direction of approximately 45 degrees relative to the length direction of the film.
[0073] As described above, the distance between the fixtures can be adjusted by adjusting the spacing between the extension device, setting the distance between the track and the standard track, and positioning the slider.
[0074] The stretch ratio in the width direction of the film in the first oblique stretching (film width at the end of the first oblique stretching / film width before the first oblique stretching) is preferably 1.1 times to 3.0 times, more preferably 1.2 times to 2.5 times, and further preferably 1.25 times to 2.0 times. When the stretch ratio is less than 1.1 times, tinplate-like wrinkles sometimes occur at the end of the contracted side. In addition, when the stretch ratio exceeds 3.0 times, the biaxiality of the obtained phase difference film becomes high, and when it is applied to a circular polarizer, the viewing angle characteristics are sometimes reduced.
[0075] In one embodiment, the first diagonal extension is carried out in such a manner that the product of the rate of change of the clamping pitch of the first clamp and the rate of change of the clamping pitch of the second clamp preferably reaches 0.7 to 1.5, more preferably 0.8 to 1.45, and still more preferably 0.85 to 1.40. When the product of the rates of change is within this range, a retardation film with high uniaxiality and in-plane orientation can be obtained.
[0076] Next, while referring to Figure 5A while specifically describing an embodiment of the second diagonal extension. In the second diagonal extension of this embodiment, the clamping pitch of the second clamp is increased from P3 to P2. On the other hand, the clamping pitch of the first clamp is maintained at P2 during the second diagonal extension. Therefore, at the end of the second diagonal extension, both the left and right clamps move with a clamping pitch of P2.
[0077] Figure 5A The rate of change (P2 / P3) of the clamping pitch of the second clamp in the second diagonal extension of the illustrated embodiment is not limited as long as the effects of the present invention are not impaired. This rate of change (P2 / P3) is, for example, 1.3 to 4.0, preferably 1.5 to 3.0.
[0078] while referring to Figure 5B while specifically describing another embodiment of the second diagonal extension. In the second diagonal extension of this embodiment, while reducing the clamping pitch of the first clamp, the clamping pitch of the second clamp is increased. Specifically, the clamping pitch of the first clamp is reduced from P2 to P4, and the clamping pitch of the second clamp is increased from P3 to P4. Therefore, at the end of the second diagonal extension, both the left and right clamps move with a clamping pitch of P4. In addition, in the illustrated example, the reduction of the clamping pitch of the first clamp and the increase of the clamping pitch of the second clamp are started simultaneously at the start of the second diagonal extension, but these can be started at different timings. Similarly, the reduction of the clamping pitch of the first clamp and the increase of the clamping pitch of the second clamp can also end at different timings.
[0079] Figure 5B The rate of change (P4 / P2) of the clamping pitch of the first clamp and the rate of change (P4 / P3) of the clamping pitch of the second clamp in the second diagonal extension of the illustrated embodiment are not limited as long as the effects of the present invention are not impaired. The rate of change (P4 / P2) is, for example, 0.4 or more and less than 1.0, preferably 0.6 to 0.95. In addition, the rate of change (P4 / P3) is, for example, more than 1.0 and 2.0 or less, preferably 1.2 to 1.8. It is preferred that P4 is equal to or greater than P1. When P4 < P1, problems such as wrinkles occurring at the ends and an increase in biaxiality may sometimes occur.
[0080] The magnification of the film in the width direction during the second diagonal extension (film width at the end of the second diagonal extension / film width at the end of the first diagonal extension) is preferably 1.1 to 3.0 times, more preferably 1.2 to 2.5 times, and further preferably 1.25 to 2.0 times. When the magnification is less than 1.1 times, wrinkles like those of galvanized iron sheets may occur at the end on the shrinking side. In addition, when the magnification exceeds 3.0 times, the biaxiality of the obtained retardation film becomes high, and when it is applied to a circular polarizing plate or the like, there may be a case where the viewing angle characteristics deteriorate. In addition, from the same viewpoint as above, the magnification of the film in the width direction during the first diagonal extension and the second diagonal extension (film width at the end of the second diagonal extension / film width before the first diagonal extension) is preferably 1.2 to 4.0 times, more preferably 1.4 to 3.0 times.
[0081] The diagonal extension can typically be carried out at a temperature T2. The temperature T2 is preferably Tg - 20°C to Tg + 30°C, more preferably Tg - 10°C to Tg + 20°C, and particularly preferably around Tg, relative to the glass transition temperature (Tg) of the film. Although it varies depending on the film used, the temperature T2 is, for example, 70°C to 180°C, preferably 80°C to 170°C. The difference between the above temperature T1 and temperature T2 (T1 - T2) is preferably ±2°C or more, more preferably ±5°C or more. In one embodiment, since T1 > T2, the film heated to temperature T1 in the preheating region can be cooled to temperature T2.
[0082] As described above, a lateral shrinkage treatment can also be carried out after the diagonal extension. For this treatment after the diagonal extension, paragraphs 0029 to 0032 of Japanese Patent Application Laid-Open No. 2014-194483 can be referred to.
[0083] A-4. Release process
[0084] At any position in the release region D, the above-mentioned film is released from the jig. In the release region D, generally neither lateral extension nor longitudinal extension is carried out. The film is heat-treated as needed to fix the extended state (thermal fixation), and / or cooled below Tg, and then the film is released from the jig. In addition, when performing thermal fixation, the jig pitch in the longitudinal direction can also be reduced to relieve stress.
[0085] The heat treatment can typically be carried out at a temperature T3. The temperature T3 varies depending on the film to be extended. There may be a case where T2 ≥ T3, or a case where T2 < T3. Generally, when the film is an amorphous material, there is a case where crystallization treatment is carried out at T2 ≥ T3; when it is a crystalline material, there is a case where crystallization treatment is carried out at T2 < T3. When T2 ≥ T3, the difference between temperature T2 and T3 (T2 - T3) is preferably 0°C to 50°C. The heat treatment time is typically 10 seconds to 10 minutes.
[0086] The stretched film released from the clamp is sent out from the outlet of the stretching device. The film sent out from the stretching device can be conveyed by rollers and wound up by a winding device to form a film roll. Alternatively, the film sent out from the stretching device can be conveyed with other long strips of optical films without being wound up, while being continuously bonded in a uniform length direction to form an optical laminate.
[0087] In one embodiment, slack is detected for the film fed from the stretching device. Based on the detected slack amount and the location where the slack occurs, the angle θ between the conveying direction Y of the film before gripping and the conveying direction X of the film during oblique stretching can be adjusted.
[0088] A-5. Detection of relaxation
[0089] The slack amount can be detected, for example, between the conveying rollers. Specifically, the slack amount can be detected as a difference in position (conveying height) in the width direction of the film at the midpoint between the conveying rollers.
[0090] The distance between the conveying rollers during the above detection is not particularly limited, and may be, for example, 500 mm to 2000 mm, and preferably 700 mm to 1500 mm.
[0091] The film tension during the above detection is not particularly limited, and may be, for example, 50 N / m to 400 N / m, preferably 100 N / m to 200 N / m. When the transport tension is too high, the film during transport may undergo elastic deformation, and relaxation may become difficult to detect. When the transport tension is too low, the tension itself may be unstable, and the measured value of relaxation may become unstable.
[0092] The above detection can be performed in a non-heating environment. The ambient temperature when detecting the relaxation amount is, for example, about 15°C to 40°C, and can also be, for example, about 20°C to 30°C.
[0093] In one embodiment, the slack amount is detected after the left and right ends in the width direction of the stretched film released from the clamp are cut off and removed. By detecting the slack amount in a state where both ends are removed, a more accurate detection result can be obtained.
[0094] The width of the end portions to be cut and removed is independent of each other, and may be, for example, 20 mm to 600 mm, and preferably 100 mm to 500 mm. The end portions may be cut and removed by ordinary slit processing.
[0095] The amount of relaxation reduction obtained by the method for manufacturing a stretched film according to an embodiment of the present invention (the amount of relaxation of a stretched film obtained by the method for manufacturing a stretched film in which the conveying direction Y of the film before gripping is parallel to the conveying direction X of the film during oblique stretching - the amount of relaxation of a stretched film obtained by the method for manufacturing a stretched film according to an embodiment of the present invention: wherein the relaxation amount measured with the distance between the rollers being 1000 mm) can be, for example, 3 mm or more, preferably 5 mm or more, more preferably 8 mm or more, and further preferably 10 mm or more. In addition, the amount of relaxation that can remain in the stretched film obtained by the method for manufacturing a stretched film according to an embodiment of the present invention can be, for example, less than 15 mm, preferably less than 10 mm, more preferably less than 8 mm, further preferably less than 5 mm, and further more preferably less than 3 mm.
[0096] B. Extending the membrane of an object
[0097] In the manufacturing method of the present invention, any appropriate film can be used. For example, a resin film that can be used as a phase difference film can be cited. As the material constituting this film, for example, polycarbonate resins, polyvinyl acetal resins, cycloolefin resins, acrylic resins, cellulose ester resins, cellulose resins, polyester resins, polyester carbonate resins, olefin resins, polyurethane resins, etc. can be cited. Preferred are polycarbonate resins, cellulose ester resins, polyester resins, polyester carbonate resins, and cycloolefin resins. The reason is that if these resins are used, a so-called wavelength-dependent phase difference film showing reverse dispersion can be obtained. These resins can be used alone or in combination with the desired properties.
[0098] As the polycarbonate resin, any appropriate polycarbonate resin may be used, and for example, a polycarbonate resin including a structural unit derived from a dihydroxy compound is preferred. Specific examples of the dihydroxy compound include 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-ethylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-propylphenyl)fluorene, 9,9-bis(4-hydroxy-3-isopropylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-sec-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-tert-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-cyclohexylphenyl)fluorene, 9,9-bis(4-hydroxy-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropyloxy)phenyl)fluorene, etc. In addition to the structural units derived from the above-mentioned dihydroxy compounds, the polycarbonate resin may also contain structural units derived from dihydroxy compounds such as isosorbide, isomannide, isoidide, spiroethylene glycol, dioxane glycol, diethylene glycol (DEG), triethylene glycol (TEG), polyethylene glycol (PEG), cyclohexanedimethanol (CHDM), tricyclodecanedimethanol (TCDDM), and bisphenols.
[0099] The details of the polycarbonate resin are described in, for example, Japanese Patent Application Laid-Open No. 2012-67300 and Japanese Patent No. 3325560. The descriptions of these patent documents are incorporated herein by reference.
[0100] The glass transition temperature of the polycarbonate resin is preferably 110°C to 250°C, more preferably 120°C to 230°C. When the glass transition temperature is too low, the heat resistance tends to deteriorate, and dimensional changes may occur after film molding. When the glass transition temperature is too high, the molding stability during film molding may deteriorate, and the transparency of the film may be impaired. In addition, the glass transition temperature is obtained according to JIS K 7121 (1987).
[0101] As the above-mentioned polyvinyl acetal resin, any appropriate polyvinyl acetal resin can be used. Representatively, the polyvinyl acetal resin can be obtained by condensing at least two aldehyde compounds and / or ketone compounds with a polyvinyl alcohol resin. Specific examples of polyvinyl acetal resins and detailed production methods are described in, for example, Japanese Patent Publication No. 2007-161994. This description is cited in this specification as a reference.
[0102] The stretched film (phase difference film) obtained by stretching the film of the above-mentioned stretching object preferably shows a refractive index characteristic of nx>ny. In one embodiment, the phase difference film can preferably function as a λ / 4 plate. In the present embodiment, the in-plane phase difference Re(550) of the phase difference film (λ / 4 plate) is preferably 100nm~180nm, more preferably 135nm~155nm. In other embodiments, the phase difference film can preferably function as a λ / 2 plate. In the present embodiment, the in-plane phase difference Re(550) of the phase difference film (λ / 2 plate) is preferably 230nm~310nm, more preferably 250nm~290nm. In addition, in this specification, nx is the refractive index in the direction where the in-plane refractive index reaches the maximum (ie, the slow axis direction), ny is the refractive index in the direction orthogonal to the slow axis (ie, the fast axis direction), and nz is the refractive index in the thickness direction. In addition, Re(λ) is the in-plane phase difference of the film measured at 23°C with light of a wavelength of λnm. Therefore, Re(550) is the in-plane retardation of the film measured with light of a wavelength of 550 nm at 23° C. Re(λ) is a value obtained by the formula: Re(λ)=(nx-ny)×d when the thickness of the film is d (nm).
[0103] The in-plane phase difference Re (550) of the phase difference film can be set to a desired range by appropriately setting the oblique stretching conditions. For example, the method of manufacturing a phase difference film having an in-plane phase difference Re (550) of 100 nm to 180 nm by oblique stretching is disclosed in detail in Japanese Patent Publication No. 2013-54338, Japanese Patent Publication No. 2014-194482, Japanese Patent Publication No. 2014-238524, Japanese Patent Publication No. 2014-194484, etc. Therefore, those skilled in the art can set appropriate oblique stretching conditions according to the disclosure.
[0104] When a circular polarizing plate is prepared using a single retardation film, or when the direction of linear polarized light is rotated 90° using a single retardation film, the slow axis direction of the retardation film used is preferably 30° to 60° or 120° to 150° relative to the length direction of the film, more preferably 38° to 52° or 128° to 142°, further preferably 43° to 47° or 133° to 137°, and particularly preferably about 45° or 135°.
[0105] In addition, when producing a circular polarizer using two retardation films (specifically, a λ / 2 plate and a λ / 4 plate), the slow axis direction of the retardation film (λ / 2 plate) used is preferably 60° to 90°, more preferably 65° to 85°, and particularly preferably about 75° with respect to the length direction of the film. In addition, the slow axis direction of the retardation film (λ / 4 plate) is preferably 0° to 30°, more preferably 5° to 25°, and particularly preferably about 15° with respect to the length direction of the film.
[0106] The retardation film preferably exhibits a so-called inverse dispersion wavelength dependence. Specifically, the in-plane retardation satisfies the relationship Re(450) < Re(550) < Re(650). Re(450) / Re(550) is preferably 0.8 or more and less than 1.0, more preferably 0.8 to 0.95. Re(550) / Re(650) is preferably 0.8 or more and less than 1.0, more preferably 0.8 to 0.97.
[0107] The absolute value of the photoelastic modulus of the retardation film is preferably 2×10 -12 (m 2 / N) to 100×10 -12 (m 2 / N), more preferably 5×10 -12 (m 2 / N) to 50×10 -12 (m 2 / N).
[0108] C. Optical laminate and manufacturing method of the optical laminate
[0109] The stretched film obtained by the manufacturing method of the present invention can be laminated with other optical films and used as an optical laminate. For example, the retardation film obtained by the manufacturing method of the present invention can be laminated with a polarizer and preferably used as a circular polarizer.
[0110] Figure 6 is a schematic cross-sectional view of an example of such a circular polarizer. The illustrated circular polarizer 500 has a polarizer 510, a first protective film 520 disposed on one side of the polarizer 510, a second protective film 530 disposed on the other side of the polarizer 510, and a retardation film 540 disposed outside the second protective film 530. The retardation film 540 is a stretched film (e.g., a λ / 4 plate) obtained by the manufacturing method described in item A. The second protective film 530 can also be omitted. In this case, the retardation film 540 can function as a protective film for the polarizer. The angle formed by the absorption axis of the polarizer 510 and the slow axis of the retardation film 540 is preferably 30° to 60°, more preferably 38° to 52°, further preferably 43° to 47°, and particularly preferably about 45°.
[0111] The phase difference film obtained by the manufacturing method of the present invention is long and has a slow axis in an oblique direction (for example, a direction of 45° relative to the length direction). In addition, in most cases, the long polarizer has an absorption axis in the length direction or the width direction. Therefore, if the phase difference film obtained by the manufacturing method of the present invention is used, the circular polarizer can be made with extremely excellent manufacturing efficiency using the so-called roll-to-roll method. In addition, roll-to-roll refers to a method in which long strips of film are rolled and transported to each other while their length directions are uniformly and continuously bonded.
[0112] In one embodiment, the method for producing an optical layered body of the present invention comprises: obtaining a long stretched film by the method for producing a stretched film described in Section A; and continuously laminating the long optical film and the long stretched film together in a uniform longitudinal direction while conveying the long optical film and the long stretched film.
[0113] [Example]
[0114] The present invention will be specifically described below by way of examples, but the present invention is not limited to these examples. In addition, the measurement and evaluation methods of the examples are as follows.
[0115] (1) Thickness
[0116] The measurement was performed using a micrometer (manufactured by PEACOCK, product name: "DG-205 type pds-2").
[0117] (2) Phase difference
[0118] The in-plane retardation Re (550) was measured using Axoscan manufactured by Axometrics.
[0119] (3) Orientation angle (direction of the slow axis)
[0120] The central portion of the film to be measured was cut into a square shape of 50 mm in width and 50 mm in length so that one side was parallel to the width direction of the film to prepare a sample. The sample was measured using Axoscan manufactured by Axometrics to measure the orientation angle θ at a wavelength of 590 nm.
[0121] (4) Glass transition temperature (Tg)
[0122] Measured according to JIS K7121.
[0123] (5) Relaxation
[0124] like Figure 7As shown in the figure, an ultrasonic displacement sensor 300 is arranged below the conveying path of the film 1 at the middle point between the conveying rollers 50a and 50b (distance between rollers: 912 mm), and the distance from the ultrasonic displacement sensor to the stretched film is measured at the center and end portions in the width direction when conveying at a conveying tension of 150 N / m, and the maximum distance (L MAX ) and the minimum distance (L MIN ) difference (L MAX -L MIN ) as the slack amount (mm). In addition, the measurement of the slack amount is performed by cutting off the tension applied to correct the slack using a suction roll or the like, and then conveying the roll at a conveying tension of 150 N / m.
[0125] <Example 1>
[0126] (Production of polyester carbonate resin film)
[0127] The polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux cooler controlled at 100° C. 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of ISB, 42.28 parts by mass (0.139 mol) of SPG, 63.77 parts by mass (0.298 mol) of DPC and 1.19×10 mol of calcium acetate monohydrate as a catalyst were added. -2 Mass parts (6.78×10 -5 mol). After the reactor was replaced with nitrogen under reduced pressure, it was heated by a heat medium and stirring was started when the internal temperature reached 100°C. After 40 minutes from the start of heating, the internal temperature reached 220°C, and the temperature was kept under control while the pressure was reduced. After reaching 220°C, it reached 13.3 kPa in 90 minutes. The phenol vapor produced as a by-product during the polymerization reaction was introduced into a 100°C reflux cooler, and a certain amount of monomer components contained in the phenol vapor was returned to the reactor. The uncondensed phenol vapor was introduced into a 45°C condenser for recovery. Nitrogen was introduced into the first reactor, and after temporarily restoring the pressure to atmospheric pressure, the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, the temperature and pressure reduction in the second reactor were started, and the internal temperature reached 240°C and the pressure reached 0.2 kPa in 50 minutes. After that, polymerization was carried out until the specified stirring power was reached. When the specified power was reached, nitrogen was introduced into the reactor for restoring the pressure, the generated polyester carbonate was extruded into water, and the strands were cut to obtain pellets. The Tg of the obtained polyester carbonate resin was 140°C.
[0128] After the obtained polyester carbonate resin was vacuum dried at 80°C for 5 hours, a resin film with a thickness of 135 μm was prepared using a film-making device having a uniaxial extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chilled roll (setting temperature: 120-130°C) and a winder.
[0129] (Production of stretched film)
[0130] use Figures 1 to 3 The stretching device shown in the figure obliquely stretches the polyester carbonate resin film obtained as above to obtain a phase difference film.
[0131] Specifically, a stretching device having a structure in which the left endless loop in the holding area is shorter and longer than the right endless loop is used. A polyester carbonate resin film is continuously supplied in an oblique direction relative to the conveying direction of the film in the stretching device (the conveying direction X of the film during oblique stretching), and the left and right ends of the film are simultaneously held at the entrance of the stretching device using left and right clamps with the same clamp spacing (P1=125mm). Specifically, the film is supplied to the stretching device in such a manner that the conveying direction Y of the film before being held by the clamp forms an angle of 10° relative to the conveying direction X of the film during oblique stretching, and the right end becomes a concave side (i.e., the conveying direction Y is rotated counterclockwise at an angle of 10° relative to the conveying direction X). In addition, the angle formed by the line Z connecting the left and right clamps when holding the film and the conveying direction Y of the film before being held by the left and right clamps is 90°. The conveying direction of the film is changed from the Y direction to the X direction in the holding area, and it is moved to the preheating area.
[0132] The film was preheated to 145° C. in the preheating zone B. In the preheating zone, the clamp distance between the left and right clamps was set to P1 (125 mm).
[0133] Next, as the film enters the stretching region C, the clamp spacing of the right clamp begins to increase and the clamp spacing of the left clamp begins to decrease. While the clamp spacing of the right clamp is increased to P2, the clamp spacing of the left clamp is reduced to P3 (first oblique extension). At this time, the clamp spacing change rate (P2 / P1) of the right clamp is 1.42, the clamp spacing change rate (P3 / P1) of the left clamp is 0.78, and the lateral stretch ratio relative to the original width of the film is 1.45 times. Next, while maintaining the clamp spacing of the right clamp at P2, the clamp spacing of the left clamp begins to increase from P3 to P2 (second oblique extension). During this period, the rate of change (P2 / P3) of the clamp spacing of the left clamp is 1.82, and the lateral stretch ratio relative to the original width of the film is 1.9 times. In addition, the stretching region C is set to Tg+3.2°C (143.2°C).
[0134] Next, the film was held at 125° C. for 60 seconds for thermal fixing in the release region D. After the thermally fixed film was cooled to 100° C., the left and right clamps were released.
[0135] Furthermore, before producing the above-mentioned stretched film, except that the film is not supplied from the oblique direction (specifically, except that the film is supplied to the stretching device in such a manner that the conveying direction Y of the film before being clamped by the clamp becomes parallel to the conveying direction X of the film during oblique stretching, and the angle formed by the line Z connecting the left and right clamps when holding the film and the conveying direction Y of the film before being clamped by the left and right clamps is 90°), when the stretched film is obtained in the same manner as in Example 1, the left end portion in the width direction slackens by 16 mm.
[0136] <Example 2>
[0137] A stretched film was obtained in the same manner as in Example 1 except that the angle between the conveying direction Y of the film before being gripped by the clamps and the conveying direction X of the film during oblique stretching was 20°. In addition, the angle between the line Z connecting the left and right clamps when gripping the film and the conveying direction Y of the film before being gripped by the left and right clamps was 90°.
[0138] Furthermore, before producing the above-mentioned stretched film, except that the film is not supplied from the oblique direction (specifically, except that the film is supplied to the stretching device in such a manner that the conveying direction Y of the film before being clamped by the clamp becomes parallel to the conveying direction X of the film during oblique stretching, and the angle formed by the line Z connecting the left and right clamps when holding the film and the conveying direction Y of the film before being clamped by the left and right clamps is 90°), when the stretched film is obtained in the same manner as in Example 2, the left end portion in the width direction slackens by 17 mm.
[0139] <Example 3>
[0140] A stretched film was obtained in the same manner as in Example 1 except that the angle between the conveying direction Y of the film before being gripped by the clamps and the conveying direction X of the film during oblique stretching was 40°. In addition, the angle between the line Z connecting the left and right clamps when gripping the film and the conveying direction Y of the film before being gripped by the left and right clamps was 90°.
[0141] Furthermore, before producing the above-mentioned stretched film, except that the film is not supplied from the oblique direction (specifically, except that the film is supplied to the stretching device in such a manner that the conveying direction Y of the film before being clamped by the clamp becomes parallel to the conveying direction X of the film during oblique stretching, and the angle formed by the line Z connecting the left and right clamps when holding the film and the conveying direction Y of the film before being clamped by the left and right clamps is 90°), when the stretched film is obtained in the same manner as in Example 3, the left end portion in the width direction relaxes by 17 mm.
[0142] <Comparative Example 1>
[0143] A stretched film is obtained in the same manner as in Example 1 except that the film is not supplied from an oblique direction (specifically, the film is supplied to the stretching device in such a manner that the conveying direction Y of the film before being clamped by the clamp becomes parallel to the conveying direction X of the film during oblique stretching, and the angle formed by the line Z connecting the left and right clamps when holding the film and the conveying direction Y of the film before being clamped by the left and right clamps is 90°).
[0144] [Appearance and handling evaluation]
[0145] The stretched films obtained in Examples 1 to 3 and Comparative Example 1 were laminated to a long masking film (Toray Film Processing Co., Ltd., product name "Toretec 7832C-30") in a roll-to-roll manner to obtain a film laminate. Next, the masking film was peeled off from the film laminate, an adhesive was applied using a gravure coater, and the film laminate was laminated to a polarizer and irradiated with UV to obtain an optical laminate. The appearance (visual) of the optical laminate and the handling properties of the stretched film were evaluated according to the following criteria.
[0146] ○: After laminating the masking film (laminating tension 150 N / m), no wrinkles were observed, and the adhesive could be applied to the entire surface of the film.
[0147] △: When laminating the masking film, the laminating tension was increased to 300 N / m, so that the masking film could be laminarized without wrinkles. However, when applying the adhesive, the adhesive could not be applied to the slackened portion.
[0148] ×: After the masking film was attached, there were wrinkles and the appearance was deteriorated.
[0149] Table 1 shows the evaluation results of the relaxation amount and the optical layered body.
[0150] Table 1
[0151]
[0152] <Evaluation>
[0153] As shown in Table 1, in the oblique stretching using the tenter-type simultaneous biaxial stretching device, by making the conveying direction of the film before being clamped by the clamps oblique relative to the conveying direction of the film during the oblique stretching, a long oblique stretched film with reduced slack can be obtained. In addition, by laminating the long oblique stretched film with reduced slack with the long optical film in a roll-to-roll manner, the occurrence of wrinkles can be suppressed.
[0154] Industrial Applicability
[0155] The method for producing a stretched film of the present invention is preferably used for producing a phase difference film, and as a result, can contribute to the production of image display devices such as liquid crystal display devices (LCD) and organic electroluminescent display devices (OLED).
Claims
1. A method for producing a stretched film, which is carried out using a stretching device in which a holding area, a preheating area, a stretching area and a release area are arranged in sequence from the inlet side to the outlet side of the film, The stretching device has left and right endless rings that are symmetrical in plan view from the preheating area to the release area. The left and right endless rings each have left and right clamps of a variable pitch type in which the clamp pitch in the longitudinal direction varies. The method for manufacturing the stretched film comprises: In the holding area, the left and right clamps are used to hold the left and right ends of the continuously conveyed long film in the width direction. In the stretching area, the left and right clamps are moved while changing the clamp spacing of at least one clamp to stretch the film obliquely. and in the release region, releasing the film from the left and right clamps; The conveying direction of the film before being gripped by the left and right clamps is inclined obliquely with respect to the conveying direction of the film during the oblique stretching. A line connecting the left and right clamps when holding the film is inclined obliquely with respect to the conveying direction of the film when the film is extended obliquely.
2. The method for producing a stretched film according to claim 1, in, The conveyance direction of the film before being gripped by the left and right clamps is inclined with respect to the conveyance direction of the film during the oblique stretching so that the unrelaxed end of the film becomes a concave side.
3. The method for producing a stretched film according to claim 1 or 2, in, The conveyance direction of the film before being gripped by the left and right clamps forms an angle of 10° to 40° with respect to the conveyance direction of the film during the oblique stretching.
4. The method for producing a stretched film according to claim 1 or 2, in, The oblique extension includes: (i) changing the clamp spacing of one of the left and right clamps from P to 1 Increase to P 2 , while changing the fixture spacing of the other fixture from P 1 Reduce to P 3 and (ii) changing the fixture spacing of each fixture in such a manner that the reduced fixture spacing and the increased fixture spacing become a prescribed equal spacing.
5. The method for producing a stretched film according to claim 4, in, P 2 / P 1 1.25~1.75, P 3 / P 1 It is greater than or equal to 0.50 and less than 1.
6. A method for producing an optical laminate, comprising: obtaining a long-strip stretched film by the production method according to any one of claims 1 to 5; and While conveying the long optical film and the long stretched film, their length directions are aligned and they are continuously bonded together.
7. The method for producing an optical layered body according to claim 6, in, The optical film is a polarizing plate, and the stretched film is a λ / 4 plate or a λ / 2 plate.
Citation Information
Patent Citations
JP1973045619A
Method for changing advancing direction of strip metal plate and device therefor
JP2000351506A
Optical film containing polymer having naphthyl group
JP2007161994A
Clip type sheet and film extension device
JP2008044339A
Web carrying direction change mechanism
JP2009046285A