Membrane for protective film formation

By setting the color difference and brightness difference between the printed and non-printed areas in the protective film forming film, the problem of reduced print visibility is solved, and clear display of semiconductor chip information is achieved after curing and reflow processes. This method is suitable for the formation of protective films for semiconductor wafers and chips.

CN115132634BActive Publication Date: 2026-11-17LINTEC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210081668.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-25
Filing Date
2022-01-24
Publication Date
2026-11-17
Estimated Expiration
2042-01-24

AI Technical Summary

Technical Problem

As semiconductor devices become smaller, the linewidth of laser-printed characters becomes narrower, leading to reduced visibility of the characters. This is especially true during the film curing and reflow processes used in protective film formation, where information becomes difficult to identify, affecting the assembly and quality display of semiconductor devices.

Method used

By setting the color difference ΔE*ab between the printed and non-printed areas to be 8 or more in the protective film forming film, and satisfying the brightness difference ΔL* to be 8 or more, the brightness of the printed area is ensured to be higher than that of the non-printed area, thus forming a protective film with sufficient color and brightness difference and improving the visibility of the printed text.

Benefits of technology

Even with narrow printing line widths, by setting color and brightness differences, the protective film forming film can still maintain sufficient printing visibility after curing and reflow processes, ensuring the identification and quality display of semiconductor chip information.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115132634B_ABST
    Figure CN115132634B_ABST
Patent Text Reader

Abstract

This invention provides a protective film for forming a protective film that ensures sufficient visibility of the laser-printed text even when the line width is narrow. The protective film for forming a protective film is used for laser-printing text on its surface, wherein the color of the printed area is set to CIE1976L. * a * b * Lightness L in the coordinate system of color representation * p chromaticity a * p chromaticity b * p And set the color of the non-printed parts to CIE1976L * a * b * Lightness L in the coordinate system of color representation * N chromaticity a * N chromaticity b * N At that time, the color difference ΔE between the printed area and the non-printed area is defined by the following formula (A). * ab It is above 8. ΔE * ab =[(L * p -L * N ) 2 +(a * p -a * N ) 2 +(b * p -b * N ) 2 ] 1 / 2 ···(A).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a protective film forming film and a protective film forming sheet containing the protective film forming film, wherein the protective film forming film is attached to the back side of a semiconductor wafer or a semiconductor chip and is used to form a protective film. Background Technology

[0002] In recent years, semiconductor devices have been manufactured using a mounting method known as flip-chip. In this method, when mounting a semiconductor chip with circuit surfaces having electrodes such as bumps, the circuit surface side of the semiconductor chip is bonded to a chip mounting portion such as a lead frame. This results in a structure where the back side of the semiconductor chip, where no circuitry is formed, is exposed.

[0003] Therefore, in many cases, a protective film made of rigid organic material is formed on the back side of a semiconductor chip to protect it. This protective film is formed by using, for example, a semiconductor back-side film or a wafer back-side protective film integrated with diced tape as shown in Patent Document 1.

[0004] Protective films are sometimes used as components to display information about workpieces (e.g., semiconductor wafers) or processed objects (e.g., semiconductor chips) that have the protective film. Specifically, printing is sometimes performed, which creates raised or recessed areas on the surface of the protective film to display relevant information about the workpiece or processed object in a recognizable manner. This printing is typically done by irradiating the surface of the protective film with a laser. For semiconductor chips, the manufacturer's name or trademark, product name, product number, specifications, and other chip attributes are printed on them.

[0005] Regarding this, the semiconductor back-side film in Patent Document 1 has a transmittance of less than 20% at wavelengths of 532 nm or 1064 nm. This allows for printing via laser irradiation while preventing adverse effects from the laser from affecting the semiconductor device. There is a need to improve the visibility of information based on the unevenness of the surface formed on the protective film through printing (referred to in this specification as "print visibility"). Patent Document 2 provides an inspiration for improving print visibility by setting the average particle size of the filler incorporated in the protective film forming film to 0.4 μm or less. However, in recent years, with the miniaturization of semiconductor devices, the tendency for print visibility to decrease has become increasingly significant. Existing technical documents Patent documents

[0006] Patent Document 1: Japanese Patent Application Publication No. 2012-28396 Patent Document 2: International Publication WO2015 / 146936 Summary of the Invention The technical problem to be solved by the present invention

[0007] The inventors of this invention have studied the main reasons for the decrease in the visibility of printed characters. Protective film forming films typically contain thermosetting or energy-curable resins, curing agents, additives, colorants, and fillers. Laser printing can be performed before the protective film is cured, or it can be performed on a cured protective film. The printed information is then verified sequentially, moving between processes before finally being transferred to the assembly process. If the printed information is not sufficiently visible, the chip's properties may not be identified, leading to misidentification and malfunctions during movement between processes or during assembly.

[0008] Furthermore, semiconductor chips with laser-printed protective films are exposed to the reflow process during the mounting process. The reflow process is a process of melting the protruding solder on the substrate used to mount the chip or on the semiconductor chip itself, thus connecting the substrate and the semiconductor chip. During this process, the semiconductor chip is heated to approximately 260°C. Through the reflow process, the semiconductor chip and substrate are connected, thereby forming the product. However, the visibility of the printed text sometimes decreases after the reflow process. The information printed on the chip is not only used in the assembly process of the semiconductor device, but it also reflects the quality of the semiconductor device and has the function of improving design. Therefore, maintaining the visibility of the printed text is also required for commercially available semiconductor devices.

[0009] On the other hand, there has been a continuous pursuit of miniaturization and higher performance in semiconductor devices. As a result, the size of semiconductor chips has been continuously reduced, from several millimeters square to less than 1 millimeter square. Along with miniaturization, the area that can be laser-printed has also gradually become narrower, and the printed characters have become smaller, with the line width of printed text and graphics sometimes being 30μm or less.

[0010] Based on these facts, the inventors of this invention believe that narrowing the line width of the printed text will cause the line width to narrow further due to heating during the curing of the protective film or during reflow, thereby reducing the visibility of the printed text. Since the fluidity of the resin component contained in the protective film is temporarily increased during curing, there is a possibility that the line width of the laser-printed portion may narrow. Furthermore, even after curing, the protective film partially softens when exposed to a high temperature of approximately 260°C, causing deformation of the laser-printed portion and further reducing the visibility of the printed text.

[0011] Therefore, the object of the present invention is to provide a protective film for forming characters that can achieve sufficient visibility of the printed characters even when the line width of the printed characters is narrow. Technical means to solve technical problems

[0012] To solve the aforementioned technical problems, the inventors of this invention conducted thorough research and discovered that by setting the color difference between the printed and non-printed areas to a predetermined value or higher, sufficient visibility of the printed characters can be achieved even when the line width of the printed characters becomes narrower, thus completing this invention. In other words, the main point of this invention, which solves the aforementioned technical problems, is as follows.

[0013] (1) A protective film forming film, wherein laser printing is performed on the surface of the protective film forming film, wherein, Set the color of the printed area to CIE1976L. * a * b * Lightness L in the coordinate system of color representation * p chromaticity a * p chromaticity b * p And set the color of the non-printed parts to CIE1976L * a * b * Lightness L in the coordinate system of color representation * N chromaticity a * N chromaticity b * N hour, The color difference ΔE between the printed and non-printed areas is defined by the following formula (A). * ab The value is 8 or higher. ΔE * ab =[(L * p -L * N ) 2 +(a * p -a * N ) 2 +(b * p -b * N ) 2 ] 1 / 2 ···(A)

[0014] (2) The protective film forming film according to (1), wherein the brightness difference ΔL between the printed area and the non-printed area is defined by the following formula (B). * The value is 8 or higher. ΔL * =[(L * p-L * N ) 2 ] 1 / 2 ···(B)

[0015] (3) A protective film forming film according to (1) or (2), wherein the brightness L of the printed portion * p The brightness L of the non-printed part * N Satisfy L * p >L * N .

[0016] (4) The protective film forming film according to any one of (1) to (3), wherein the color of the printed part and the color of the non-printed part are: the color measured after the protective film forming film is heated to 130°C and cured after laser printing.

[0017] (5) The protective film forming film according to any one of (1) to (3), wherein the color of the printed portion and the color of the non-printed portion are: the color measured after the protective film forming film is heated to 180°C and cured by laser printing, and then further heated to 260°C for 10.8 minutes three times.

[0018] (6) A protective film forming film according to any one of (1) to (5), wherein the printed portion includes a portion with a line width of 50 μm or less.

[0019] (7) A protective film forming sheet comprising the protective film forming sheet and the support sheet described in any one of (1) to (6) above. Invention Effects

[0020] This invention provides a protective film for forming a protective film that ensures sufficient visibility of printed text even when the line width of the printed text is narrow during the curing of the protective film or the reflow process. Attached Figure Description

[0021] Figure 1 This is a schematic diagram illustrating an example of a protective film forming sheet according to this embodiment. Figure 2 This is a schematic diagram illustrating an example of a protective film forming sheet according to this embodiment. Figure 3 This is a schematic diagram illustrating an example of a protective film forming sheet according to this embodiment. Figure 4 This is a schematic diagram illustrating an example of a protective film forming sheet according to this embodiment. Figure 5This is a schematic diagram illustrating an example of a protective film forming sheet according to this embodiment. Figure 6 This is a schematic diagram illustrating an example of a protective film forming sheet according to this embodiment. Figure 7 This is a schematic diagram illustrating an example of a protective film forming sheet according to this embodiment. Figure 8 This is a schematic diagram illustrating an example of a protective film forming sheet according to this embodiment. Figure 9 This is a schematic diagram illustrating an example of the manufacturing process of the protective film forming sheet according to this embodiment. Explanation of reference numerals in the attached figures 1A, 1B, 1C, 1D, 1E, 1F, 1G, 1H: Protective film forming sheet; 10: Support sheet; 10a: Surface of support sheet; 10b: Back side (exposed side) of support sheet; 11: Substrate; 11a: Surface of substrate; 11b: Back side of substrate; 12: Adhesive layer; 12a: Surface of adhesive layer; 13, 23: Protective film forming layer; 13a, 23a: Surface of protective film forming layer; 14: Coating layer; 14a: Surface of coating layer; 14b: Back side of coating layer; 15: Release film; 15a: Surface of release film. Detailed Implementation

[0022] Membrane for protective film formation The protective film forming film is a curable film used to form a protective film on a workpiece such as a semiconductor wafer or a processed object (e.g., a semiconductor chip) obtained by processing the workpiece.

[0023] The protective film forming film of this embodiment is used as a protective film that is ultimately attached to workpieces such as semiconductor chips and has laser-printed on its surface. The protective film forming film of this embodiment undergoes surface modification by irradiation with a laser, and has a printed area with text, graphics, etc., and a non-printed area that is not irradiated with laser.

[0024] For the protective film forming film of this embodiment, the color of the printed area is set to CIE1976L. * a * b * Lightness L in the coordinate system of color representation * p chromaticity a * p chromaticity b * p And set the color of the non-printed parts to CIE1976L * a * b * Lightness L in the coordinate system of color representation *N chromaticity a * N chromaticity b * N At that time, the color difference ΔE between the printed area and the non-printed area * ab The value is 8 or higher, preferably 10 or higher, and even more preferably 15 or higher. Color difference ΔE * ab There is no specific upper limit, but considering design considerations, it is preferably below 120, more preferably below 90, and even more preferably below 80. If the color difference ΔE * ab If the value is 8 or higher, the visibility of the printed characters can be maintained even when exposed to heating caused by the curing or reflow of the protective film forming film when the printed characters are narrow. In addition, color difference ΔE * ab Defined by the following formula (A). ΔE * ab =[(L * p -L * N ) 2 +(a * p -a * N ) 2 +(b * p -b * N) 2 ] 1 / 2 ···(A)

[0025] In the protective film forming of this embodiment, the brightness difference ΔL between the printed area and the non-printed area is preferred. * The value is 8 or higher, and more preferably 10 or higher. Lightness difference ΔL * There is no specific upper limit, but considering design considerations, it is preferably 85 or below, more preferably 70 or below, and even more preferably 60 or below. If the brightness difference ΔL * If the value is 8 or higher, the visibility of the printed characters can be maintained even when exposed to heating caused by the curing or reflow of the protective film forming film when the printed characters are narrow. In addition, the difference in brightness ΔL * Defined by the following formula (B). ΔL * =[(L * p -L * N ) 2 ] 1 / 2···(B)

[0026] In the protective film forming film of this embodiment, the brightness L of the printed area is further preferred. * p The brightness L of the non-printed part * N Satisfy L * p >L * N Further optimization of L * p >1.5×L * N That is, if the brightness L of the printed characters... * p Brightness L higher than that of non-printed characters * N In this case, the printed text will appear to float on a darker background, thus providing excellent visibility.

[0027] As long as the color difference ΔE in this implementation plan is within the acceptable range. * ab Immediately after laser printing, the above-mentioned range is sufficient, but it is preferable that the range remains within this range throughout all subsequent processes. Regarding the brightness difference ΔL... * That's also true.

[0028] When laser printing is performed on an uncured protective film forming film, the color difference ΔE is preferably achieved in the following states: uncured state, state where the protective film forming film is cured to form a protective film, and state after the chip with the protective film is exposed to reflow conditions. * ab and brightness difference ΔL * Within the aforementioned range. Furthermore, when a protective film is formed by curing a protective film and then laser-printed onto it, the color difference ΔE is preferably achieved immediately after laser printing and after exposing the chip with the protective film to reflow conditions. * ab and brightness difference ΔL * Within the aforementioned range.

[0029] The protective film can be either thermosetting or energy-curable. When the protective film is thermosetting, the curing conditions are varied. In this embodiment, the color difference ΔE is measured in the state where the protective film is cured to form a protective film. * ab and brightness difference ΔL * During evaluation, the color difference ΔE was evaluated for the protective film obtained by heating and curing the protective film at 180°C for a sufficient time. * aband brightness difference ΔL * .

[0030] When mounting a chip with a protective film onto a substrate, a reflow process melts the solder, connecting the chip to the substrate. The heating conditions for the reflow process are not particularly limited. In this embodiment, the color difference ΔE after exposure to reflow conditions is measured. * ab and brightness difference ΔL * During the evaluation, the protective film on the chip was heated three times at 260°C for 10.8 minutes each under simulated reflow conditions, and the color difference ΔE was evaluated. * ab and brightness difference ΔL * .

[0031] This invention ensures sufficient visibility of the printed text even when the line width of the printed text is narrow, both during the curing of the protective film and after a reflow process. If the line width of the printed text is narrow, it will become even narrower, particularly in the narrower areas, during the curing of the protective film or the reflow process, thus reducing visibility. However, with the protective film of this embodiment, sufficient color difference exists between the printed and non-printed areas, ensuring adequate visibility even when the line width of the printed text becomes narrower after curing or the reflow process. Therefore, the protective film of this embodiment is particularly preferred for applications where the printed text has a width of 50 μm or less.

[0032] The protective film forming film of this embodiment may have a release film on one side or on both sides. When the release film is on two sides, the release films on the two sides may be the same or different. By having a release film, the protective film forming film of this embodiment can be provided as a long strip film wound into a roll. The release film is not particularly limited, and the same release film used in the protective film forming sheet described later can be used.

[0033] The protective film in this embodiment is cured to become a protective film. This protective film is used to protect the back side (the side opposite to the electrode formation surface) of a semiconductor wafer or semiconductor chip. The protective film is a soft film that can be easily attached to the object to which it is to be attached.

[0034] The following are non-limiting examples of the materials and manufacturing methods for the protective film forming of this embodiment.

[0035] As long as it is based on CIE1976L * a * b * In the coordinate system specified by the color system, the color difference ΔE between the printed and unprinted areas is... *ab If the above values ​​are met, the protective film can be either thermosetting or energy-curable. After curing, the protective film becomes a highly impact-resistant protective film. This protective film, for example, not only prevents cracks from forming on the semiconductor chip after the dicing process, but also enables good detection of the semiconductor chip with the protective film housed in a carrier tape.

[0036] The protective film can be formed using a thermosetting protective film forming film composition or an energy-curable protective film forming film composition (hereinafter, they are sometimes collectively referred to as "protective film forming film composition").

[0037] The protective film can be a single layer or multiple layers. When there are multiple layers, these multiple layers can be the same as each other or different from each other, and there is no particular limitation on the combination of these multiple layers.

[0038] The thickness of the protective film is not particularly limited, but is preferably 1 to 100 μm, more preferably 5 to 75 μm, and particularly preferably 5 to 50 μm. By making the thickness of the protective film at or above the aforementioned lower limit, the effect of preventing damage to the semiconductor wafer as the laser penetrates is improved when laser printing is performed on the protective film or the protective film forming film by irradiating it with a laser. In addition, the protective performance of the protective film is improved. On the other hand, by making the thickness of the protective film forming film below or below the aforementioned upper limit, the shrinkage of the film during curing can be reduced, and the effect of reducing the warpage of the semiconductor chip with the protective film is improved. Furthermore, during temperature cycling tests, the effect of suppressing stress generation caused by the difference in the coefficients of linear expansion between the protective film and the semiconductor wafer and the effect of suppressing the peeling of the protective film from the semiconductor wafer are improved.

[0039] The “thickness of the protective film forming membrane” refers to the overall thickness of the protective film forming membrane. For example, the thickness of the protective film forming membrane, which is composed of multiple layers, refers to the total thickness of all the layers that make up the protective film forming membrane.

[0040] The following will describe the case where the protective film forming film of this embodiment is a thermosetting protective film forming film formed by a thermosetting protective film forming film composition, and the case where the protective film forming film of this embodiment is an energy-curable protective film forming film formed by an energy-curable protective film forming film composition.

[0041] Thermosetting protective film forming membrane Examples of thermosetting protective film forming films include those containing a polymer component (A) and a thermosetting component (B), as described later. The polymer component (A) is considered to be a component formed by a polymerization reaction of a polymeric compound. Furthermore, the thermosetting component (B) is a component capable of undergoing a curing (polymerization) reaction induced by heat. Additionally, in this invention, the polymerization reaction also includes a condensation polymerization reaction.

[0042] <<Thermosetting Protective Film Forming Film Compositions>> A thermosetting protective film forming film can be formed from a thermosetting protective film forming film composition containing the constituent materials of the thermosetting protective film forming film. For example, a thermosetting protective film forming film composition can be applied to the surface to which the thermosetting protective film forming film is to be formed, and then dried as needed, thereby forming a thermosetting protective film forming film on the target area. The content ratio of the components that do not vaporize at room temperature in the thermosetting protective film forming film composition is generally the same as the content ratio of the aforementioned components in the thermosetting protective film forming film.

[0043] In addition, in this instruction manual, "room temperature" refers to the temperature without special cooling or heating, that is, the normal temperature, such as temperatures of 15 to 25°C.

[0044] The coating of the film composition for thermosetting protective film formation can be carried out using known methods, such as air knife coating machines, blade coaters, bar coaters, gravure coating machines, roller coaters, roller knife coaters, screen coaters, die coaters, knife coaters, screen coaters, Mayer bar coaters, kiss coaters, and other coating machines.

[0045] There are no particular limitations on the drying conditions of the film composition for forming thermosetting protective films, but when the film composition for forming thermosetting protective films contains the solvent described later, it is preferable to heat and dry it, for example, at 70 to 130°C for 10 seconds to 5 minutes.

[0046] <Film Composition for Protective Film Formation (1)> Examples of thermosetting protective film forming film compositions include thermosetting protective film forming film composition (1) containing polymer component (A) and thermosetting component (B) (sometimes abbreviated as "protective film forming film composition (1)" in this specification).

[0047] [Polymer component (A)] Polymer component (A) is a polymer compound used to impart film-forming properties, flexibility, etc., to thermosetting protective film formation.

[0048] The polymer component (A) contained in the protective film forming composition (1) and the thermosetting protective film forming film can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0049] Examples of polymer components (A) include acrylic resins (e.g., resins having (meth)acryloyl groups), polyesters, urethane resins (e.g., resins having urethane bonds), acrylate urethane resins, silicone resins (e.g., resins having siloxane bonds), rubber resins (e.g., resins having a rubber structure), phenoxy resins, thermosetting polyimides, etc., with acrylic resins being preferred.

[0050] As an acrylic resin in polymer component (A), well-known acrylic polymers can be cited.

[0051] The weight-average molecular weight (Mw) of the acrylic resin is preferably 10,000 to 2,000,000, more preferably 100,000 to 1,500,000. By setting the weight-average molecular weight of the acrylic resin to the lower limit or above, the shape stability (time stability during storage) of the thermosetting protective film is increased. Furthermore, by setting the weight-average molecular weight of the acrylic resin to the upper limit or below, the thermosetting protective film can more easily follow the uneven surface of the substrate, further suppressing the formation of voids between the substrate and the thermosetting protective film.

[0052] In addition, unless otherwise specified in this specification, “weight-average molecular weight” refers to the converted value of polystyrene determined by gel permeation chromatography (GPC).

[0053] The glass transition temperature (Tg) of the acrylic resin is preferably -60 to 70°C, more preferably -30 to 50°C. By setting the Tg of the acrylic resin to the lower limit or above, the adhesion between the protective film and the support sheet can be suppressed, and the peelability of the support sheet can be increased. Furthermore, by setting the Tg of the acrylic resin to the upper limit or below, the adhesion between the thermosetting protective film and the protective film and the adherend can be increased.

[0054] In this specification, "glass transition temperature" refers to the temperature at which the DSC curve of a sample is inflected when the sample is measured using a differential scanning calorimeter.

[0055] Examples of acrylic resins include polymers of one or more (meth)acrylates; copolymers of at least two monomers selected from (meth)acrylic acid, itaconic acid, vinyl acetate, acrylonitrile, styrene, and N-hydroxymethylacrylamide.

[0056] Examples of the (meth)acrylates constituting acrylic resins include, for example, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, n-octyl methacrylate, n-nonyl methacrylate, isononyl methacrylate, and so on. Alkyl methacrylates, including decyl methacrylate, undecyl methacrylate, dodecyl methacrylate (also known as lauryl methacrylate), tridecyl methacrylate, tetradecyl methacrylate (also known as myristyl methacrylate), pentadecyl methacrylate, hexadecyl methacrylate (also known as palmitate methacrylate), heptadecanyl methacrylate, octadecyl methacrylate (also known as stearate methacrylate), etc., in which the alkyl group constituting the alkyl ester has a chain structure with 1 to 18 carbon atoms; Isoborneol ester (meth)acrylate, dicyclopentyl ester (meth)acrylate, and other cycloalkyl esters of (meth)acrylate; (Meth)benzyl acrylate and other (meth)acrylate aralkyl esters; (Meth)acrylate dicyclopentenyl ester and other (meth)acrylate cycloalkenyl esters; (Meth)acrylate dicyclopentenoxyethyl ester and other (meth)acrylate cycloalkenyloxyalkyl esters; (meth)acrylimide; (Meth)acrylates containing glycidyl groups, such as glycidyl acrylate; Hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl methacrylate, and other hydroxyl-containing methacrylates; (Meth)acrylates such as N-methylaminoethyl methacrylate and other (meth)acrylates containing substituted amino groups. Here, "substituted amino group" refers to a group in which one or two hydrogen atoms of an amino group are replaced by a group other than a hydrogen atom.

[0057] Among them, n-butyl acrylate, methyl acrylate, glycidyl methacrylate and 2-hydroxyethyl acrylate are preferred.

[0058] Acrylic resins can be, for example, acrylic resins copolymerized from one or more monomers selected from (meth)acrylate, itaconic acid, vinyl acetate, acrylonitrile, styrene, and N-hydroxymethylacrylamide, in addition to the (meth)acrylates mentioned above.

[0059] The monomers that make up acrylic resins can be just one type or two or more types. When there are two or more types, their combination and ratio can be chosen arbitrarily.

[0060] Acrylic resins may possess functional groups such as vinyl, (meth)acryloyl, amino, hydroxyl, carboxyl, and isocyanate groups, which enable them to bond with other compounds. These functional groups of acrylic resins can be bonded to other compounds via a crosslinking agent (F) described later, or they can be directly bonded to other compounds without the crosslinking agent (F). By bonding acrylic resins to other compounds through the aforementioned functional groups, there is a tendency to increase the reliability of encapsulation obtained using protective film forming sheets.

[0061] In this invention, both thermoplastic resins other than acrylic resins (hereinafter, sometimes simply referred to as "thermoplastic resins") and acrylic resins can be used as polymer components (A).

[0062] By using the aforementioned thermoplastic resin, the peelability of the protective film when it is peeled off from the support sheet is increased, and the thermosetting protective film forming film becomes easier to follow the uneven surface of the substrate, which can further suppress the generation of gaps between the substrate and the thermosetting protective film forming film.

[0063] The weight-average molecular weight of the above-mentioned thermoplastic resin is preferably 1,000 to 100,000, more preferably 3,000 to 80,000.

[0064] The glass transition temperature (Tg) of the above-mentioned thermoplastic resin is preferably -30 to 150°C, more preferably -20 to 120°C.

[0065] Examples of the aforementioned thermoplastic resins include polyester, polyurethane, phenoxy resin, polybutene, polybutadiene, and polystyrene.

[0066] The thermoplastic resin contained in the protective film forming composition (1) and the thermosetting protective film forming film may be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0067] Regardless of the type of polymer component (A), the content of polymer component (A) is preferably 5 to 50% by mass, more preferably 10 to 40% by mass, and particularly preferably 15 to 35% by mass, relative to the total mass of all components except the solvent constituting the protective film forming composition (1) (i.e., relative to the total mass of the thermosetting protective film forming film).

[0068] Polymer component (A) is sometimes also a thermosetting component (B). In this invention, when the protective film forming film composition (1) contains such a component that is both a polymer component (A) and a thermosetting component (B), it is considered that the protective film forming film composition (1) contains both polymer component (A) and thermosetting component (B).

[0069] [Thermosetting component (B)] Thermosetting component (B) is a component used to cure the thermosetting protective film to form a hard protective film.

[0070] The thermosetting component (B) contained in the protective film forming composition (1) and the thermosetting protective film forming film can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0071] Examples of thermosetting components (B) include epoxy thermosetting resins, thermosetting polyimides, polyurethanes, unsaturated polyesters, and silicone resins, with epoxy thermosetting resins being preferred.

[0072] (Epoxy thermosetting resins) Epoxy thermosetting resins consist of epoxy resin (B1) and thermosetting agent (B2).

[0073] The epoxy thermosetting resin contained in the protective film forming composition (1) and the thermosetting protective film forming film can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0074] ·Epoxy resin (B1) As for epoxy resin (B1), well-known epoxy resins can be listed, such as multifunctional epoxy resins, biphenyl compounds, bisphenol A diglycidyl ether and its hydrides, o-cresol phenolic varnish epoxy resin, dicyclopentadiene type epoxy resin, biphenyl type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, phenylene skeleton type epoxy resin, and other epoxy compounds with more than one function.

[0075] Among them, bisphenol A type epoxy resin and dicyclopentadiene type epoxy resin are preferred.

[0076] As the epoxy resin (B1), an epoxy resin having unsaturated hydrocarbon groups can be used. Epoxy resins with unsaturated hydrocarbon groups have higher compatibility with acrylic resins than epoxy resins without unsaturated hydrocarbon groups. Therefore, by using an epoxy resin with unsaturated hydrocarbon groups, the reliability of the encapsulation obtained using a protective film forming sheet is increased.

[0077] As epoxy resins having unsaturated hydrocarbon groups, examples include compounds formed by converting a portion of the epoxy groups of multifunctional epoxy resins into groups having unsaturated hydrocarbon groups. These compounds can be obtained, for example, by reacting the epoxy groups with (meth)acrylic acid or a derivative thereof via an addition reaction.

[0078] In addition, in this specification, "derivative" refers to a substance in which at least one hydrogen atom of the original compound is replaced by a group (substituent) other than the hydrogen atom.

[0079] Furthermore, as epoxy resins having unsaturated hydrocarbon groups, examples include compounds formed by directly bonding unsaturated hydrocarbon groups to aromatic rings that constitute epoxy resins.

[0080] Unsaturated hydrocarbon groups are unsaturated groups that can polymerize. Specific examples include methine (vinyl), 2-propenyl (allyl), (meth)acryloyl, (meth)acrylamido, etc., with acryloyl being preferred.

[0081] The number average molecular weight of epoxy resin (B1) is not particularly limited, but from the perspective of curability of the film for forming thermosetting protective film, as well as the strength and heat resistance of the cured protective film, it is preferably 300 to 30,000, more preferably 300 to 10,000, and particularly preferably 300 to 3,000.

[0082] In this specification, unless otherwise specified, "number-average molecular weight" refers to the number-average molecular weight expressed as a conversion of standard polystyrene determined by gel permeation chromatography (GPC).

[0083] The epoxy equivalent of the epoxy resin (B1) is preferably 100 to 1100 g / eq, more preferably 150 to 1000 g / eq.

[0084] In this specification, "epoxy equivalent" refers to the number of grams (g / eq) of an epoxy compound containing 1 gram equivalent of epoxy groups, which can be determined according to the method of JIS K 7236:2001.

[0085] Epoxy resin (B1) can be used alone or in combination with two or more. When two or more are used, their combination and ratio can be chosen arbitrarily.

[0086] • Thermosetting agent (B2) The thermosetting agent (B2) functions as a curing agent for epoxy resin (B1).

[0087] As a thermosetting agent (B2), examples include compounds having at least two functional groups in one molecule that can react with epoxy groups. Examples of such functional groups include phenolic hydroxyl groups, alcoholic hydroxyl groups, amino groups, carboxyl groups, and groups formed by anhydride modification of acid groups. Phenolic hydroxyl groups, amino groups, or groups formed by anhydride modification of acid groups are preferred, and phenolic hydroxyl groups or amino groups are more preferred.

[0088] Among thermosetting agents (B2), phenolic curing agents with phenolic hydroxyl groups include, for example, multifunctional phenolic resins, biphenyl, phenolic varnish-type phenolic resins, dicyclopentadiene phenolic resins, and arylalkyl phenolic resins.

[0089] Among thermosetting agents (B2), amine curing agents containing amino groups are, for example, dicyandiamide.

[0090] Thermosetting agent (B2) may have unsaturated hydrocarbon groups.

[0091] Examples of thermosetting agents (B2) with unsaturated hydrocarbon groups include compounds in which a portion of the hydroxyl groups of phenolic resin are replaced by groups with unsaturated hydrocarbon groups, and compounds in which groups with unsaturated hydrocarbon groups are directly bonded to the aromatic ring of phenolic resin.

[0092] The unsaturated hydrocarbon groups in the thermosetting agent (B2) are the same as the unsaturated hydrocarbon groups in the epoxy resin having unsaturated hydrocarbon groups.

[0093] When using a phenolic curing agent as a thermosetting agent (B2), the thermosetting agent (B2) with a high softening point or glass transition temperature is preferred, in order to improve the peelability of the protective film when it is peeled off from the support sheet.

[0094] Thermosetting agent (B2) is preferably a thermosetting agent that is solid at room temperature and does not exhibit curing activity to epoxy resin (B1), but dissolves upon heating and exhibits curing activity to epoxy resin (B1) (hereinafter, sometimes abbreviated as "thermally active latent epoxy resin curing agent").

[0095] In addition, in this instruction manual, "room temperature" refers to the temperature without special cooling or heating, that is, the normal temperature, such as temperatures of 15 to 25°C.

[0096] The aforementioned thermoactive latent epoxy resin curing agent is stably dispersed in epoxy resin (B1) in the thermosetting protective film forming film at room temperature, but it becomes compatible with and reacts with epoxy resin (B1) upon heating. By using this thermoactive latent epoxy resin curing agent, the storage stability of the protective film forming sheet is significantly improved. For example, the migration of the curing agent from the protective film forming film to adjacent support sheets can be suppressed, effectively inhibiting the decrease in the thermosetting properties of the thermosetting protective film forming film. Furthermore, since the degree of thermosetting based on heating of the thermosetting protective film forming film further increases, the pick-up capability of the semiconductor chip with the protective film described later is improved.

[0097] Examples of thermoactive latent epoxy resin curing agents include onium salts, dicarboxylic acid hydrazides, dicyandiamide, and amine adducts of curing agents.

[0098] In the thermosetting agent (B2), for example, the number average molecular weight of the resin components such as multifunctional phenolic resin, phenolic varnish-type phenolic resin, dicyclopentadiene phenolic resin, and aralkyl phenolic resin is preferably 300 to 30,000, more preferably 400 to 10,000, and particularly preferably 500 to 3,000.

[0099] In the thermosetting agent (B2), the molecular weight of non-resin components such as biphenyl hydroquinone and dicyandiamide is not particularly limited, but is preferably, for example, 60 to 500.

[0100] Thermosetting agent (B2) can be used alone or in combination with two or more. When two or more are used, their combination and ratio can be chosen arbitrarily.

[0101] In the protective film forming composition (1) and the thermosetting protective film forming film, the content of the thermosetting agent (B2) is preferably 0.1 to 500 parts by mass, more preferably 1 to 200 parts by mass, relative to 100 parts by mass of epoxy resin (B1). By setting the content of the thermosetting agent (B2) to the lower limit or above, it is easier to cure the thermosetting protective film forming film. Furthermore, by setting the content of the thermosetting agent (B2) to the upper limit or below, the moisture absorption rate of the thermosetting protective film forming film can be reduced, and the reliability of the encapsulation obtained by using the protective film forming sheet is further improved.

[0102] In the protective film forming composition (1) and the thermosetting protective film forming film, the content of the thermosetting component (B) (e.g., the total content of epoxy resin (B1) and thermosetting agent (B2)) is preferably 1 to 100 parts by mass, more preferably 1.5 to 85 parts by mass, and particularly preferably 2 to 70 parts by mass, relative to 100 parts by mass of the polymer component (A). By keeping the above-mentioned content of the thermosetting component (B) within the above-mentioned range, the adhesion between the protective film and the support sheet can be suppressed, and the peelability of the support sheet is increased.

[0103] As another aspect, in the protective film forming film composition (1) and the thermosetting protective film forming film, the content of thermosetting component (B) is preferably 1 to 90% by mass, more preferably 10 to 80% by mass, and even more preferably 30 to 70% by mass, relative to the total mass of all components except solvent in the protective film forming film composition (1).

[0104] [Curing Accelerator (C)] The protective film forming film composition (1) and the thermosetting protective film forming film may contain a curing accelerator (C). The curing accelerator (C) is a component used to adjust the curing speed of the protective film forming film composition (1).

[0105] Preferred curing accelerators (C) include, for example, tertiary amines such as triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; imidazoles (imidazoles in which at least one hydrogen atom is substituted by a group other than a hydrogen atom) such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; organophosphines (phosphines in which at least one hydrogen atom is substituted by an organic group) such as tributylphosphine, diphenylphosphine, and triphenylphosphine; and tetraphenylboron salts such as tetraphenyl phosphonium tetraphenyl borate and triphenylphosphine tetraphenylborate.

[0106] Among them, 2-phenyl-4,5-dihydroxymethylimidazole is preferred.

[0107] The curing accelerator (C) contained in the protective film forming composition (1) and the thermosetting protective film forming film can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0108] When using the curing accelerator (C), in the protective film forming film composition (1) and the thermosetting protective film forming film, the content of the curing accelerator (C) is preferably 0.01 to 10 parts by mass relative to 100 parts by mass of the thermosetting component (B), more preferably 0.1 to 5 parts by mass. By setting the content of the curing accelerator (C) to the lower limit or above, the effects of using the curing accelerator (C) can be obtained more significantly. Furthermore, by setting the content of the curing accelerator (C) to the upper limit or below, for example, the effect of suppressing the highly polar curing accelerator (C) from migrating to the bonding interface with the adherend under high temperature and high humidity conditions in the thermosetting protective film forming film becomes more pronounced, and the reliability of the encapsulation obtained by using the protective film forming sheet is further improved.

[0109] [Filling Material (D)] The protective film forming composition (1) and the thermosetting protective film forming film may contain a filler material (D). By including the filler material (D) in the thermosetting protective film forming film, it becomes easier to adjust the coefficient of thermal expansion of the protective film obtained by curing the thermosetting protective film forming film. By optimizing the coefficient of thermal expansion for the object to which the protective film is formed, the reliability of the encapsulation obtained by using the protective film forming sheet is further improved. In addition, by including the filler material (D) in the thermosetting protective film forming film, the moisture absorption rate of the protective film can be reduced and the heat dissipation can be improved.

[0110] The filler material (D) can be either organic or inorganic, but is preferably inorganic.

[0111] Preferred inorganic filler materials include, for example, powders of inorganic materials such as silica, alumina, talc, calcium carbonate, titanium dioxide, red iron oxide, silicon carbide, and boron nitride; beads obtained by spherizing these inorganic filler materials; surface modifiers of these inorganic filler materials; single-crystal fibers of these inorganic filler materials; and glass fibers. Among these, silica or alumina are preferred inorganic filler materials.

[0112] The average particle size of the filler material (D) is preferably set to 0.1 to 10 μm. By keeping the particle size of the filler material (D) within the above range, the smoothness of the protective film can be maintained, and the filling performance can also be improved.

[0113] The filler material (D) contained in the protective film forming composition (1) and the thermosetting protective film forming film can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0114] When using filler material (D), in the protective film forming film composition (1), the content of filler material (D) relative to the total content (total mass) of all components except solvent (i.e., the content of filler material (D) in the thermosetting protective film forming film) is preferably 5 to 80% by mass, more preferably 7 to 60% by mass. By keeping the content of filler material (D) within the above range, the adjustment of the coefficient of thermal expansion becomes easier.

[0115] [Coupled agent (E)] The protective film forming composition (1) and the thermosetting protective film forming film may contain a coupling agent (E). As the coupling agent (E), by using a coupling agent having functional groups capable of reacting with inorganic or organic compounds, the adhesion and sealing properties of the thermosetting protective film forming film to the adhered object can be improved. Furthermore, by using the coupling agent (E), the heat resistance of the protective film obtained by curing the thermosetting protective film forming film is not compromised, and its water resistance is increased.

[0116] The coupling agent (E) is preferably a compound having functional groups that can react with functional groups of polymer component (A), thermosetting component (B), etc., and more preferably a silane coupling agent.

[0117] Examples of silane coupling agents include 3-glycidyl etheroxypropyltrimethoxysilane, 3-glycidyl etheroxypropylmethyldiethoxysilane, 3-glycidyl etheroxypropyltriethoxysilane, 3-glycidyl etheroxymethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, and 3-(2-aminoethylamino)propyltrimethoxysilane. Oxysilanes, 3-(2-aminoethylamino)propylmethyldiethoxysilane, 3-(phenylamino)propyltrimethoxysilane, 3-anilinepropyltrimethoxysilane, 3-ureapropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, bis(3-triethoxysilylpropyl)tetrasulfide, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriacetoxysilane, imidazole silane, etc.

[0118] The coupling agent (E) contained in the protective film forming composition (1) and the thermosetting protective film forming film can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0119] When using coupling agent (E), in the protective film forming film composition (1) and the thermosetting protective film forming film, the content of coupling agent (E) is preferably 0.03 to 20 parts by mass, more preferably 0.05 to 10 parts by mass, and particularly preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the total content of polymer component (A) and thermosetting component (B). By setting the content of coupling agent (E) to the lower limit or above, the effects of using coupling agent (E), such as improving the dispersibility of filler material (D) in the resin or improving the adhesion between the thermosetting protective film forming film and the adherend, can be obtained more significantly. Furthermore, by setting the content of coupling agent (E) to the upper limit or below, the generation of outgassing can be further suppressed.

[0120] [Crosslinking agent (F)] When the aforementioned acrylic resin or other components having functional groups such as vinyl, (meth)acryloyl, amino, hydroxyl, carboxyl, and isocyanate groups that can bond with other compounds are used as polymer components (A), the protective film forming film composition (1) and the thermosetting protective film forming film may further contain a crosslinking agent (F) for crosslinking the aforementioned functional groups with other compounds. By using the crosslinking agent (F) for crosslinking, the initial adhesive force and cohesive force of the thermosetting protective film forming film can be adjusted.

[0121] Examples of crosslinking agents (F) include organic polyisocyanate compounds, organic polyimide compounds, metal chelate crosslinking agents (crosslinking agents with metal chelate structures), and aziridine crosslinking agents (crosslinking agents with aziridine groups).

[0122] Examples of the aforementioned organic polyisocyanate compounds include, for example, aromatic polyisocyanate compounds, aliphatic polyisocyanate compounds, and alicyclic polyisocyanate compounds (hereinafter, these compounds are sometimes collectively referred to as "aromatic polyisocyanate compounds, etc."); trimers, isocyanurates, and adducts of the aforementioned aromatic polyisocyanate compounds, etc.; and terminal isocyanate carbamate prepolymers obtained by reacting the aforementioned aromatic polyisocyanate compounds, etc., with polyol compounds. The term "adduct" refers to the reaction product of the aforementioned aromatic polyisocyanate compounds, aliphatic polyisocyanate compounds, or alicyclic polyisocyanate compounds with low-molecular-weight compounds containing active hydrogen, such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, or castor oil. Examples of such adducts include the trimethylolpropane phenylene diisocyanate adduct, which will be described later. Furthermore, "terminal isocyanate carbamate prepolymer" refers to a prepolymer having a carbamate bond and an isocyanate group at the molecule's terminal end.

[0123] More specifically, examples of the aforementioned organic polyisocyanate compounds include 2,4- Compounds obtained by adding all or part of the hydroxyl groups of polyols such as toluene diisocyanate, 2,6-toluene diisocyanate, 1,3-phenylenedimethylene diisocyanate, 1,4-xylene diisocyanate, diphenylmethane-4,4'-diisocyanate, diphenylmethane-2,4'-diisocyanate, 3-methyldiphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, trimethylolpropane, etc., to any two or more of toluene diisocyanate, hexamethylene diisocyanate, and phenylenedimethylene diisocyanate; lysine diisocyanate, etc.

[0124] Examples of such organic polyimide compounds include N,N'-diphenylmethane-4,4'-bis(1-aziridinylcarboxamide), trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, and N,N'-toluene-2,4-bis(1-aziridinylcarboxamide)triethylene melamine.

[0125] When using an organic polyisocyanate compound as a crosslinking agent (F), a hydroxyl-containing polymer is preferably used as the polymer component (A). When the crosslinking agent (F) has isocyanate groups and the polymer component (A) has hydroxyl groups, a crosslinked structure can be easily introduced into the thermosetting protective film forming film through the reaction of the crosslinking agent (F) and the polymer component (A).

[0126] The crosslinking agent (F) contained in the protective film forming composition (1) and the thermosetting protective film forming film can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0127] When using a crosslinking agent (F), in the protective film forming film composition (1), the content of the crosslinking agent (F) is preferably 0.01 to 20 parts by mass relative to 100 parts by mass of the polymer component (A), more preferably 0.1 to 10 parts by mass, and particularly preferably 0.5 to 5 parts by mass. By setting the above-mentioned content of the crosslinking agent (F) to the lower limit or above, the effects brought about by using the crosslinking agent (F) can be obtained more significantly. Furthermore, by setting the above-mentioned content of the crosslinking agent (F) to the upper limit or below, excessive decrease in the adhesion between the thermosetting protective film forming film and the support sheet or the thermosetting protective film forming film and the semiconductor wafer or semiconductor chip can be suppressed. In the present invention, the effects of the present invention can be fully obtained even without using the crosslinking agent (F).

[0128] [Energy-cured resin (G)] The protective film forming composition (1) may contain an energy-curable resin (G). By containing the energy-curable resin (G) in the thermosetting protective film forming film, its properties can be changed by irradiation with energy rays.

[0129] Energy-curable resin (G) is obtained by polymerizing (curing) an energy-curable compound.

[0130] Examples of energy-curable compounds include those having at least one polymerizable double bond within the molecule, with acrylate compounds having a (meth)acryloyl group being preferred.

[0131] Examples of the aforementioned acrylate compounds include, for example, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and other (meth)acrylates containing a chain-like aliphatic backbone; dicyclopentyl di(meth)acrylate and other (meth)acrylates containing a cyclic aliphatic backbone; polyethylene glycol di(meth)acrylate and other polyalkylene glycol (meth)acrylates; low-polyester (meth)acrylates; urethane (meth)acrylate oligomers; epoxy-modified (meth)acrylates; polyether (meth)acrylates other than the aforementioned polyalkylene glycol (meth)acrylates; itaconic acid oligomers, etc.

[0132] The weight-average molecular weight of the above-mentioned energy-curable compound is preferably 100 to 30,000, more preferably 300 to 10,000.

[0133] The energy-curable compound used for polymerization can be one or more compounds. When there are more than two compounds, their combination and ratio can be arbitrarily selected.

[0134] The energy-curable resin (G) contained in the protective film forming film composition (1) can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0135] In the protective film forming film composition (1), the content of energy-curable resin (G) is preferably 1 to 95% by mass, more preferably 2 to 90% by mass, and particularly preferably 3 to 85% by mass, relative to the total mass of all components of the protective film forming film composition (1) excluding solvent.

[0136] [Photopolymerization initiator (H)] When the protective film forming film composition (1) contains an energy-curable resin (G), it may also contain a photopolymerization initiator (H) in order to effectively carry out the polymerization reaction of the energy-curable resin (G).

[0137] As the photopolymerization initiator (H) in the protective film forming film composition (1), the same photopolymerization initiator as the photopolymerization initiator in the adhesive composition (i) described later can be listed.

[0138] The photopolymerization initiator (H) contained in the protective film forming film composition (1) can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0139] In the protective film forming film composition (1), the content of photopolymerization initiator (H) is preferably 0.1 to 20 parts by mass, more preferably 1 to 10 parts by mass, and particularly preferably 2 to 5 parts by mass, relative to 100 parts by mass of energy-curable resin (G).

[0140] [Coloring agent (I)] From the CIE1976L * a * b * In the coordinate system specified by the color system, the color difference ΔE between the printed and unprinted areas is... * ab From the perspective of a protective film forming film that satisfies the above values, it is preferable that the protective film forming film composition (1) contains a colorant (I).

[0141] As a coloring agent (I), as long as it is possible to obtain the colorant according to CIE 1976L * a * b * In the coordinate system specified by the color system, the color difference ΔE between the printed and unprinted areas is... * ab There are no particular limitations on the protective film forming film that meets the above values. For example, known colorants such as inorganic pigments, organic pigments, and organic dyes can be used.

[0142] Examples of organic pigments and dyes mentioned above include, for example, aminium pigments, anthocyanin pigments, croconium pigments, squarylium pigments, azulenium pigments, polymethystylene pigments, naphthoquinone pigments, pyranium pigments, phthalocyanine pigments, naphthocyanin pigments, naphtholactam pigments, azo pigments, and condensed doublet pigments. Nitrogen-based pigments, indigo-based pigments, perinone-based pigments, perylene-based pigments, dioxazine-based pigments, quinacridone-based pigments, isoindolineone-based pigments, quinolineone-based pigments, pyrrole-based pigments, thioindigo-based pigments, metal complex pigments (metal complex salt dyes), dithiol metal complex pigments, indolephenol-based pigments, triarylmethane-based pigments, anthraquinone-based pigments, naphthol-based pigments, methylimino-based pigments, benzimidazole-based pigments, pinantrone-based pigments, and threne-based pigments, etc.

[0143] Examples of inorganic pigments mentioned above include carbon black, cobalt pigments, iron pigments, chromium pigments, titanium pigments, vanadium pigments, zirconium pigments, molybdenum pigments, ruthenium pigments, platinum pigments, ITO (indium tin oxide) pigments, and ATO (antimony tin oxide) pigments.

[0144] The colorant (I) contained in the protective film forming film composition (1) may be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0145] As long as we can obtain the standard CIE1976L * a * b * In the coordinate system specified by the color system, the color difference ΔE between the printed and unprinted areas is... * ab For a protective film forming film that satisfies the above values, the content of colorant (I) in the thermosetting protective film forming film is not particularly limited. However, relative to the total content (total mass) of all components except the solvent, the content of colorant (I) in the thermosetting protective film forming film is preferably 0.2% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.5% by mass or more. The upper limit of the content of colorant (I) in the thermosetting protective film forming film is not particularly limited. However, from the perspective of suppressing excessive decrease in the light transmittance of the thermosetting protective film forming film, the content of colorant (I) in the thermosetting protective film forming film is preferably 10% by mass or less, or may be set to 5% by mass or less, relative to the total content (total mass) of all components except the solvent.

[0146] [General Additives (J)] Without impairing the effects of the present invention, the protective film forming composition (1) and the thermosetting protective film forming film may contain general additives (J).

[0147] The general additive (J) can be any known additive and can be selected arbitrarily according to the purpose without particular limitation. However, as preferred examples, plasticizers, antistatic agents, antioxidants, and absorbents can be listed.

[0148] The protective film forming composition (1) and the thermosetting protective film forming film contain only one or more general additives (J). When there are two or more additives, their combination and ratio can be arbitrarily selected.

[0149] The content of the protective film forming composition (1) and the general additive (J) for thermosetting protective film forming is not particularly limited, and can be selected appropriately according to the purpose.

[0150] [Solvent (K)] The protective film forming membrane composition (1) preferably further contains a solvent (K). The protective film forming membrane composition (1) containing solvent (K) has good operability.

[0151] The solvent (K) mentioned above is not particularly limited, but as preferred examples, examples include hydrocarbons such as toluene and xylene; alcohols such as methanol, ethanol, 2-propanol, isobutanol (2-methylpropane-1-ol), and 1-butanol; esters such as ethyl acetate; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; and amides (compounds with amide bonds) such as dimethylformamide and N-methylpyrrolidone.

[0152] The solvent (K) contained in the protective film forming membrane composition (1) can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0153] From the perspective of being able to mix the components contained in the protective film forming film composition (1) more evenly, the solvent (K) contained in the protective film forming film composition (1) is preferably methyl ethyl ketone or the like.

[0154] Relative to the total mass of the above-mentioned protective film forming membrane composition, the solvent content is preferably an amount that makes the solid component concentration of the above-mentioned protective film forming membrane composition 10 to 80% by mass, more preferably an amount that makes the solid component concentration 20 to 70% by mass, and even more preferably an amount that makes the solid component concentration 30 to 65% by mass.

[0155] <<Preparation Method of Film Composition for Thermosetting Protective Film Formation>> The thermosetting protective film forming film composition (1) is obtained by incorporating each component used to constitute the thermosetting protective film forming film composition.

[0156] There is no particular order of addition when mixing the ingredients, and two or more ingredients may be added at the same time.

[0157] When using a solvent, the component can be pre-diluted by mixing the solvent with any other component besides the solvent, or it can be used by mixing the solvent with these components without pre-diluting any other component besides the solvent.

[0158] There are no particular limitations on the method of mixing the components during blending; any appropriate method may be selected from the following known methods: mixing by rotating a stir bar or stirring blade; mixing by using a mixer; mixing by applying ultrasound, etc.

[0159] As long as the individual blended components do not deteriorate, there are no particular limitations on the temperature and time when adding and mixing the components; they can be adjusted appropriately. However, the preferred temperature is 15℃ to 30℃.

[0160] • Membrane for forming protective films that can be cured by energy rays The film for forming an energy-curable protective film contains an energy-curable component (a).

[0161] The energy-curable component (a) is preferably uncured, more preferably adhesive, and even more preferably uncured and adhesive.

[0162] Furthermore, in this specification, "energy rays" refers to rays containing energy quanta within electromagnetic waves or charged particle beams. Examples of such energy rays include ultraviolet light and electron beams. For example, ultraviolet light can be irradiated using a high-pressure mercury lamp, a fusion lamp, or a xenon lamp as the ultraviolet light source. As for electron beams, irradiation can be achieved using electron beam accelerators or similar devices.

[0163] Furthermore, in this specification, "energy-ray curing property" refers to the property of curing by irradiation with energy rays, and "non-energy-ray curing property" refers to the property of not curing even when irradiated with energy rays.

[0164] <<Film Compositions for Forming Energy-Radiation Curable Protective Films>> The film for forming an energy-curable protective film can be formed from a film composition containing the constituent materials of the energy-curable protective film for forming an energy-curable protective film. For example, the film can be formed on the target area by coating the film composition with the energy-curable protective film for forming an surface and drying it as needed. The content ratio of the components that do not vaporize at room temperature in the film composition for forming an energy-curable protective film is generally the same as the content ratio of the components in the film for forming an energy-curable protective film. Herein, "room temperature" is as described above.

[0165] The coating of the film composition for forming an energy-curable protective film can be carried out using known methods, such as air knife coating machines, blade coaters, bar coaters, gravure coating machines, roller coaters, roller knife coaters, screen coaters, die coaters, knife coaters, screen coaters, Mayer bar coaters, kiss coaters, and other coating machines.

[0166] There are no particular limitations on the drying conditions of the film composition for forming an energy-curable protective film, but when the film composition for forming an energy-curable protective film contains the solvent described later, it is preferable to heat-dry it, for example, at 70 to 130°C for 10 seconds to 5 minutes.

[0167] <Film Composition for Protective Film Formation (2)> As a membrane composition for forming an energy-curable protective film, examples include an energy-curable protective film composition (2) containing the energy-curable component (a) described below (in this specification, it is sometimes simply referred to as "protective film forming membrane composition (2)").

[0168] [Energy-based solidification component (a)] The energy-curable component (a) is a component that is cured by irradiation with energy rays, and it is also a component used to impart film-forming properties, flexibility, etc., to the formation of energy-curable protective films.

[0169] Examples of energy-curable components (a) include polymers (a1) with a weight-average molecular weight of 80,000 to 2,000,000 having energy-curable groups, and compounds (a2) with a molecular weight of 100 to 80,000 having energy-curable groups. At least a portion of the polymer (a1) may be cross-linked by a cross-linking agent, or may not be cross-linked.

[0170] (Polymers with a weight-average molecular weight of 80,000 to 2,000,000 that have energy-ray curable groups (a1)) As a polymer (a1) having an energy-curable group with a weight average molecular weight of 80,000 to 2,000,000, an example of an acrylic resin (a1-1) can be cited. This acrylic resin (a1-1) is formed by an addition reaction between an acrylic polymer (a11) having functional groups that can react with groups that are present in other compounds and an energy-curable compound (a12) having groups that react with the aforementioned functional groups and energy-curable groups such as energy-curable double bonds.

[0171] Examples of functional groups in acrylic polymers (a11) that can react with groups found in other compounds include hydroxyl, carboxyl, amino, substituted amino (a group in which one or two hydrogen atoms of an amino group are replaced by a group other than a hydrogen atom), and epoxy groups. However, to prevent corrosion of circuits such as semiconductor wafers or semiconductor chips, functional groups other than carboxyl groups are preferred. The functional group mentioned above is preferably a hydroxyl group.

[0172] • Acrylic polymers with functional groups (a11) As an acrylic polymer with functional groups (a11), examples include polymers formed by copolymerizing acrylic monomers with the aforementioned functional groups with acrylic monomers without the aforementioned functional groups, and polymers formed by further copolymerizing monomers other than acrylic monomers (non-acrylic monomers) in addition to these monomers.

[0173] Furthermore, the aforementioned acrylic polymer (a11) can be a random copolymer or a block copolymer.

[0174] Examples of acrylic monomers having the aforementioned functional groups include hydroxyl-containing monomers, carboxyl-containing monomers, amino-containing monomers, substituted amino-containing monomers, and epoxy-containing monomers.

[0175] Examples of hydroxyl-containing monomers include hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl methacrylate, and other hydroxyalkyl methacrylates; and non-methacrylic unsaturated alcohols such as vinyl alcohol and allyl alcohol (i.e., unsaturated alcohols that do not have a methacryloyl skeleton).

[0176] Examples of the aforementioned carboxyl-containing monomers include, for example, (meth)acrylic acid, crotonic acid, and other olefinically unsaturated monocarboxylic acids (i.e., monocarboxylic acids having olefinically unsaturated bonds); fumaric acid, itaconic acid, maleic acid, citraconic acid, and other olefinically unsaturated dicarboxylic acids (i.e., dicarboxylic acids having olefinically unsaturated bonds); anhydrides of the aforementioned olefinically unsaturated dicarboxylic acids; and (meth)acrylic acid carboxyl alkyl esters such as 2-carboxyethyl methacrylate.

[0177] Acrylic monomers having the above-mentioned functional groups are preferably hydroxyl-containing monomers or carboxyl-containing monomers, and more preferably hydroxyl-containing monomers.

[0178] Furthermore, in this specification, "(meth)acrylic acid" is a concept that includes both "acrylic acid" and "methacrylic acid". Similarly, similar terms, such as "(meth)acrylate", include both "acrylate" and "methacrylate". "(Meth)acryloyl" is a concept that includes both "acryloyl" and "methacryloyl".

[0179] The acrylic monomers having the above-mentioned functional groups constituting the above-mentioned acrylic polymer (a11) can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0180] As acrylic monomers lacking the aforementioned functional groups, preferably (meth)acrylate alkyl esters, where the alkyl group constituting the alkyl ester has a chain structure with 1 to 18 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and so on. Octyl acrylate, nonyl acrylate, isononyl acrylate, decyl acrylate, undecyl acrylate, dodecyl acrylate (also known as lauryl acrylate), tridecyl acrylate, tetradecyl acrylate (also known as myristyl acrylate), pentadecyl acrylate, hexadecyl acrylate (also known as palmitate acrylate), heptadecanyl acrylate, octadecyl acrylate (also known as stearate acrylate), etc.

[0181] In addition, examples of acrylic monomers that do not have the above-mentioned functional groups include methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, and other methacrylates containing alkoxyalkyl groups; methacrylates containing aromatic groups such as phenyl methacrylate and aryl methacrylates; non-crosslinked methacrylamide and its derivatives; and non-crosslinked methacrylates containing tertiary amino groups such as N,N-dimethylaminoethyl methacrylate and N,N-dimethylaminopropyl methacrylate.

[0182] The acrylic monomers that do not have the above-mentioned functional groups that constitute the above-mentioned acrylic polymer (a11) can be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0183] Examples of non-acrylic acid monomers mentioned above include olefins such as ethylene and norbornene; vinyl acetate; and styrene.

[0184] The non-acrylic monomers constituting the above-mentioned acrylic polymer (a11) may be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0185] In the aforementioned acrylic polymer (a11), the proportion (content) of structural units derived from acrylic monomers having the aforementioned functional groups, relative to the total mass of the structural units constituting the acrylic polymer (a11), is preferably 0.1 to 50% by mass, more preferably 1 to 40% by mass, and particularly preferably 3 to 30% by mass. By keeping the above proportions within the above range, the degree of curing of the protective film can be easily adjusted within a preferred range by adjusting the content of energy-curable groups in the acrylic resin (a1-1) obtained by copolymerizing the aforementioned acrylic polymer (a11) with the aforementioned energy-curable compound (a12).

[0186] The acrylic polymer (a11) constituting the acrylic resin (a1-1) may be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0187] • Energy-curing compounds (a12) The aforementioned energy-curable compound (a12) preferably has one or more groups selected from the group consisting of isocyanate groups, epoxy groups, and carboxyl groups, which are functional groups capable of reacting with the aforementioned acrylic polymer (a11). More preferably, it has an isocyanate group as the aforementioned functional group. When the aforementioned energy-curable compound (a12) has, for example, an isocyanate group as the aforementioned functional group, the isocyanate group readily reacts with the hydroxyl group of the acrylic polymer (a11) having a hydroxyl group as the aforementioned functional group.

[0188] The above-mentioned energy-curing compound (a12) preferably has 1 to 5 of the above-mentioned energy-curing groups in one molecule, and more preferably has 1 to 2 of the above-mentioned energy-curing groups.

[0189] Examples of energy-curable compounds (a12) include 2-methacryloyloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloyl isocyanate, allyl isocyanate, and ethyl 1,1-(bisacryloyloxymethyl)isocyanate. Acryloyl monoisocyanate compounds are obtained by reacting diisocyanate compounds or polyisocyanate compounds with hydroxyethyl (meth)acrylate. Acryloyl monoisocyanate compounds, etc., are obtained by reacting diisocyanate compounds or polyisocyanate compounds with polyol compounds and hydroxyethyl (meth)acrylate.

[0190] The energy-curable compound (a12) is preferably 2-methacryloyloxyethyl isocyanate.

[0191] The energy-curable compound (a12) constituting the above-mentioned acrylic resin (a1-1) may be only one type or two or more types. When there are two or more types, their combination and ratio can be arbitrarily selected.

[0192] The content of acrylic resin (a1-1) is preferably 1 to 40% by mass, more preferably 2 to 30% by mass, and particularly preferably 3 to 20% by mass, relative to the total mass of the components other than the solvent in the protective film forming film composition (2).

[0193] In the aforementioned acrylic resin (a1-1), the content of the energy-curable groups from the aforementioned energy-curable compound (a12) relative to the content of the aforementioned functional groups from the aforementioned acrylic polymer (a11) is preferably 20 to 120 mol%, more preferably 35 to 100 mol%, and particularly preferably 50 to 100 mol%. By keeping the content within the aforementioned range, the adhesive strength of the cured protective film is further increased. Furthermore, when the aforementioned energy-curable compound (a12) is a monofunctional compound (having one of the aforementioned groups in one molecule), the upper limit of the aforementioned content ratio is 100 mol%, but when the aforementioned energy-curable compound (a12) is a polyfunctional compound (having two or more of the aforementioned groups in one molecule), the upper limit of the aforementioned content ratio is sometimes greater than 100 mol%. Here, "from" refers to a change in chemical structure for polymerization.

[0194] The weight-average molecular weight (Mw) of the polymer (a1) is preferably 100,000 to 2,000,000, more preferably 300,000 to 1,500,000. The weight-average molecular weight is as described above.

[0195] When at least a portion of the polymer (a1) is crosslinked by a crosslinking agent, the polymer (a1) may be: a polymer formed by polymerizing a monomer that is not one of the monomers described as constituting the acrylic polymer (a11) and has a group that reacts with the crosslinking agent, and crosslinking it at the group that reacts with the crosslinking agent; or a polymer formed by crosslinking it at the group that reacts with the functional group from the energy ray curable compound (a12).

[0196] The protective film forming composition (2) and the energy-curable protective film forming film contain only one or more of the above-mentioned polymers (a1). When there are two or more polymers, their combination and ratio can be arbitrarily selected.

[0197] (Compounds with molecular weights of 100–80,000 that have energy-ray curing groups (a2)) The energy-curing group of a compound (a2) with a molecular weight of 100 to 80,000 that has an energy-curing group can be exemplified by groups containing energy-curing double bonds, and as preferred examples, (meth)acryloyl, vinyl, etc.

[0198] As long as the above conditions are met, the above compound (a2) is not particularly limited, and examples include low molecular weight compounds with energy-curable groups, epoxy resins with energy-curable groups, phenolic resins with energy-curable groups, etc.

[0199] As a low molecular weight compound having an energy-curable group in the above-mentioned compound (a2), examples include multifunctional monomers or oligomers, and preferably acrylate compounds having a (meth)acryloyl group.

[0200] Examples of the aforementioned acrylate compounds include 2-hydroxy-3-(meth)acryloyloxypropyl methacrylate, polyethylene glycol di(meth)acrylate, propoxylated ethoxylated bisphenol A di(meth)acrylate, 2,2-bis[4-((meth)acryloyloxypolyethoxy)phenyl]propane, ethoxylated bisphenol A di(meth)acrylate, 2,2-bis[4-((meth)acryloyloxydiethoxy)phenyl]propane, 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene, 2,2-bis[4-((meth)acryloyloxypolypropoxy)phenyl]propane, tricyclodecanediethanol di(meth)acrylate, and 1,10-decanediol. Di(meth)acrylates such as 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polybutylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 2,2-bis[4-((meth)acryloyloxyethoxy)phenyl]propane, neopentyl glycol di(meth)acrylate, ethoxylated polypropylene glycol di(meth)acrylate, and 2-hydroxy-1,3-di(meth)acryloyloxypropane are all difunctional (meth)acrylates. Tris(2-(meth)acryloyloxyethyl)isocyanurate, ε-caprolactone-modified tris(2-(meth)acryloyloxyethyl)isocyanurate, glyceryl ethoxylate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, di(trimethylolpropane)tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate ethoxylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate, dipentaerythritol hexa(meth)acrylate and other multifunctional (meth)acrylates; Multifunctional (meth)acrylate oligomers, such as urethane (meth)acrylate oligomers.

[0201] As for the epoxy resin having energy-curable groups or the phenolic resin having energy-curable groups in the above-mentioned compound (a2), for example, the resin described in paragraph 0043 of Japanese Patent Application Publication No. 2013-194102 can be used. Although the above-mentioned resin also belongs to the category of resins constituting the thermosetting components described later, it is regarded as the above-mentioned compound (a2) in this invention.

[0202] The weight-average molecular weight of the above-mentioned compound (a2) is preferably 100 to 30,000, more preferably 300 to 10,000.

[0203] The protective film forming composition (2) and the energy ray curable protective film forming film contain only one or more of the above-mentioned compounds (a2). When there are two or more compounds, their combination and ratio can be arbitrarily selected.

[0204] [Polymers without energy-curing groups (b)] When the protective film forming composition (2) and the energy-curable protective film forming film contain the above-mentioned compound (a2) as the above-mentioned energy-curable component (a), it is preferable to further contain a polymer (b) that does not have an energy-curable group. At least a portion of the polymer (b) described above may be cross-linked by a cross-linking agent, or may not be cross-linked.

[0205] Examples of polymers (b) that do not have energy-curable groups include acrylic polymers, phenoxy resins, urethane resins, polyesters, rubber resins, and urethane acrylate resins.

[0206] Among them, the polymer (b) is preferably an acrylic polymer (hereinafter, sometimes abbreviated as "acrylic polymer (b-1)").

[0207] The acrylic polymer (b-1) can be a known acrylic polymer, such as a homopolymer of one acrylic monomer, a copolymer of two or more acrylic monomers, or a copolymer of one or more acrylic monomers with one or more monomers other than acrylic monomers (non-acrylic monomers).

[0208] Examples of acrylic monomers constituting acrylic polymers (b-1) include alkyl (meth)acrylates, (meth)acrylates having a cyclic backbone, (meth)acrylates containing glycidyl groups, (meth)acrylates containing hydroxyl groups, and (meth)acrylates containing substituted amino groups. The term "substituted amino group" is as described above.

[0209] As the aforementioned alkyl methacrylates, preferably alkyl methacrylates in which the alkyl group forming the alkyl ester has a chain structure with 1 to 18 carbon atoms, such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, amyl methacrylate, hexyl methacrylate, heptyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, and so on. Octyl acrylate, nonyl acrylate, isononyl acrylate, decyl acrylate, undecyl acrylate, dodecyl acrylate (also known as lauryl acrylate), tridecyl acrylate, tetradecyl acrylate (also known as myristyl acrylate), pentadecyl acrylate, hexadecyl acrylate (also known as palmitate acrylate), heptadecanyl acrylate, octadecyl acrylate (stearate acrylate), etc.

[0210] Examples of (meth)acrylates having a cyclic skeleton include isobornyl (meth)acrylate, dicyclopentyl (meth)acrylate, and other cycloalkyl (meth)acrylates. (Meth)benzyl acrylate and other (meth)acrylate aralkyl esters; (Meth)acrylate dicyclopentenyl ester and other (meth)acrylate cycloalkenyl esters; (Meth)acrylate dicyclopentenyloxyethyl ester, etc., (meth)acrylate cyclopentenyloxyalkyl ester, etc. Examples of glycidyl acrylates containing glycidyl groups include glycidyl acrylate. Examples of hydroxyl-containing (meth)acrylates include hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0211] Examples of the aforementioned (meth)acrylates containing substituted amino groups include N-methylaminoethyl (meth)acrylate.

[0212] Examples of non-acrylic monomers constituting acrylic polymers (b-1) include olefins such as ethylene and norbornene; vinyl acetate; and styrene.

[0213] As a polymer (b) that is at least partially crosslinked by a crosslinking agent and does not have energy-curable groups, for example, a polymer formed by reacting the reactive functional groups in the polymer (b) with a crosslinking agent can be listed.

[0214] The reactive functional groups mentioned above can be selected appropriately based on the type of crosslinking agent, and there are no particular limitations. For example, when the crosslinking agent is a polyisocyanate compound, hydroxyl, carboxyl, and amino groups can be listed as reactive functional groups, among which hydroxyl groups, which have high reactivity with isocyanate groups, are preferred. Furthermore, when the crosslinking agent is an epoxy compound, carboxyl, amino, and amide groups can be listed as reactive functional groups, among which carboxyl groups, which have high reactivity with epoxy groups, are preferred. However, in order to prevent corrosion of the circuitry of semiconductor wafers or semiconductor chips, the reactive functional groups mentioned above are preferably groups other than carboxyl groups.

[0215] As a polymer (b) having the aforementioned reactive functional groups but lacking energy-curable groups, examples include polymers obtained by polymerizing monomers having at least the aforementioned reactive functional groups. When polymer (b) is an acrylic polymer (b-1), any one or both of the aforementioned acrylic monomers and non-acrylic monomers listed as monomers constituting the acrylic polymer, having the aforementioned reactive functional groups, may be used. For example, as a polymer (b) having a hydroxyl group as a reactive functional group, examples include polymers obtained by polymerizing hydroxyl-containing (meth)acrylates. In addition, polymers obtained by polymerizing monomers in which one or more hydrogen atoms of the aforementioned acrylic monomers or non-acrylic monomers are replaced by the aforementioned reactive functional groups may also be listed.

[0216] In the polymer (b) having reactive functional groups, the proportion (content) of structural units derived from monomers having reactive functional groups relative to the total mass of the structural units constituting the polymer (b) is preferably 1 to 20% by mass, more preferably 2 to 10% by mass. By keeping the above proportion within the above range, the degree of crosslinking in the polymer (b) becomes a more preferred range.

[0217] From the perspective of improving the film-forming properties of the protective film-forming film composition (2), the weight-average molecular weight (Mw) of the polymer (b) without energy-curable groups is preferably 10,000 to 2,000,000, more preferably 100,000 to 1,500,000. Herein, "weight-average molecular weight" is as described above.

[0218] The protective film forming composition (2) and the energy-curable protective film forming film contain only one polymer (b) that does not have energy-curable groups. When there are two or more polymers, their combination and ratio can be arbitrarily selected.

[0219] As a protective film forming membrane composition (2), examples include compositions containing either or both of the above-described polymer (a1) and compound (a2). Furthermore, when the protective film forming membrane composition (2) contains compound (a2), it is preferable to further contain a polymer (b) without energy-curable groups, and in this case, it is also preferable to further contain (a1). Alternatively, the protective film forming membrane composition (2) may not contain compound (a2), but may simultaneously contain the above-described polymer (a1) and polymer (b) without energy-curable groups.

[0220] When the protective film forming film composition (2) contains the above-mentioned polymer (a1), the above-mentioned compound (a2) and a polymer (b) without energy-curable groups, the content of the above-mentioned compound (a2) in the protective film forming film composition (2) is preferably 10 to 400 parts by mass, more preferably 30 to 350 parts by mass, relative to the total content of the above-mentioned polymer (a1) and the polymer (b) without energy-curable groups of 100 parts by mass.

[0221] In the protective film forming composition (2), the total content (total mass) of the energy-curable component (a) and the polymer (b) without energy-curable groups (i.e., the total content of the energy-curable component (a) and the polymer (b) without energy-curable groups in the energy-curable protective film forming film) is preferably 5 to 90% by mass, more preferably 10 to 80% by mass, and particularly preferably 20 to 70% by mass, relative to the total content (total mass) of the components other than the solvent. By keeping the above-mentioned proportion of the energy-curable component within the above-mentioned range, the energy-curability of the energy-curable protective film forming film becomes better.

[0222] The content of the energy-curable component (a) is preferably 1 to 80% by mass relative to the total mass of the components other than the solvent in the protective film forming film composition (2).

[0223] The content of the energy-curable component (a1) is preferably 1 to 80% by mass relative to the total mass of the components other than the solvent in the protective film forming film composition (2).

[0224] The content of the energy-curable component (a2) is preferably 1 to 80% by mass relative to the total mass of the components other than the solvent in the protective film forming film composition (2).

[0225] The content of the polymer (b) that does not have energy-curable groups is preferably 1 to 80% by mass relative to the total mass of the components other than the solvent in the protective film forming film composition (2).

[0226] In addition, the total content of the above components (a1), (a2), and (b) does not exceed 100% by mass.

[0227] In addition to the aforementioned energy-curable components, the protective film forming composition (2) may further contain one or more of the following selected from the group consisting of thermosetting components, photopolymerization initiators, fillers, coupling agents, crosslinking agents, colorants, and general additives, depending on the purpose. For example, by using the protective film forming composition (2) containing the aforementioned energy-curable components and thermosetting components, the adhesive force of the energy-curable protective film forming film to the adhered object increases upon heating, and the strength of the protective film formed by the energy-curable protective film forming film also increases.

[0228] The thermosetting components, photopolymerization initiator, filler, coupling agent, crosslinking agent, colorant, and general additives in the protective film forming film composition (2) can be listed as the same components as the thermosetting components (B), photopolymerization initiator (H), filler (D), coupling agent (E), crosslinking agent (F), colorant (I), and general additives (J) in the protective film forming film composition (1).

[0229] In the protective film forming film composition (2), the above-mentioned thermosetting components, photopolymerization initiators, fillers, coupling agents, crosslinking agents, colorants and general additives can each be used individually or two or more at the same time. When two or more are used at the same time, their combination and ratio can be arbitrarily selected.

[0230] The contents of the above-mentioned thermosetting components, photopolymerization initiators, fillers, coupling agents, crosslinking agents, colorants and general additives in the protective film forming film composition (2) can be adjusted appropriately according to the purpose, without any particular limitation.

[0231] Since the operability of the protective film forming film composition (2) is improved by dilution, it is preferable to further contain a solvent.

[0232] As a solvent contained in the protective film forming membrane composition (2), for example, the same solvent as that in the protective film forming membrane composition (1) can be listed.

[0233] The protective film forming composition (2) may contain only one solvent or two or more solvents.

[0234] <<Preparation Method of Film Composition for Energy-Based Curable Protective Film Formation>> The protective film forming composition (2) is an energy-curable protective film forming composition that can be obtained by incorporating the components used to constitute the composition.

[0235] There is no particular restriction on the order of addition when mixing the ingredients, and two or more ingredients can be added at the same time.

[0236] When using a solvent, the component can be pre-diluted by mixing the solvent with any other component besides the solvent, or it can be used by mixing the solvent with these components without pre-diluting any other component besides the solvent.

[0237] There are no particular limitations on the method of mixing the components during blending; any appropriate method may be selected from the following known methods: mixing by rotating a stir bar or stirring blade; mixing by using a mixer; mixing by applying ultrasound, etc.

[0238] As long as the individual blended components do not deteriorate, there are no particular limitations on the temperature and time when adding and mixing the components; they can be adjusted appropriately. However, the preferred temperature is 15℃ to 30℃.

[0239] Control of film color for protective film formation If the color difference ΔE between the printed area and the non-printed area * ab If the value is 8 or higher, the composition of the protective film forming film is not particularly limited. The protective film forming film contains the aforementioned resin components, additives such as curing agents, colorants (I), and fillers (D). The color of the protective film forming film is determined by the types and mixing ratios of these components. The color difference ΔE between the printed and non-printed areas. * ab and brightness difference ΔL * The difference in hue between the printed area (where the surface roughness of the irradiated area has changed due to laser irradiation, or the composition of the irradiated area has been modified, or the composition ratio has changed due to component volatilization) and the non-printed area (where the composition of the irradiated area ...) is defined in CIE 1976L. * a * b * The value is obtained by numerical conversion in the color system.

[0240] In this specification, the color difference ΔE between the printed area and the non-printed area is... * ab and brightness difference ΔL* The colors of the printed and unprinted areas after laser printing are calculated based on the conditions described in the embodiments below. Color difference ΔE between printed and non-printed areas * ab and brightness difference ΔL * The composition of the protective film can be controlled by the types and mixing ratios of the components that make up the film.

[0241] For example, by intensifying the color on the surface of the protective film before laser printing, the color difference ΔE * ab and brightness difference ΔL * The color difference is easily amplified. This is because the surface roughness of the printed area, generated by laser printing, increases the perceived whiteness due to diffuse reflection. Furthermore, compared to shades within the same color family, color differences are more likely to increase when designing tones that achieve complementary color relationships before and after laser printing, by employing a color scheme that creates complementary colors before and after the printing process. Additionally, when using colorants that are prone to evaporation due to laser irradiation, the amount of colorant in the printed area decreases, resulting in a different hue from the non-printed areas, leading to a color difference ΔE. * ab and brightness difference ΔL * It gets bigger.

[0242] Protective film forming sheet The protective film forming sheet of this embodiment includes the protective film forming film described above and the support sheet described later. Furthermore, the protective film forming film may have a release film on the surface where the support sheet is not present.

[0243] After the release film is removed, the protective film forming sheet of this embodiment is attached to the surface (back side) of the semiconductor wafer opposite to the side where the circuit is located using the protective film forming film. Then, at any stage, the protective film forming film is cured to form a protective film. Next, a stack consisting of a support sheet, a protective film or a protective film forming film, and a semiconductor wafer is further diced to create a stack consisting of a support sheet, a protective film or a protective film forming film, and a semiconductor chip. Finally, the semiconductor chip is picked up from the support sheet with a protective film on its back side. Thus, the protective film forming sheet of this embodiment is used to form a protective film on the back side of a semiconductor chip.

[0244] In this specification, even if the protective film forming sheet in the protective film forming sheet is cured by heating or irradiation with energy rays to form a protective film, it is still referred to as a protective film forming sheet as long as the laminated structure of the support sheet and the protective film is maintained. Furthermore, for example, when the support sheet in the protective film forming sheet has an adhesive layer, even if the adhesive layer is cured, it is still referred to as a protective film forming sheet as long as the laminated structure of the cured adhesive layer and the protective film forming sheet or the protective film is maintained.

[0245] As a support sheet, examples include support sheets having a substrate, and examples of such support sheets include sheets consisting only of a substrate; sheets consisting of other layers such as an adhesive layer, an intermediate layer, and a coating layer laminated on a substrate. These other layers can be a single layer or multiple layers (two or more). When there are multiple layers, these multiple layers can be the same or different from each other, and the combination of these multiple layers is not particularly limited. Furthermore, in this specification, it is not limited to the aforementioned other layers; "multiple layers can be the same or different from each other" means "all layers can be the same, all layers can be different, or only some layers can be the same." Further, "multiple layers can be different from each other" means "at least one of the materials and thicknesses of each layer is different from each other."

[0246] As described above, in this embodiment, sheets of various shapes can be used as the aforementioned support sheets. The protective film forming sheet of this embodiment will be described below according to the type of support sheet. Furthermore, for ease of understanding of the features of the present invention, important parts of the figures used in the following description are sometimes enlarged, and the dimensions and proportions of each component may not be the same as in reality.

[0247] Figure 1 A cross-sectional view of one embodiment of the protective film forming sheet of this embodiment is shown schematically.

[0248] Figure 1 The protective film forming sheet 1A shown has an adhesive layer 12 on a substrate 11, and a protective film forming film 13 on the adhesive layer 12. The support sheet 10 is a laminate of the substrate 11 and the adhesive layer 12, and the protective film forming sheet 1A has a configuration in which the protective film forming film 13 is laminated on one surface 10a of the support sheet 10. Furthermore, the protective film forming sheet 1A further has a release film 15 on the protective film forming film 13.

[0249] In the protective film forming sheet 1A, an adhesive layer 12 is laminated on one surface 11a of the substrate 11. A protective film forming film 13 is laminated on the entire surface 12a of the adhesive layer 12 (the side of the adhesive layer 12 opposite to the side that contacts the substrate 11). A clamping adhesive layer 16 is laminated on a portion of the surface 13a of the protective film forming film 13 (the side of the protective film forming film 13 opposite to the side that contacts the adhesive layer 12). A release film 15 is laminated on the surface of the protective film forming film 13a where the clamping adhesive layer 16 is not laminated and on the surface 16a of the clamping adhesive layer 16 (the upper surface, i.e., the side of the clamping adhesive layer 16 opposite to the side that contacts the protective film forming film 13 and the side surface).

[0250] The adhesive layer 16 for the fixture can be, for example, a single-layer structure containing adhesive components or a multi-layer structure, wherein layers containing adhesive components are stacked on both sides of the sheet serving as the core material.

[0251] Figure 1 The protective film forming sheet 1A shown is used in the following manner: with the release film 15 removed, the back side of a semiconductor wafer (not shown) is attached to the surface 13a of the protective film forming sheet 13, and further, the upper surface of the surface 16a of the clamping adhesive layer 16 is attached to a clamp such as an annular frame.

[0252] Figure 2 A cross-sectional view is shown schematically of another embodiment of the protective film forming sheet of this embodiment. Additionally, in Figure 2 In China, for the sake of Figure 1 The constituent elements shown are the same as the constituent elements, and are marked with the same constituent elements. Figure 1 The same symbols are used, but their detailed descriptions are omitted. In Figure 3 The same applies to subsequent diagrams.

[0253] Aside from the fact that it lacks the adhesive layer 16 for the clamps, Figure 2 The protective film forming sheet 1B shown is Figure 1 The protective film forming sheet 1A shown is the same. That is, in the protective film forming sheet 1B, an adhesive layer 12 is laminated on one surface 11a of the substrate 11, a protective film forming film 13 is laminated on the entire surface 12a of the adhesive layer 12 (the side of the adhesive layer 12 opposite to the side that contacts the substrate 11), and a release film 15 is laminated on the entire surface 13a of the protective film forming film 13 (the side of the protective film forming film 13 opposite to the side that contacts the adhesive layer 12).

[0254] Figure 2The protective film forming sheet 1B shown is used in the following manner: with the release film 15 removed, the back side of a semiconductor wafer (not shown) is attached to a portion of the central side of the surface 13a of the protective film forming sheet 13; further, the area of ​​the protective film forming sheet 13 surrounding the periphery of the semiconductor wafer is attached to a jig such as an annular frame.

[0255] Figure 3 A cross-sectional view is shown schematically of another embodiment of the protective film forming sheet of this embodiment.

[0256] Aside from the fact that it lacks adhesive layer 12, Figure 3 The protective film forming sheet 1C shown is Figure 1 The protective film forming sheet 1A shown is the same. That is, in the protective film forming sheet 1C, the support sheet 10 is composed only of the substrate 11. Furthermore, a protective film forming film 13 is laminated on one surface 11a of the substrate 11, a clamping adhesive layer 16 is laminated on a portion of the surface 13a of the protective film forming film 13 (the side of the protective film forming film 13 opposite to the side that contacts the substrate), and a release film 15 is laminated on the surface of the protective film forming film 13a where the clamping adhesive layer 16 is not laminated and on the surface 16a of the clamping adhesive layer 16 (the upper surface, i.e., the side of the clamping adhesive layer 16 opposite to the side that contacts the protective film forming film 13 and the side surface).

[0257] and Figure 1 The protective film forming sheet 1A shown is the same. Figure 3 The protective film forming sheet 1C shown is used in the following manner: with the release film 15 removed, the back side of a semiconductor wafer (not shown) is attached to the surface 13a of the protective film forming sheet 13, and further, the upper surface of the surface 16a of the clamping adhesive layer 16 is attached to a clamp such as an annular frame.

[0258] Figure 4 A cross-sectional view is shown schematically of another embodiment of the protective film forming sheet of this embodiment.

[0259] Aside from the fact that it lacks the adhesive layer 16 for the clamps, Figure 4 The protective film forming sheet 1D shown is Figure 3 The protective film forming sheet 1C shown is the same. That is, in the protective film forming sheet 1D, a protective film forming film 13 is laminated on one surface 11a of the substrate 11, and a release film 15 is laminated on the entire surface 13a of the protective film forming film 13 (the side of the protective film forming film 13 opposite to the side that contacts the substrate).

[0260] and Figure 2The protective film forming sheet 1B shown is the same. Figure 4 The protective film forming sheet 1D shown is used in the following manner: with the release film 15 removed, the back side of a semiconductor wafer (not shown) is attached to a portion of the central side of the surface 13a of the protective film forming sheet 13; further, the area of ​​the protective film forming sheet 13 surrounding the periphery of the semiconductor wafer is attached to a fixture such as an annular frame.

[0261] Figure 5 A cross-sectional view is shown schematically of another embodiment of the protective film forming sheet of this embodiment.

[0262] In addition to having a coating layer 14 on the surface of the substrate 11 opposite to the side without the adhesive layer 12 (hereinafter, sometimes referred to as the back side of the substrate) 11b, Figure 5 The protective film forming sheet 1E shown is... Figure 1 The protective film forming sheet 1A shown is the same.

[0263] That is, in the protective film forming sheet 1E, the support sheet 10 is a laminate formed by sequentially stacking a coating layer 14, a substrate 11 and an adhesive layer 12, and the protective film forming sheet 1E has a structure in which a protective film forming film 13 is stacked on one surface 10a of the support sheet 10. Furthermore, an adhesive layer 12 is laminated on one surface 11a of the substrate 11, a protective film forming film 13 is laminated on the entire surface 12a of the adhesive layer 12 (the side of the adhesive layer 12 opposite to the side that contacts the substrate 11), a clamping adhesive layer 16 is laminated on a portion of the surface 13a of the protective film forming film 13 (the side of the protective film forming film 13 opposite to the side that contacts the adhesive layer 12), and a release film 15 is laminated on the surface of the protective film forming film 13a where the clamping adhesive layer 16 is not laminated and on the surface 16a of the clamping adhesive layer 16 (the upper surface, i.e. the side of the clamping adhesive layer 16 opposite to the side that contacts the protective film forming film 13 and the side surface).

[0264] and Figure 1 The protective film forming sheet 1A shown is the same. Figure 5 The protective film forming sheet 1E shown is used in the following manner: with the release film 15 removed, the back side of a semiconductor wafer (not shown) is attached to the surface 13a of the protective film forming sheet 13, and the upper surface of the surface 16a of the clamping adhesive layer 16 is further attached to a clamp such as an annular frame.

[0265] Figure 6 A cross-sectional view of another embodiment of the protective film forming sheet of this embodiment is shown for illustrative purposes.

[0266] Except for the lack of the adhesive layer 16 for the clamp, the protective film forming sheet 1F shown here is... Figure 5 The protective film forming sheet 1E shown is the same. That is, in the protective film forming sheet 1F, an adhesive layer 12 is laminated on one surface 11a of the substrate 11, a protective film forming film 13 is laminated on the entire surface 12a of the adhesive layer 12 (the side of the adhesive layer 12 opposite to the side that contacts the substrate 11), and a release film 15 is laminated on the entire surface 13a of the protective film forming film 13 (the side of the protective film forming film opposite to the side that contacts the adhesive layer 12). Furthermore, similar to... Figure 5 Similar to the protective film forming sheet 1E shown, a coating layer 14 is laminated on the back side 11b of the protective film forming sheet of the substrate 11 (the side of the substrate 11 opposite to the side that contacts the adhesive layer 12).

[0267] and Figure 2 The protective film forming sheet 1B is the same as that shown. Figure 6 The protective film forming sheet 1F is used in the following manner: with the release film 15 removed, the back side of a semiconductor wafer (not shown) is attached to a portion of the central side of the surface 13a of the protective film forming sheet 13, and the area of ​​the protective film forming sheet 13 surrounding the periphery of the semiconductor wafer is further attached to a jig such as an annular frame.

[0268] Figure 7 A cross-sectional view of another embodiment of the protective film forming sheet of this embodiment is shown schematically.

[0269] Apart from the difference in the shape of the protective film forming sheet, the protective film forming sheet 1G shown here is similar to... Figure 1 The protective film forming sheet 1G shown is the same as the protective film forming sheet 1A. That is, the protective film forming sheet 1G has an adhesive layer 12 on the substrate 11, and a protective film forming film 23 on the adhesive layer 12. The support sheet 10 is a laminate of the substrate 11 and the adhesive layer 12, and the protective film forming sheet 1G has a configuration in which the protective film forming film 23 is laminated on one surface 10a of the support sheet 10. In addition, the protective film forming sheet 1G further has a release film 15 on the protective film forming film 23. Except for the difference in shape, the protective film forming film 23 is the same as the protective film forming film 13.

[0270] When viewed from above and viewed from above, the protective film forming sheet 1G has a smaller surface area than the adhesive layer 12 and has a shape such as a circle.

[0271] In the protective film forming sheet 1G, an adhesive layer 12 is laminated on one surface 11a of the substrate 11, and a protective film forming film 23 is laminated on a portion of the surface 12a of the adhesive layer 12 (the side of the adhesive layer 12 opposite to the side that contacts the substrate 11). Furthermore, a release film 15 is laminated on the surface of the adhesive layer 12a where the protective film forming film 23 is not laminated and on the surface 23a of the protective film forming film 23 (the upper surface, i.e., the side of the protective film forming film 23 opposite to the side that contacts the adhesive layer 12 and the side surface).

[0272] Figure 7 The protective film forming sheet 1G shown is used in the following manner: with the release film 15 removed, the back side of a semiconductor wafer (not shown) is attached to the surface 23a of the protective film forming sheet 23, and further, the unlaminated protective film forming sheet 23 in the surface 12a of the adhesive layer 12 is attached to a fixture such as an annular frame.

[0273] Figure 8 A cross-sectional view is shown schematically of another embodiment of the protective film forming sheet of this embodiment.

[0274] Except for the absence of adhesive layer 12, the protective film forming sheet 1H shown here is... Figure 7 The protective film forming sheet 1G shown is the same. That is, in the protective film forming sheet 1H, the support sheet is only composed of the substrate 11. In addition, a protective film forming film 23 is laminated on a portion of a surface 11a of the substrate 11, and a release film 15 is laminated on the surface of the substrate 11a where the protective film forming film 23 is not laminated and on the surface 23a of the protective film forming film 23 (the upper surface, i.e., the side of the protective film forming film 23 opposite to the surface that contacts the substrate 11 and the side surface).

[0275] Figure 8 The protective film forming sheet 1H shown is used in the following manner: with the release film 15 removed, the back side of a semiconductor wafer (not shown) is attached to the surface 23a of the protective film forming film 23. Further, the unlaminated protective film forming film 23 on the surface 11a of the substrate 11 is attached to a jig such as an annular frame using a jig adhesive layer (not shown). The jig adhesive layer can be made of materials that are compatible with... Figure 1 The same adhesive layer for clamps as shown in the figure 16.

[0276] In addition, for protective film forming sheets, regardless of the composition of the support sheet, they can be attached to clamps such as ring frames using an adhesive layer for clamping.

[0277] The protective film forming sheet in this embodiment is not limited to Figures 1-8 The protective film forming sheet shown can, without impairing the effects of the present invention, [provide protection for...]. Figures 1-8 The components of the protective film forming sheet shown may be modified or deleted, or other components may be added to the protective film forming sheet described herein.

[0278] In addition, Figure 1 , Figure 2 , Figure 5 , Figure 6 and Figure 7 In the previous description, a protective film forming sheet was used, in which the adhesive layer was directly contacted and placed on the substrate. However, in this embodiment, the protective film forming sheet may have an intermediate layer between the substrate and the adhesive layer. That is, in the protective film forming sheet of this embodiment, the support sheet may have a laminated structure consisting of a substrate, an intermediate layer, and an adhesive layer stacked sequentially.

[0279] In addition, Figure 3 , Figure 4 and Figure 8 In the previous section, a sheet for forming a protective film was described as having the protective film formed on a substrate in direct contact. However, in this embodiment, the protective film forming sheet may have an intermediate layer between the substrate and the protective film forming sheet.

[0280] Here, any layer can be selected as the intermediate layer depending on the purpose. As a preferred intermediate layer, for example, an intermediate layer that improves the tightness of two adjacent layers can be listed.

[0281] Furthermore, the layers of the protective film forming sheet in this embodiment, other than the aforementioned intermediate layer, can be disposed at any position.

[0282] The following provides a detailed description of each component of the protective film forming sheet according to this embodiment.

[0283] ○ Support plate In this embodiment, the support sheet constituting the protective film forming sheet is not particularly limited as long as the aforementioned protective film forming film can be provided. Preferred support sheets include, for example, those commonly used in the field of semiconductor wafer processing sheets as described above, which are composed solely of a substrate; support sheets formed by stacking a substrate and an adhesive layer; support sheets formed by stacking a coating layer and a substrate; and support sheets formed by sequentially stacking a coating layer, a substrate, and an adhesive layer. Furthermore, preferred support sheets include, for example, support sheets formed by stacking a substrate, an intermediate layer, and an adhesive layer; and support sheets in the above-described stacked structures where an intermediate layer is provided between adjacent layers.

[0284] That is, the support sheet can be composed of one layer (single layer) or multiple layers (two or more layers). When the support sheet is composed of multiple layers, these multiple layers can be the same as each other or different from each other, and there is no particular limitation on the combination of these multiple layers.

[0285] The thickness of the support sheet can be appropriately selected according to the purpose. From the perspective of giving the above-mentioned protective film forming sheet sufficient flexibility and attaching it well to the semiconductor wafer, it is preferably 10 to 500 μm, more preferably 20 to 350 μm, and even more preferably 30 to 200 μm.

[0286] The “thickness of the support sheet” refers to the total thickness of the various layers that make up the support sheet. For example, when the support sheet is made of a laminated substrate and an adhesive layer, it refers to the total thickness of the substrate and the adhesive layer.

[0287] Furthermore, in this specification, "thickness" refers to the average value obtained by measuring the thickness at any five points using a contact thickness gauge.

[0288] Substrate In this embodiment, the substrate constituting the support sheet is preferably made of various resins. Specific examples include polyethylene (low-density polyethylene, linear low-density polyethylene, high-density polyethylene, etc.), polypropylene, ethylene-propylene copolymer, polybutene, polybutadiene, polymethylpentene, polyvinyl chloride, vinyl chloride copolymer, polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyurethane, polyurethane acrylate, polyimide, ethylene-vinyl acetate copolymer, ionomer resin, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid copolymer, polystyrene, polycarbonate, fluororesin, and any hydrogenated, modified, crosslinked, or copolymerized resins of these resins.

[0289] The thickness of the substrate can be selected appropriately according to the purpose. When the support sheet is formed by stacking substrate, adhesive layer, and other layers, the thickness of the substrate is preferably 15 to 300 μm, more preferably 20 to 200 μm. By keeping the thickness of the substrate within the above range, the flexibility of the protective film forming sheet and its adhesion to semiconductor wafers or semiconductor chips are further improved.

[0290] The substrate can consist of one layer (single layer) or multiple layers (two or more layers). When the substrate consists of multiple layers, these multiple layers can be the same as each other or different from each other, and there are no particular restrictions on the combination of these multiple layers.

[0291] In addition, when the substrate is composed of multiple layers, the total thickness of each layer can be set to the preferred substrate thickness described above.

[0292] To improve the adhesion between the substrate and other layers such as adhesive layers, protective films, and coating layers disposed on the substrate, the surface can be subjected to oxidation treatments such as sandblasting, solvent treatment, embossing, corona discharge treatment, electron beam irradiation treatment, plasma treatment, ozone-ultraviolet irradiation treatment, flame treatment, chromic acid treatment, and hot air treatment. Furthermore, a primer can be applied to the surface of the substrate.

[0293] ·Adhesive layer In this embodiment, the adhesive layer constituting the above-mentioned support sheet may appropriately use a known adhesive layer.

[0294] The adhesive layer can be formed from an adhesive composition containing various components such as adhesives. The content ratio of components in the adhesive composition that do not vaporize at room temperature is generally the same as the content ratio of the aforementioned components in the adhesive layer. Here, "room temperature" is as described above.

[0295] The thickness of the adhesive layer can be appropriately selected according to the purpose, but it is preferably 1 to 100 μm, more preferably 2 to 80 μm, and even more preferably 3 to 50 μm.

[0296] The adhesive layer can consist of one layer (single layer) or multiple layers (two or more layers). When the adhesive layer consists of multiple layers, these multiple layers can be the same as each other or different from each other, and there is no particular limitation on the combination of these multiple layers.

[0297] When the adhesive layer consists of multiple layers, the total thickness of each layer can be set to the preferred adhesive layer thickness described above.

[0298] Examples of adhesives mentioned above include acrylic resins, urethane resins, rubber resins, silicone resins, and vinyl ether resins. When considering the function of such resins, examples include energy-curable resins.

[0299] Here, "energy rays" and "energy ray solidification" are as described above.

[0300] Examples of energy-curable resins include those having polymerizable groups such as (meth)acryloyl and vinyl groups.

[0301] The adhesive resin is preferably an acrylic resin, and more preferably a (meth)acrylate copolymer containing structural units derived from (meth)acrylates.

[0302] When the aforementioned adhesive layer contains components such as energy-curable resins that are polymerized by irradiation with energy rays, it becomes an energy-curable adhesive layer. Irradiation with energy rays reduces its adhesiveness, thereby facilitating the pickup of the semiconductor chip with a protective film, as described later. The aforementioned adhesive layer can, for example, be formed from various adhesive compositions containing components that are polymerized by irradiation with energy rays.

[0303] <<Adhesive Compositions>> As a preferred example of the above-mentioned adhesive composition, an adhesive composition containing an ingredient that is polymerized by irradiation with energy rays can be listed. Examples of such adhesive compositions include, for example, an adhesive composition containing an acrylic resin and an energy-ray polymerizable compound (hereinafter, sometimes abbreviated as "adhesive composition (i)"); an adhesive composition containing the above-mentioned acrylic resin having hydroxyl groups and polymerizable groups on the side chain (e.g., an acrylic resin having hydroxyl groups and polymerizable groups on the side chain via urethane bonds) and an isocyanate crosslinking agent (hereinafter, sometimes abbreviated as "adhesive composition (ii)").

[0304] [Adhesive composition (i)] The adhesive composition (i) contains the above-mentioned acrylic resin and energy-ray polymerizable compound as essential components. The following is a description of each component.

[0305] (Acrylic resins) As a preferred example of the acrylic resin in the adhesive composition (i), for example, a (meth)acrylate copolymer obtained by polymerizing (meth)acrylate as a monomer and monomers other than (meth)acrylate used as needed.

[0306] Examples of the aforementioned (meth)acrylates include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate (also known as (meth)acrylate). Laurethyl ester, tridecyl methacrylate, tetradecyl methacrylate (myristyl methacrylate), pentadecyl methacrylate, hexadecyl methacrylate (also known as palmitate methacrylate), heptadecanyl methacrylate, octadecyl methacrylate (also known as stearate methacrylate), isooctadecyl methacrylate (also known as isostearate methacrylate), etc., and alkyl methacrylates in which the alkyl group is a chain structure with 1 to 18 carbon atoms. Isoborneol ester (meth)acrylate, dicyclopentyl ester (meth)acrylate, and other cycloalkyl esters of (meth)acrylate; (Meth)benzyl acrylate and other (meth)acrylate aralkyl esters; (Meth)acrylate dicyclopentenyl ester and other (meth)acrylate cycloalkenyl esters; (Meth)acrylate dicyclopentenyloxyethyl ester and other (meth)acrylate cyclopentenyloxyalkyl esters; (meth)acrylimide; (Meth)acrylates containing glycidyl groups, such as glycidyl acrylate; Hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl methacrylate, and other hydroxyl-containing methacrylates.

[0307] Among them, methyl methacrylate, 2-ethylhexyl acrylate, and 2-hydroxyethyl acrylate are preferred.

[0308] Other monomers besides (meth)acrylates mentioned above include (meth)acrylic acid, itaconic acid, vinyl acetate, acrylonitrile, styrene, N-hydroxymethylacrylamide, etc.

[0309] The various monomers constituting acrylic resins, such as the (meth)acrylates and monomers other than (meth)acrylates, may be only one type or two or more types.

[0310] The adhesive composition (i) may contain only one type of acrylic resin or two or more types.

[0311] The content of acrylic resin in the adhesive composition (i) is preferably 40 to 99% by mass, more preferably 50 to 91% by mass, relative to the total mass of all components except the solvent in the adhesive composition (i).

[0312] (A polymerizable compound due to energy rays) The energy-ray polymerizable compound in the adhesive composition (i) is a compound that is polymerized and cured by irradiation with energy rays. Examples of such compounds include those having energy-ray polymerizable groups such as energy-ray curable double bonds within the molecule.

[0313] Examples of energy-ray polymerizable compounds include, for instance, low molecular weight compounds (monomers and oligomers with monofunctional or polyfunctional groups), such as those possessing energy-ray polymerizable groups. More specifically, examples include trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, and 1,6- Hexanediol di(meth)acrylate and other (meth)acrylates; Dicyclopentadiene dimethoxydi(meth)acrylate and other (meth)acrylates containing a cyclic aliphatic backbone; Polyethylene glycol di(meth)acrylate, low polyester (meth)acrylate, urethane (meth)acrylate oligomers, epoxy-modified (meth)acrylate, polyether (meth)acrylate, itaconic acid oligomers, and other (meth)acrylate compounds.

[0314] The molecular weight of the above-mentioned energy-ray polymerizable compound is preferably 100 to 30,000, more preferably 300 to 10,000.

[0315] The adhesive composition (i) may contain only one or more energy-emitting polymerizable compounds.

[0316] Relative to the content of the above-mentioned acrylic resin in 100 parts by mass, the content of the energy-ray polymerizable compound in the adhesive composition (i) is preferably 1 to 125 parts by mass, more preferably 10 to 125 parts by mass.

[0317] (Photopolymerization initiator) In addition to the aforementioned acrylic resins and energy-ray polymerizable compounds, the adhesive composition (i) may contain a photopolymerization initiator.

[0318] The aforementioned photopolymerization initiator can be a known photopolymerization initiator. Specifically, examples include 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)one, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxyphenylacetone, 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propanoyl)-benzyl]phenyl}-2-methyl-propane-1-one and other α-keto alcohol compounds. Acetophenone, dimethylaminoacetophenone, methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, and other acetophenone compounds; Benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, anisonitrile methyl ether, and other benzoin ether compounds; Ketals such as benzyl dimethyl ketal and acetophenone dimethyl ketal; Aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; Photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(O-ethoxycarbonyl)oxime and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]acetophenone 1-(O-acetyloxime); Benzophenone, p-phenylbenzophenone, benzoylbenzoic acid, dichlorobenzophenone, 4,4'-diethylaminobenzophenone, 3,3'-dimethyl-4-methoxybenzophenone and other benzophenone compounds; Anthraquinone compounds such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, and 2-aminoanthraquinone; Thioxanone, 2-chlorothioxanone, 2-methylthioxanone, 2-ethylthioxanone, isopropylthioxanone, 2,4-dimethylthioxanone, 2,4-diethylthioxanone, 2,4-dichlorothioxanone, 2,4-diisopropylthioxanone and other thioxanone compounds; p-Dimethylaminobenzoate; camphorquinone; halogenated ketones; acylphosphine oxides such as diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide; acylphosphonate; oligomeric [2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]acetone], etc.

[0319] The photopolymerization initiator contained in the adhesive composition (i) may be only one type or two or more types.

[0320] When using a photopolymerization initiator, the content of the photopolymerization initiator in the adhesive composition (i) is preferably 0.1 to 10 parts by mass, more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the aforementioned energy-ray polymerizable compound. By setting the aforementioned content of the photopolymerization initiator to the lower limit or above, the effects brought about by using the photopolymerization initiator can be sufficiently obtained. Furthermore, by setting the aforementioned content of the photopolymerization initiator to the upper limit or below, the generation of byproducts from excessive photopolymerization initiator can be suppressed, resulting in better curing of the adhesive layer.

[0321] (Cross-linking agent) In addition to the aforementioned acrylic resins and energy-ray polymerizable compounds, the adhesive composition (i) may further contain a crosslinking agent.

[0322] Examples of crosslinking agents include organic polyisocyanate compounds and organic polyimide compounds.

[0323] Examples of the aforementioned organic polyisocyanate compounds include, for instance, aromatic polyisocyanate compounds, aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds, and their trimers, isocyanurates, and adducts, or terminal isocyanate carbamate prepolymers obtained by reacting the aforementioned aromatic, aliphatic, or alicyclic polyisocyanate compounds with polyol compounds. The aforementioned adducts refer to the reaction products of the aforementioned aromatic, aliphatic, or alicyclic polyisocyanate compounds with low-molecular-weight compounds containing active hydrogen, such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, or castor oil.

[0324] More specifically, examples of the aforementioned organic polyisocyanate compounds include 2,4- Compounds obtained by adding toluene diisocyanate; 2,6-toluene diisocyanate; 1,3-phenylenedimethylene diisocyanate; 1,4-xylene diisocyanate; diphenylmethane-4,4'-diisocyanate; diphenylmethane-2,4'-diisocyanate; 3-methyldiphenylmethane diisocyanate; hexamethylene diisocyanate; isophorone diisocyanate; dicyclohexylmethane-4,4'-diisocyanate; dicyclohexylmethane-2,4'-diisocyanate; compounds obtained by adding all or part of the hydroxyl groups of polyols such as trimethylolpropane to toluene diisocyanate and hexamethylene diisocyanate, or any one or two of them; lysine diisocyanate, etc.

[0325] Examples of the aforementioned organic polyimide compounds include N,N'-diphenylmethane-4,4'-bis(1-aziridinylcarboxamide), trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, and N,N'-toluene-2,4-bis(1-aziridinylcarboxamide)triethylene melamine.

[0326] When using isocyanate compounds as crosslinking agents, hydroxyl-containing polymers are preferred as acrylic resins. When the crosslinking agent has isocyanate groups and the acrylic resin has hydroxyl groups, a crosslinked structure can be easily introduced into the adhesive layer through the reaction of these isocyanate groups with the hydroxyl groups. The adhesive composition (i) may contain only one type of crosslinking agent or two or more types.

[0327] When using a crosslinking agent, the content of the crosslinking agent in the adhesive composition (i) is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 16 parts by mass, relative to 100 parts by mass of the above-mentioned acrylic resin.

[0328] (solvent) In addition to the aforementioned acrylic resins and energy-ray polymerizable compounds, the adhesive composition (i) preferably further contains a solvent.

[0329] The solvents mentioned above are not particularly limited. Preferred examples include hydrocarbons such as toluene and xylene; alcohols such as methanol, ethanol, 2-propanol, isobutanol (also known as 2-methylpropane-1-ol), and 1-butanol; esters such as vinyl acetate; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; and amides such as dimethylformamide and N-methylpyrrolidone (i.e., compounds having amide bonds). The adhesive composition (i) may contain only one solvent or two or more solvents.

[0330] When the adhesive composition (i) contains a solvent, the solvent content is preferably 40 to 90% by mass, more preferably 50 to 80% by mass, relative to the total mass of the adhesive composition.

[0331] (Other ingredients) In addition to the aforementioned acrylic resins and energy-ray polymerizable compounds, the adhesive composition (i) may further contain other components that are not among the aforementioned photopolymerization initiators, crosslinking agents, and solvents, without impairing the effects of the present invention.

[0332] The other components mentioned above can be well-known components and can be selected arbitrarily according to the purpose without particular limitation. As preferred examples, various additives such as colorants (dyes, pigments), anti-deterioration agents, antistatic agents, flame retardants, organosilicon compounds, and chain transfer agents can be listed. The adhesive composition (i) may contain only one or more of the other components mentioned above.

[0333] [Adhesive Composition (ii)] The adhesive composition (ii) contains an acrylic resin having hydroxyl groups and polymerizable groups on its side chains (e.g., an acrylic resin having hydroxyl groups and polymerizable groups on its side chains via urethane bonds) and an isocyanate crosslinking agent as essential components.

[0334] When using adhesive composition (ii), because acrylic resins have polymerizable groups on their side chains, compared to adhesive composition (i) which uses energy-ray polymerizable compounds and causes polymerization by irradiation with energy rays, the peelability of the adhesive layer decreases after polymerization (curing), resulting in increased peelability when peeling it from the adhered object, and thus increased pick-up of semiconductor chips with protective films.

[0335] In addition, unless otherwise specified in this specification, the term "acrylic resin" in adhesive composition (ii) refers to "acrylic resin having polymerizable groups on its side chains".

[0336] (Acrylic resins) As an example of an acrylic resin having polymerizable groups on its side chain, the following acrylic resin can be cited: an acrylic resin obtained by copolymerizing a non-hydroxyl-containing (meth)acrylate monomer with a hydroxyl-containing (meth)acrylate or other hydroxyl-containing compound, and reacting the hydroxyl groups of the resulting hydroxyl-containing copolymer with the isocyanate groups of a compound having isocyanate groups and polymerizable groups to form urethane bonds.

[0337] As an example of the above-mentioned hydroxyl-free (meth)acrylate, other than hydroxyl-containing (meth)acrylates can be listed as (meth)acrylates in the adhesive composition (i).

[0338] Furthermore, examples of the hydroxyl-containing compounds mentioned above include the same hydroxyl-containing (meth)acrylate as the hydroxyl-containing compound in the adhesive composition (i).

[0339] The non-hydroxyl-containing (meth)acrylate and the hydroxyl-containing compound constituting the above-mentioned acrylic resin may be only one type or two or more types.

[0340] Examples of compounds having isocyanate groups and polymerizable groups include 2- Methacryloxyethyl isocyanate and other isocyanate-containing (meth)acrylates.

[0341] The compounds constituting the above-mentioned acrylic resins, which have isocyanate groups and polymerizable groups, may be only one type or two or more types.

[0342] The adhesive composition (ii) may contain only one type of acrylic resin or two or more types.

[0343] The content of acrylic resin in adhesive composition (ii) is preferably 80 to 99% by mass, more preferably 90 to 97% by mass, relative to the total mass of all components except solvent in adhesive composition (ii).

[0344] (Isocyanate crosslinking agents) As the aforementioned isocyanate crosslinking agent, examples include isocyanate crosslinking agents that are the same as the aforementioned organic polyisocyanate compounds used as crosslinking agents in adhesive composition (i). The adhesive composition (ii) may contain only one type of isocyanate crosslinking agent or two or more types.

[0345] Preferably, the molar number of isocyanate groups in the isocyanate crosslinking agent in adhesive composition (ii) is 0.2 to 3 times the molar number of hydroxyl groups in the acrylic resin in adhesive composition (ii). By setting the molar number of isocyanate groups to the lower limit or above, the peelability when peeling from the adhered object, which is caused by a decrease in the adhesiveness of the cured adhesive layer, is increased, and the pick-up performance of the semiconductor chip with the protective film is improved. Furthermore, by setting the molar number of isocyanate groups to the upper limit or below, the generation of byproducts caused by the reaction between isocyanate crosslinking agents can be further suppressed.

[0346] The content of the isocyanate crosslinking agent in the adhesive composition (ii) can be appropriately adjusted in such a way that the molar number of isocyanate groups is within the above-mentioned range. However, it is preferable that, based on satisfying this condition, the content of the isocyanate crosslinking agent in the adhesive composition (ii) is 0.01 to 20 parts by mass relative to 100 parts by mass of acrylic resin, more preferably 0.1 to 15 parts by mass, and particularly preferably 0.3 to 12 parts by mass.

[0347] (Photopolymerization initiator) In addition to the acrylic resins and isocyanate crosslinking agents mentioned above, the adhesive composition (ii) may contain a photopolymerization initiator.

[0348] As the aforementioned photopolymerization initiator, examples include photopolymerization initiators identical to those in adhesive composition (i). Adhesive composition (ii) may contain only one or more photopolymerization initiators.

[0349] When using a photopolymerization initiator, the content of the photopolymerization initiator in the adhesive composition (ii) is preferably 0.05 to 20 parts by weight relative to 100 parts by weight of acrylic resin.

[0350] By setting the content of the photopolymerization initiator to the lower limit or above, the effects of using the photopolymerization initiator can be fully obtained. Furthermore, by setting the content of the photopolymerization initiator to the upper limit or below, the generation of byproducts caused by excessive photopolymerization initiator can be suppressed, resulting in better curing of the adhesive layer.

[0351] (solvent) In addition to the acrylic resins and isocyanate crosslinking agents mentioned above, the adhesive composition (ii) preferably further contains a solvent.

[0352] As the solvents described above, examples include solvents identical to those in adhesive composition (i). Adhesive composition (ii) may contain only one solvent or two or more solvents.

[0353] When the adhesive composition (ii) contains a solvent, the solvent content is preferably 40 to 90% by mass, more preferably 50 to 80% by mass, relative to the total mass of the adhesive composition (ii).

[0354] (Other ingredients) In addition to the acrylic resins and isocyanate crosslinking agents mentioned above, the adhesive composition (ii) may contain other components that are not part of the above-mentioned photopolymerization initiators and solvents, without impairing the effects of the present invention.

[0355] Other components mentioned above may include, for example, components identical to those in adhesive composition (i). Adhesive composition (ii) may contain only one or more of the aforementioned other components.

[0356] Thus far, an adhesive composition containing components that polymerize by irradiation with energy rays has been described. However, for the formation of the adhesive layer, an adhesive composition not containing components that polymerize by irradiation with energy rays can also be used. That is, the adhesive layer can be a non-energy-ray-curable adhesive layer that does not have energy-ray curing properties.

[0357] As a preferred example of the above-mentioned non-energy-curable adhesive composition, examples include adhesive compositions containing acrylic resins and crosslinking agents (hereinafter, sometimes abbreviated as "adhesive composition (iii)"), which may contain any components such as solvents and other components that are not solvents.

[0358] [Adhesive composition (iii)] The acrylic resin, crosslinking agent, solvent and other components contained in adhesive composition (iii) are the same as those in adhesive composition (i).

[0359] The content of acrylic resin in adhesive composition (iii) is preferably 40 to 99% by mass, more preferably 50 to 97% by mass, relative to the total mass of all components except solvent in adhesive composition (iii).

[0360] The crosslinking agent content of the adhesive composition (iii) is preferably 2 to 30 parts by mass, more preferably 4 to 25 parts by mass, relative to 100 parts by mass of acrylic resin.

[0361] Apart from the points mentioned above, adhesive composition (iii) is the same as adhesive composition (i).

[0362] <<Preparation Method of Adhesive Composition>> The adhesive compositions (i) to (iii) are obtained by mixing the adhesive with other components, such as those added as needed, to form the adhesive composition.

[0363] There is no particular restriction on the order of addition when mixing the ingredients, and two or more ingredients can be added at the same time.

[0364] There are no particular limitations on the method of mixing the components during blending; any appropriate method may be selected from the following known methods: mixing by rotating a stir bar or stirring blade; mixing by using a mixer; mixing by applying ultrasound, etc.

[0365] As long as the individual blended components do not deteriorate, there are no particular limitations on the temperature and time when adding and mixing the components; they can be adjusted appropriately. However, the preferred temperature is 15℃ to 30℃.

[0366] ○ Peel-off film Examples of release films include known release films with a release treatment surface used in this field. As for the release treatment of the aforementioned release treatment surface, various release agents such as alkyd, silicone, fluorinated, unsaturated polyester, polyolefin, or wax can be used. Regarding heat resistance, alkyd, silicone, or fluorinated release agents are preferred.

[0367] The thickness of the release film is not particularly limited, but is preferably 20–85 μm, more preferably 25–75 μm. By making the thickness of the release film above the lower limit, it is easier to peel off the release film in the target stage, and after the protective film forming sheet is wound into a roll, curl marks are less likely to form on the release film. On the other hand, by making the thickness of the release film below the upper limit, the effect of suppressing the peeling of the release film in stages other than the target stage is further enhanced.

[0368] <Manufacturing Method of Protective Film Forming Sheet> The protective film forming sheet of this embodiment can be manufactured by a manufacturing method including the following steps: a step of forming a laminated structure of the support sheet and the protective film forming sheet (hereinafter, sometimes referred to as "laminarization step (P1)"); and a step of forming a laminated structure of the protective film forming sheet and the release film (hereinafter, sometimes referred to as "laminarization step (P2)").

[0369] When the support sheet consists of multiple layers, the support sheet can be manufactured simply by stacking these multiple layers.

[0370] When manufacturing a support sheet formed by laminating other layers (e.g., adhesive layer, intermediate layer, coating layer, etc.) onto a substrate, for example, it is sufficient to simply apply a composition containing components for constituting the other layers (e.g., adhesive composition, intermediate layer forming composition, coating layer composition, etc.) to the surface of the substrate and dry it as needed, thereby laminating the other layers onto the substrate. Alternatively, when manufacturing a support sheet formed by laminating other layers onto a substrate, for example, the other layers can be pre-formed on the release material by applying a composition containing components for constituting the other layers to the release treatment surface of the release material and drying it as needed. Then, the other layers are laminated onto the substrate by adhering the surface (exposed surface) of the formed other layers to the surface of the substrate. In this case, the release material only needs to be removed as needed before performing a certain operation on the other layers, such as when laminating a protective film forming film onto the other layers.

[0371] As the aforementioned release material, any release material known in the art can be used, for example, the same release material as the release film constituting the protective film forming sheet of this embodiment can be used.

[0372] For example, a composition capable of being directly coated onto a substrate on which the other layers described above have been laminated on one or two surfaces can be further formed into additional layers. However, in the above-described case, it is preferable to employ a method that adheres the other layers pre-formed on the release material to the substrate or other layers already laminated on the substrate in the manner described above.

[0373] In the above-mentioned lamination process (P1), the laminated structure of the support sheet and the protective film forming film can be formed, for example, by coating the surface of the support sheet with a protective film forming film composition and drying it as needed to form a protective film forming film (hereinafter, this process is sometimes specifically referred to as "Lamination Process (P1)-11").

[0374] In the above-described lamination process (P1), the laminated structure of the support sheet and the protective film forming film can also be formed, for example, by the same method as when manufacturing a support sheet consisting of multiple layers. That is, by coating the release treatment surface of the release material with a protective film forming film composition and drying it as needed, a protective film forming film is pre-formed on the release material. Then, the surface of the formed protective film forming film that is not provided with the release material is bonded to the surface of the support sheet, thereby forming a laminated structure of the support sheet and the protective film forming film (hereinafter, this process is sometimes specifically referred to as "Lamination Process (P1)-12").

[0375] As the release material in this method, any release material known in the art can be used, for example, preferably the same release material as the release film of the protective film forming sheet constituting this embodiment.

[0376] For example, when the support sheet is formed by laminating the other layers on one or two surfaces of a substrate, a protective film forming film can be formed by directly coating the support sheet with a protective film forming film composition. However, in the above case, in the lamination process (P1), it is preferable to use a method that laminates the protective film forming film pre-formed on the release material to the support sheet in the manner described above.

[0377] When the above-described lamination process (P1)-11 is used as the lamination process (P1), in the above-described lamination process (P2), it is only necessary to attach the release film to the surface of the protective film forming film on the side where the support sheet is not provided.

[0378] On the other hand, when the above-mentioned lamination process (P1)-12 is used as the lamination process (P1), in the above-mentioned lamination process (P2), it is only necessary to remove the release material provided on the surface of the protective film forming film opposite to the side where the support sheet is provided, so that one surface of the protective film forming film is exposed, and then the release film is attached to the exposed surface of the protective film forming film.

[0379] Furthermore, when the above-described lamination process (P1)-12 is used as lamination process (P1), by using the above-described release film (the release film constituting the protective film forming sheet of this embodiment) as the release material for pre-forming the protective film forming film, this lamination process (P1)-12 can also serve as the above-described lamination process (P2). It can be said that this manufacturing method is a preferred method in terms of simplifying the manufacturing process. Hereinafter, the process of forming the laminated structure of the support sheet and the protective film forming film in this manufacturing method will sometimes be specifically referred to as "lamination process (P1')".

[0380] For example, such as Figure 7 As shown, when manufacturing a protective film forming sheet viewed from below the peel film side, if the surface area of ​​the protective film forming sheet is smaller than that of the adhesive layer, in the above manufacturing method, it is only necessary to provide a protective film forming sheet pre-cut to a specified size and shape on the adhesive layer.

[0381] When manufacturing the protective film forming sheet of this embodiment, as described above, the protective film forming film can be formed by coating the protective film forming film composition on the surface to which the protective film forming film is to be formed.

[0382] When manufacturing the protective film forming sheet of this embodiment, for example, the adhesive layer can be formed by coating the adhesive composition described above onto the surface to which the adhesive layer is to be formed, and preferably by drying it. The adhesive composition can be applied using the same method as when coating the film composition for forming the protective film.

[0383] The applied adhesive composition can be crosslinked by heating, and this heat-based crosslinking can be carried out simultaneously with drying. Heating conditions can be set, for example, at 100–130°C for 1–5 minutes, but are not limited thereto.

[0384] The following is an example of a protective film forming sheet according to this embodiment. Figure 9 , for as Figure 2 The manufacturing method for forming the protective film shown herein, including the aforementioned lamination process (P1'), will be described. Furthermore, the manufacturing method described here is merely an example; when… Figure 2 When other manufacturing methods for protective film forming sheets with the configuration shown or other manufacturing methods for protective film forming sheets have the same or similar processes as those described below, those processes may also be performed in the same manner as those described below.

[0385] In this method, a thermosetting protective film forming composition or an energy-curable protective film forming composition is coated onto the peeling treatment surface 15b of the peeling film 15, such as... Figure 9As shown in (a), a protective film forming film 13 is formed. Furthermore, for ease of comparison with the protective film forming sheet 1B, an example is shown where the protective film forming film 13 is positioned below the release film 15, but this does not mean that the orientation of the release treatment surface 15b of the release film 15 is limited as shown in the image. Figure 9 The downward direction shown in (a) can also be the opposite, facing upward, but facing upward is preferred.

[0386] Furthermore, a release material (not shown) can be additionally adhered to the surface (exposed surface) of the protective film forming film 13 opposite to the side that contacts the release film 15. Here, the same release material as the release material to which the adhesive composition is coated described later can be listed.

[0387] Then, in this method, as Figure 9 As shown in (b), an adhesive composition is applied to the peel treatment surface 90b of the peeling material 90 to form an adhesive layer 12. Here, for ease of comparison with the protective film forming sheet 1B, an example is shown where the adhesive layer 12 is positioned below the peeling material 90, but this does not mean that the orientation of the peel treatment surface 90b of the peeling material 90 is limited when the adhesive composition is applied. Figure 9 The downward direction shown in (b) can also be the opposite, facing upward, but facing upward is preferred.

[0388] Then, in this method, as Figure 9 As shown in (c), the substrate 11 is bonded to the surface (exposed surface) opposite to the side of the adhesive layer 12 that is in contact with the release material 90. At this time, the bonding surface of the adhesive layer 12 is selected from the substrate 11 in such a way that the surface roughness of the surface 11b of the side of the substrate 11 where the adhesive layer 12 is not bonded is 0.5 μm or less. Thus, support sheet 10 is obtained.

[0389] Then, in this method, as Figure 9 As shown in (d), the exposed surface of the adhesive layer 12, which is exposed by removing the release material 90 from the adhesive layer 12 of the support sheet 10, is bonded to the exposed surface of the protective film forming film 13, thereby achieving the desired effect. Figure 9 As shown in (e), a protective film forming sheet 1B is obtained. When additionally attaching the aforementioned release material to the surface (exposed surface) of the protective film forming film 13 opposite to the side that contacts the release film 15, it is only necessary to attach the exposed surface of the protective film forming film 13 to the exposed surface of the adhesive layer 12 after removing the release material.

[0390] Next, the protective film forming sheet of this embodiment is... Figure 1The manufacturing method of the protective film forming sheet shown will be explained (illustrations omitted).

[0391] In this method, the manufacturing method of the protective film forming sheet 1B described above can be used.

[0392] First, a cut is formed on a laminated sheet on one side of the adhesive tape used to form the adhesive layer 16 for the clamp, wherein a release film 15 is laminated, and a cut is formed at a target location on the adhesive tape in such a way that a target shape is formed. Here, the target shape is, for example, a circular shape when viewed from above with the surface of the laminated sheet viewed from below.

[0393] Then, the adhesive tape of the target shape (e.g., circular in plan view) is removed from the laminate, resulting in a processed laminate in which the release material is exposed in the area where the adhesive tape has been removed. That is, in the case where the adhesive tape that is circular in plan view has been removed, the processed laminate is a laminate in which the adhesive tape has been completely removed at the target location.

[0394] Then, the release film 15 is removed from the protective film forming sheet 1B obtained above, and the exposed surface of the protective film forming film 13 is bonded to the adhesive tape of the processed laminated sheet, thereby obtaining... Figure 1 The protective film forming sheet 1A is shown. In this method, when the protective film forming sheet 1B is not used as a roll-shaped protective film forming sheet, the same protective film forming sheet as the protective film forming sheet 1B can be used as the bonding object of the above-mentioned processed laminated sheet, except that it has a known release material other than the release film 15 to replace the release film 15.

[0395] However, the above manufacturing method is only an example, and the manufacturing method of the protective film forming sheet 1A is not limited to this.

[0396] <Instructions for using protective film forming sheets> The method of using the protective film forming sheet in this embodiment is as follows, for example.

[0397] First, the method of using the protective film forming sheet when the protective film is thermosetting will be explained.

[0398] When the protective film forming film is thermosetting, firstly, the back side of the semiconductor wafer is attached to the protective film forming sheet, and at the same time, the protective film forming sheet is fixed on the dicing device.

[0399] Then, the protective film is cured by heating, thereby forming the protective film. When a backing tape is attached to the surface (electrode forming surface) of a semiconductor wafer, the protective film is usually formed after the backing tape is removed from the semiconductor wafer.

[0400] Then, the semiconductor wafer and the protective film are cut together to form a semiconductor chip. During the period from the formation of the protective film to the cutting, a laser can be irradiated onto the protective film from the support side of the protective film forming sheet to print text on the surface of the protective film (laser printing).

[0401] Then, the semiconductor chip with a protective film is obtained by peeling it off from the support sheet along with the cut protective film attached to its back side. For example, when the support sheet is a sheet with a substrate and an adhesive layer stacked together, and the adhesive layer is an energy-curable layer, the semiconductor chip with a protective film can be more easily obtained by curing the adhesive layer with energy rays and picking it off from the cured adhesive layer along with the protective film attached to its back side.

[0402] The semiconductor chips with protective films are picked up one by one and transported to the next process.

[0403] Then, the semiconductor chip with the protective film is mounted in the reflow process. For example, the obtained semiconductor chip with the protective film can be mounted by flip-chip bonding to the circuit surface of the substrate. Then, the entire assembly is sealed with resin to form a semiconductor package. Then, the target semiconductor device can be manufactured using this semiconductor package.

[0404] Furthermore, this section has described the case where the protective film is formed by curing the protective film and then dicing it. However, it is also possible to dicing without curing the protective film and then cure the protective film after dicing to form a protective film. Additionally, laser printing can be performed on the uncured protective film. By laser printing on the protective film and then curing it, a semiconductor wafer with a laser-printed protective film is obtained.

[0405] Next, the method of using the protective film forming sheet when the protective film is curable by energy rays will be explained.

[0406] When the protective film forming film is energy-curable, the process is the same as when the protective film forming film is thermosetting. The back side of the semiconductor wafer is attached to the protective film forming sheet, and the protective film forming sheet is fixed on the cutting device at the same time.

[0407] Then, the protective film is solidified by irradiating it with energy rays, thereby producing the protective film. When a backing tape is applied to the surface (electrode forming surface) of a semiconductor wafer, a protective film is typically formed after the backing tape is removed from the semiconductor wafer.

[0408] Then, the semiconductor wafer and the protective film are diced together to form a semiconductor chip. During the period from the formation of the protective film to the dicing, a laser can be irradiated onto the protective film from the support side of the protective film forming sheet to imprint text on the surface of the protective film.

[0409] Then, the semiconductor chip and the cut protective film attached to its back are peeled off from the support sheet and picked up, thus obtaining a semiconductor chip with a protective film.

[0410] This method is particularly suitable for, for example, the use of a support sheet formed from a laminated substrate and an adhesive layer, wherein the adhesive layer is a protective film forming sheet other than an energy-curable adhesive layer.

[0411] For example, when using a support sheet that is a protective film formed from a laminated substrate and an adhesive layer, wherein the adhesive layer is an energy-curable adhesive layer, the method described below is preferred.

[0412] That is, firstly, in the same manner as described above, the back side of the semiconductor wafer is attached to the protective film forming sheet of the protective film forming sheet, and at the same time, the protective film forming sheet is fixed on the dicing device.

[0413] Then, as needed, a laser is irradiated onto the protective film forming film from the support sheet side to imprint text on the surface of the protective film forming film. Then, the semiconductor wafer is cut to produce a semiconductor chip.

[0414] Then, the protective film is cured by irradiating it with energy rays, thereby forming a protective film. At the same time, the adhesive layer is cured. The semiconductor chip and the protective film attached to its back are picked up from the cured adhesive layer, thus obtaining a semiconductor chip with a protective film. The printing applied to the surface of the protective film is also maintained in the same state in the protective film.

[0415] The subsequent processes are the same as when the protective film used for forming the film is thermosetting.

[0416] Furthermore, the method described here is the same as when the protective film forming film is thermosetting, but modifications can be made. That is, the case of cutting after curing the protective film forming film to form a protective film has been described so far, but it is also possible to cut without curing the protective film forming film, and then cure the protective film forming film after the cut to form a protective film. Example

[0417] The present invention will now be described in more detail through specific embodiments. However, the present invention is not limited to the embodiments shown below.

[0418] The following are the raw materials used to prepare the film composition for forming a protective film.

[0419] [Polymer component (A)] (A)-1: Acrylic polymer: An acrylic polymer copolymer composed of 15 parts by mass of n-butyl acrylate, 10 parts by mass of methyl methacrylate, 60 parts by mass of methyl acrylate and 15 parts by mass of 2-hydroxyethyl acrylate (weight average molecular weight: 600,000, glass transition temperature: 1℃).

[0420] [Thermosetting component (B)] ·Epoxy resin (B1) (B1)-1: Bisphenol A type liquid epoxy resin (manufactured by NIPPON SHOKUBAI CO., LTD, BPA328, epoxy equivalent of 230) (B1)-2: Bisphenol A type epoxy resin ("jER1055" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent of 800-900) (B1)-3: Bisphenol F type liquid epoxy resin ("jERYL983U" manufactured by Mitsubishi Chemical Corporation, with an epoxy equivalent of 165-175)

[0421] • Thermosetting agent (B2) (B2)-1: Dicyandiamide (thermally active latent epoxy resin curing agent, "ADEKAHARDNER EH-3636AS" manufactured by ADEKACORPORATION)

[0422] [Curing Accelerator (C)] (C)-1: 2-Phenylon-4,5-Dihydroxymethylimidazol (“CUREZOL 2PHZ” manufactured by SHIKOKU CHEMICALS CORPORATION)

[0423] [Filling Material (D)] (D)-1: Silica filler (ADMATECHS Co., Ltd. SC105G-MMQ: Spherical silica, average 0.3μm)

[0424] [Coupled agent (E)] (E)-1: 3-Epoxypropoxypropyltrimethoxysilane (3-Glycidyl etheroxypropyltrimethoxysilane) (manufactured by Shin-Etsu Chemical Co., Ltd., KBM403)

[0425] [Coloring agent (I)] (I)-1: Carbon black (MA600B manufactured by Mitsubishi Chemical Corporation, with an average particle size of 28 nm)

[0426] The support sheet and release film used are as follows. The support sheet is a commercially available adhesive tape used as a cutting disc. Substrate: Adwill G-535H (90μm thick) manufactured by Lintec Corporation Release film: SP-PET381130 (38μm thick) manufactured by Lintec Corporation.

[0427] [Example 1] Manufacturing of protective film forming sheets (Preparation of film compositions for thermosetting protective film formation) As shown in Table 1, polymer component (A)-1 (20 parts by mass), epoxy resin (B1)-1 (15 parts by mass), epoxy resin (B1)-2 (1.8 parts by mass), thermosetting agent (B2)-1 (0.45 parts by mass), curing accelerator (C)-1 (0.45 parts by mass), filler (D)-1 (60 parts by mass), coupling agent (E)-1 (0.4 parts by mass), and colorant (I)-1 (1.9 parts by mass) were mixed, and methyl ethyl ketone was further mixed in. The mixture was stirred at 23°C for 60 minutes to obtain a protective film forming film composition (1-1) with a solid content of 52% by mass. Furthermore, the amounts of components other than methyl ethyl ketone shown here and in Table 1 are all solid content amounts.

[0428] (Formation of the protective film) Using a doctor blade coater, the above-obtained protective film forming composition (1-1) is applied to the peeling surface of the release film, and dried at 110°C for 2 minutes to form a protective film forming film with a thickness of 25 μm. Further, the peeling surface of the release film is adhered to the exposed surface of this protective film forming film on the side opposite to the side where the release film is located.

[0429] (Manufacturing of sheets for forming protective films) Remove the release film from one surface of the protective film forming film obtained above, and remove the release film disposed on the adhesive layer of the support sheet. Laminate the exposed surface of the protective film forming film with the exposed surface of the adhesive layer to obtain a protective film forming sheet formed by sequentially stacking the substrate, the adhesive layer, the protective film forming film and the release film.

[0430] (Manufacturing of silicon chips with protective films) The obtained protective film forming sheet is attached to the #2000 polished surface of a 6-inch silicon wafer (100μm thick) via its protective film forming film. The sheet is then fixed on an annular frame and left to stand for 30 minutes. Then, the silicon wafer with the protective film forming film is heat-treated at 130°C for 2 hours to solidify the protective film forming film and form a protective film.

[0431] Then, using a green laser marking machine (CSM300M manufactured by EOTECH), laser marking is performed on the protective film forming film under the following conditions. Wavelength: 532nm Output power: 0.38W Frequency: 20kHz Scanning speed: 100mm / second Printed text: ABCD Text size: 300μm (height) × 200μm (width) Text line width: 35μm

[0432] Then, using a dicing blade, the silicon wafer and protective film are cut together to achieve single-chip processing, resulting in silicon chips with dimensions of 3mm in length and 3mm in width, a protective layer thickness of 25μm, and a Si layer thickness of 350μm. Next, a die bonder ("BESTEM-D02" manufactured by Canon Machinery Inc.) is used to pick up the silicon chips with the protective film, resulting in silicon chips with printed markings on the protective film.

[0433] A silicon chip with a protective film was heat-treated at 260°C for 10.8 minutes, then allowed to return to room temperature. This process was repeated three times. This operation simulates the reflow process performed during the mounting process. The chip before heat treatment is denoted as "before reflow," and the chip after heat treatment is denoted as "after reflow."

[0434] (Color measurement) Before and after the reflow process, for both printed and non-printed areas, the CIE1976L standard was measured using an SE6000 manufactured by Nippon Denshoku Industries Co., Ltd., through reflection from a C / 2 light source. * a * b * Lightness (L) in the color system * chromaticity a * chromaticity b * . Calculate the color difference ΔE between the printed and non-printed areas. * ab and brightness difference ΔL * The results are shown in Table 1.

[0435] (Evaluation of visibility) Before and after the reflow process, the visibility of the printed text was evaluated based on the following criteria. The results are shown in Table 1. • Good: More than 4 out of 5 people can see the printed words. • Qualified: 2 to 3 out of 5 people can see the printed words. • Bad: Less than 1 out of 5 people can see the printed words.

[0436] [Examples 2 and 3, Comparative Example 1] Except for changing the components as shown in Table 1 when preparing the thermosetting protective film forming composition, a protective film forming sheet was manufactured in the same manner as in Example 1 to obtain a silicon chip with a protective film. The evaluation was conducted in the same manner as in Example 1. The results are shown in Table 1.

[0437] [Table 1]

[0438] The results above confirm that the protective film forming film according to this embodiment can achieve sufficient visibility of the printed text even when the line width of the printed text is narrow during the curing of the protective film forming film or the reflow process.

Claims

1. A protective film forming film, wherein laser printing is performed on its surface, wherein, Set the color of the printed area to CIE1976L. Lightness L in the coordinate system of color representation chromaticity a chromaticity b And set the color of the non-printed parts to CIE1976L Lightness L in the coordinate system of color representation chromaticity a chromaticity b hour, The color difference between the printed area and the non-printed area is defined by the following formula (A). Amount 8 or above The colors of the printed and non-printed areas are determined by heating the protective film to 180°C after laser printing to cure it, followed by three further heatings at 260°C for 10.8 minutes each. The printed portion includes a section with a line width of 50μm or less.

2. The protective film forming membrane according to claim 1, wherein, The brightness difference ΔL between the printed and non-printed areas is defined by the following formula (B). Amount 8 or above 。 3. The protective film forming membrane according to claim 1 or 2, wherein, The brightness L of the printed characters The brightness L of the non-printed part satisfy .

4. The protective film forming film according to claim 1 or 2, wherein it contains 1.5% by mass or more carbon black.

5. A protective film forming sheet comprising the protective film forming film and the support sheet as described in any one of claims 1 to 4.

Citation Information

Patent Citations

  • Film for backside of flip-chip type semiconductor, film for backside of dicing tape integrated semiconductor, method of manufacturing semiconductor device, and flip-chip type semiconductor device

    JP2012028396A

  • Adhesive composition, adhesive sheet and method for manufacturing semiconductor device

    JP2013194102A

  • Protection membrane forming film, protection membrane forming utilization sheet, production method and inspection method for workpiece or processed product, workpiece determined as adequate product, and processed product determined as adequate product

    WO2015146936A1

  • Polyacetal resin composition for laser-marking and laser-marked molded article

    JP2001089632A

  • KR20200138157A