Glass powder and preparation method thereof
The electron beam melting technology is used to prepare glass powder in a high vacuum environment, which solves the high cost and difficult continuous production problems of traditional high-temperature melting methods, improves the performance and production efficiency of glass powder, and realizes the rapid production of barium, strontium, and zirconium glass powder. Batch preparation.
Patent Information
- Application Number
- CN202210726797.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-06-23
AI Technical Summary
The traditional high-temperature melting method to prepare glass powder has the problems of high melting point, high cost, difficulty in continuous production and poor uniformity, which affects the batch consistency of product performance and glass fluidity.
Electron beam melting technology is used to prepare glass powder in a high vacuum environment. The electron beam is used to scan and melt the powder layer under the protection of an inert gas. The temperature and distribution of the molten pool are controlled to obtain glass powder. The final product is obtained through water quenching and grinding. product.
The rapid batch preparation of barium, strontium and zirconium glass powder is achieved, the specific surface area, transmittance and flexural strength of the glass powder are improved, and the production cost and process complexity are reduced.
Smart Images

Figure CN115124248B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of glass powder, and particularly relates to glass powder and a preparation method thereof. Background Art
[0002] At present, the fillers of dental composite resin mainly include quartz powder, barium, strontium, zirconium glass powder and ceramic powder. The advantage of using them as fillers is that when they are added to the resin, the resin has excellent optical properties and X-ray blocking properties after polymerization. Due to the addition of heavy metal components, barium, strontium and zirconium glass powders need to be pre-mixed, heated at high temperature for a long time to ensure uniform mixing, and finally ground and sieved step by step to make the powder. The final finished product particle size is usually as small as 0.4-2μm.
[0003] The heavy metal oxides used in the glass powder formula are BaO, ZrO2, SrO2, etc., and their added content is 10%-50%. The main function is to increase the light transmittance of the glass and increase the radiation resistance of the glass. The aluminum oxide content is 10-50%, which is used to build the basic framework of the glass powder. The silicon oxide content is 10-50%, which is used to build the basic framework of the glass powder. The boron content is 10-30%, which plays a solubilizing role and can effectively reduce the melting temperature of the glass. The other ingredients are 1-5%.
[0004] The traditional preparation process of glass powder is:
[0005] (1) Batching and mixing: Batching the components according to the weight percentage. After batching, mix the components evenly by general stirring, dry method or wet method.
[0006] (2) Melting-water quenching: Melting at a temperature of 1500℃~1700℃ for 4-8 hours until the melt is clarified and uniform. The specific melting temperature depends on the actual situation. It is best to keep the melt clarified and maintain a certain homogenization time. After the glass melt is formed, the homogenization time should be maintained for more than 1 hour. Too long homogenization time will cause a certain degree of volatilization of the glass components. Water quenching after melting: The resulting melt is quenched in deionized water to obtain a glass frit.
[0007] (3) Fine screening: The obtained glass frit material is dried, and then dried after dry grinding or wet grinding. The obtained glass powder material is screened and selected, and then wet-ground in a ball mill, and then screened using a vibrating screening machine.
[0008] (4) Silanization treatment: The obtained glass powder is subjected to silanization treatment under a high-speed mixing device.
[0009] However, the traditional preparation process has the following disadvantages:
[0010] (1) The melting temperature is high. Glass powder containing barium, strontium and zirconium generally has a high melting temperature, above 1600°C. A special high-temperature furnace is required for processing. If a certain fluidity is required, the temperature of the furnace will be further increased.
[0011] (2) The output is low and it is difficult to carry out continuous production. Due to the high melting temperature and the need for a platinum crucible, special equipment and tools are required, and the investment and process operation of continuous production are relatively difficult. In addition, the high temperature causes the volatilization loss of B2O3 in the composition, affecting the batch consistency of product performance, and the glass has poor fluidity. Therefore, expensive platinum crucibles are usually required for smelting.
[0012] (3) Uniformity is difficult to ensure. The fluidity of the molten material during the smelting process is very poor, and a long reaction time is required. The temperature is high, boron volatilizes severely, the system compatibility is very poor, and the fusion of the metal oxide and glass system requires a long time. Summary of the invention
[0013] The purpose of the present invention is to propose a glass powder based on electron beam melting technology and a preparation method thereof, thereby overcoming the shortcomings of high melting point, high cost and difficulty in continuous production of glass prepared by high temperature melting method, and being able to quickly prepare barium, strontium and zirconium glass powders in batches.
[0014] In order to achieve the above object, the technical solution of the present invention is as follows:
[0015] A method for preparing glass powder comprises the following steps:
[0016] Weigh the raw materials and grind them;
[0017] Laying the ground raw material powder on a substrate to obtain a powder layer;
[0018] Under the protection of inert gas, the powder layer is scanned by an electron beam, and the powder layer is melted by electron beam irradiation to obtain a molten material; the irradiation density of the electron beam is 4000-6000kW / m 2 ;
[0019] Adding the molten material into water for water quenching to obtain glass cullets, and grinding the glass cullets to obtain the glass powder;
[0020] The raw materials include a first component, silicon dioxide, and a boron source compound; the first component is selected from one or more of a barium source compound, a strontium source compound, and a zirconium source compound.
[0021] The process characteristic of electron beam melting is that the melting is carried out in a high vacuum environment (the melting vacuum degree is generally 10 -3The temperature and distribution of the molten pool can be controlled during melting, and the maintenance time of the molten pool can be adjusted within a wide range. The melting is carried out in a crucible. It can be said that electron beam melting provides an indispensable means for the preparation of high melting point glass.
[0022] There are three basic processes in the electron beam melting process: (1) Vacuuming, vacuuming the material and the cavity. Reduce the resistance of the electron spray path to ensure that the electron beam can act on the material surface to the maximum extent; (2) Electron beam injection and acceleration. The electron beam is ejected through the electron gun. As the electron gun voltage increases, the initial velocity of the electron gun reaches the maximum. In addition, a magnetic field is applied to the ejected electrons during the injection process to ensure that they are injected onto the material surface with maximum accuracy. (3) Move the material so that the electron beam can be evenly sprayed on the material surface, and rotate the material so that each area can be evenly heated and melted.
[0023] The present invention finds that the glass powder can be prepared by electron beam melting technology using 4000-6000kW / m 2 The electron beam irradiation density is high, which greatly improves the specific surface area, transmittance and flexural strength of the obtained glass powder.
[0024] Preferably, in the above-mentioned method for preparing glass powder, the thickness of the powder layer is 0.5-3 mm.
[0025] Preferably, in the above-mentioned method for preparing glass powder, the melting rate of the powder layer is 50-1000 g / hr, more preferably 250-350 g / hr.
[0026] In electron beam melting technology, melting power, melting speed and material thickness are the most important factors affecting melting, and there is a certain restrictive relationship between them, which needs to be considered comprehensively. The present invention finds that by using the above-mentioned combination of electron beam irradiation density, powder layer thickness and melting speed, the specific surface area, light transmittance and flexural strength of the obtained glass powder are better.
[0027] Preferably, in the above-mentioned method for preparing glass powder, when the powder layer is melted by electron beam irradiation, the voltage of the electron gun emitting the electron beam is 50-300 kV.
[0028] Preferably, in the above-mentioned method for preparing glass powder, the raw materials, calculated on a total mass basis, comprise: 5-60% of the first component, 5-60% of silicon dioxide, and 1-25% of a boron source compound.
[0029] Further preferably, the raw materials include, by total mass, 20-40% of the first component, 20-40% of silicon dioxide, and 5-15% of the boron source compound. When the first component, silicon dioxide, and the boron source compound in the above proportions are compounded as the main raw materials, the specific surface area, light transmittance, and flexural strength of the obtained glass powder are better.
[0030] Preferably, in the above-mentioned method for preparing glass powder, the raw materials, calculated on a total mass basis, further comprise: 5 to 60% of an aluminum source compound, wherein the aluminum source compound is selected from one or more of aluminum oxide, aluminum hydroxide, aluminum carbonate, and aluminum nitrate; further preferably, the content of the aluminum source compound is 20 to 40%, and adding the aluminum source compound in the above-mentioned proportion can improve light transmittance.
[0031] Preferably, in the above-mentioned method for preparing glass powder, the raw materials, calculated on a total mass, further comprise: 0.1-6% of a second component, wherein the second component is arsenic trioxide and / or antimony oxide. Preferably, the content of the second component is 0.5-5%. Adding the second component in the above-mentioned proportion can improve light transmittance and reduce bubbles.
[0032] Preferably, in the above-mentioned method for preparing glass powder, the barium source compound is selected from one or more of barium carbonate, barium sulfate, barium hydroxide, barium oxide, and barium nitrate;
[0033] And / or, the strontium source compound is selected from one or more of strontium carbonate, strontium sulfate, strontium hydroxide, strontium oxide, and strontium nitrate;
[0034] And / or, the zirconium source compound is selected from one or more of zirconium nitrate, zirconium oxide, zirconium carbonate and zirconium hydroxide;
[0035] And / or, the boron source compound is selected from one or more of boric acid, borax, boron oxide and sodium borohydride.
[0036] Preferably, in the above-mentioned method for preparing glass powder, before spreading the powder, the raw material powder is dried at 100-200° C. for 3-5 hours.
[0037] Preferably, in the above-mentioned method for preparing glass powder, the particle size of the raw material powder after grinding is 0.1-2 microns.
[0038] The present invention also provides a glass powder, which is prepared by the above-mentioned preparation method.
[0039] The present invention has the following advantages:
[0040] The glass powder provided by the present invention is prepared by electron beam melting, and the specific surface area of the formed glass powder reaches 18m 2 / g or more, the light transmittance reaches more than 60%, and the flexural strength reaches more than 80Mpa. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is an electron microscope image of the raw material powder of Example 1 before melting.
[0042] Figure 2This is an electron microscope image of the raw material powder of Example 1 after electron beam melting.
[0043] Figure 3 This is an electron microscope image of the raw material powder of Example 2 before melting.
[0044] Figure 4 This is an electron microscope image of the raw material powder of Example 2 after electron beam melting. DETAILED DESCRIPTION
[0045] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0046] Example 1
[0047] Ingredients: barium carbonate 33%, silicon dioxide 30%, aluminum oxide 20%, boric acid 10%, sodium hydroxide 5%, solvent 2%;
[0048] Grinding: The above materials were ball milled for 4 hours at a grinding speed of 2000 rpm. The particle size of the raw material powder after grinding was 0.1-2 microns;
[0049] Drying: The above materials are dried in an oven to remove moisture, and the drying time is 10 hours;
[0050] Melting: The above materials are injected into the electron beam melting furnace, and smelted 4 times, each time four crucibles are put into the furnace with a total mass of 1kg. The material thickness is 1mm, and the electron beam density of the melting furnace is 5000kW / m 2 , melting time is 4 hr;
[0051] Water quenching: Put the molten material into cold water for water quenching to obtain glass;
[0052] Glass coarse grinding: the obtained glass is put into a jaw crusher to produce glass powder with a particle size of 10-500 μm;
[0053] Fine grinding of glass powder: the coarsely ground glass powder is put into a vibration mill to obtain glass powder with a particle size of 0.4-2 μm;
[0054] Drying: Dry the obtained sand-milled material in an oven for 10 hours;
[0055] Surface treatment: The obtained glass powder is surface treated with a silane coupling agent under high-speed dispersion;
[0056] Screening: The treated glass powder is screened to obtain the barium glass powder.
[0057] Figure 1 This is an electron microscope image of the raw material powder of Example 1 before melting. Figure 2This is an electron microscope image of the raw material powder after electron beam melting in Example 1. By comparison, it can be seen that under the above electron beam melting conditions, the raw material powder becomes a molten material.
[0058] Example 2
[0059] Ingredients: strontium carbonate 35%, silicon dioxide 30%, aluminum oxide 20%, borax 15%;
[0060] Grinding: The above materials were ball milled for 4 hours at a grinding speed of 2000 rpm. The particle size of the raw material powder after grinding was 0.1-2 microns;
[0061] Drying: The above materials are dried in an oven to remove moisture, and the drying time is 10 hours;
[0062] Melting: The above materials were injected into an electron beam melting furnace, and eight crucibles were put into the furnace twice with a total mass of 2 kg. The material thickness was 1 mm. The electron beam density of the melting furnace was 5000 kW / m2, and the melting time was 6 hours.
[0063] Water quenching: Put the molten material into cold water for water quenching to obtain glass;
[0064] Glass coarse grinding: the obtained glass is put into a jaw crusher to obtain a particle size of 10-500μm;
[0065] Fine grinding of glass powder: the coarsely ground glass powder is put into a vibration mill to obtain glass powder with a particle size of 0.4-2 μm;
[0066] Drying: Dry the obtained sand-milled material in an oven for 10 hours;
[0067] Surface treatment: The obtained glass powder is surface treated with a silane coupling agent under high-speed dispersion;
[0068] Screening: The treated glass powder is screened to obtain the strontium glass powder.
[0069] Figure 3 This is an electron microscope image of the raw material powder before melting. Figure 4 This is an electron microscope image of the raw material powder after electron beam melting. By comparison, it can be seen that under the above electron beam melting conditions, the raw material powder becomes a molten material.
[0070] Example 3
[0071] Ingredients: zirconium nitrate 35%, silicon dioxide 40%, borax 25%;
[0072] Grinding: The above materials were ball milled for 4 hours at a grinding speed of 2000 rpm. The particle size of the raw material powder after grinding was 0.1-2 microns;
[0073] Drying: The above materials are dried in an oven to remove moisture, and the drying time is 10 hours;
[0074] Melting: The above materials were injected into an electron beam melting furnace, and eight crucibles were put into the furnace twice with a total mass of 2 kg. The material thickness was 2 mm. The electron beam density of the melting furnace was 5000 kW / m2, and the melting time was 8 hours.
[0075] Water quenching: Put the molten material into cold water for water quenching to obtain glass;
[0076] Glass coarse grinding: the obtained glass is put into a jaw crusher to produce glass powder with a particle size of 10-500 μm;
[0077] Fine grinding of glass powder: the coarsely ground glass powder is put into a vibration mill to produce glass powder with a particle size of 0.4-2 μm;
[0078] Drying: Dry the obtained sand-milled material in an oven for 10 hours;
[0079] Surface treatment: The obtained glass powder is surface treated with a silane coupling agent under high-speed dispersion;
[0080] Screening: The treated glass powder is screened to obtain the zirconium glass powder.
[0081] Comparative Example 1
[0082] Compared with Example 1, the difference is that high temperature melting is used instead of electron beam melting.
[0083] Ingredients: barium carbonate 33%, silicon dioxide 30%, aluminum oxide 20%, boric acid 10%, sodium hydroxide 5%, solvent 2%;
[0084] Grinding: The above materials were ball milled for 4 hours at a grinding speed of 2000 rpm. The particle size of the raw material powder after grinding was 0.1-2 microns;
[0085] Drying: The above materials are dried in an oven to remove moisture, and the drying time is 10 hours;
[0086] Melting: inject the above materials into a glass melting furnace, the melting time is 15 hours, and the temperature is 1700-1800℃;
[0087] Water quenching: Put the molten material into cold water for water quenching to obtain glass;
[0088] Glass coarse grinding: the obtained glass is put into a jaw crusher to obtain a particle size of 10-500μm;
[0089] Fine grinding of glass powder: the coarsely ground glass powder is put into a vibration mill to obtain glass powder with a particle size of 0.4-2 μm;
[0090] Drying: Dry the obtained sand-milled material in an oven for 10 hours;
[0091] Surface treatment: The obtained glass powder is surface treated with a silane coupling agent under high-speed dispersion;
[0092] Screening: The treated glass powder is screened to obtain the barium glass powder.
[0093] Test example
[0094] 1. Use laser particle size instrument to measure particle size;
[0095] 2. Use the BET specific surface area test method to test the specific surface area of the particle surface;
[0096] 3. The obtained glass powder was mixed with a photocurable resin (the mixing ratio of the resin to the glass powder was 7:3), and the transmittance of the cured resin sample was measured using an ultraviolet spectrophotometer; the photocurable resin was a resin monomer BisGMA, and the photoinitiator was camphorquinone;
[0097] 4. Mix the obtained glass powder and light-curing resin, and use a mechanical testing machine to perform mechanical measurements on the cured resin sample.
[0098] Table 1
[0099]
[0100] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for preparing glass powder, characterized in that: The following steps are involved: Weigh the raw materials and grind them; Laying the ground raw material powder on a substrate to obtain a powder layer; the thickness of the powder layer is 0.5-3 mm, and the melting rate of the powder layer is 250-350 g / hr; Under the protection of inert gas, the powder layer is scanned by an electron beam, and the powder layer is melted by electron beam irradiation to obtain a molten material; the irradiation density of the electron beam is 4000-6000kW / m 2 ; Adding the molten material into water for water quenching to obtain glass cullets, and grinding the glass cullets to obtain the glass powder; The raw materials, calculated by total mass, include: 20-40% of the first component, 20-40% of silicon dioxide, and 5-15% of a boron source compound; the first component is selected from one or more of a barium source compound, a strontium source compound, and a zirconium source compound; The barium source compound is selected from one or more of barium carbonate, barium sulfate, barium hydroxide, barium oxide, and barium nitrate; The strontium source compound is selected from one or more of strontium carbonate, strontium sulfate, strontium hydroxide, strontium oxide, and strontium nitrate; The zirconium source compound is selected from one or more of zirconium nitrate, zirconium oxide, zirconium carbonate and zirconium hydroxide; The boron source compound is selected from one or more of boric acid, borax, boron oxide and sodium borohydride.
2. The method for preparing glass powder according to claim 1, characterized in that: The raw material further comprises, based on the total mass, 5 to 60% of an aluminum source compound, wherein the aluminum source compound is selected from one or more of aluminum oxide, aluminum hydroxide, aluminum carbonate, and aluminum nitrate, and the content of the aluminum source compound is 20 to 40%.
3. The method for preparing glass powder according to claim 1, characterized in that: The raw material further comprises, based on the total mass, 0.1-6% of a second component, wherein the second component is arsenic trioxide and / or antimony oxide, and the content of the second component is 0.5-5%.
4. The method for preparing glass powder according to any one of claims 1 to 3, characterized in that: Before spreading the powder, the raw material powder is dried at 100-200° C. for 3-5 hours.
5. A glass powder, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 4.