A method for designing aggregate gradation for forming cement concrete skeleton

By adding aggregates of different particle sizes step by step to determine the optimal proportion, the problem of ignoring changes in coarse aggregates in traditional design is solved, the mechanical properties and pavement quality of cement concrete are improved, and the economic applicability and Service life.

CN115148314BActive Publication Date: 2024-11-05DALI HUAYUN TONGDA TRANSPORTATION TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210821153.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-13
Publication Date
2024-11-05
Estimated Expiration
2042-07-13

Smart Images

  • Figure CN115148314B_ABST
    Figure CN115148314B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of civil engineering application technology, and discloses an aggregate gradation design method for forming a cement concrete skeleton, comprising the following steps: grading the aggregates according to a preset particle size range, and sorting and numbering them according to the particle size; measuring the tap density after mixing aggregate A and aggregate B, and taking the mixing ratio corresponding to the maximum tap density point as the optimal mixing ratio of aggregate A and aggregate B; and so on, until the optimal mixing ratio of other numbered aggregates except the last numbered one has been determined; measuring the skeleton penetration pressure after mixing the mixed aggregate and the last numbered aggregate, and obtaining the optimal mixing ratio of all numbered aggregates. This scheme obtains the optimal ratio of each grade of aggregates when the aggregate density is the largest and the skeleton uniaxial penetration pressure is the best by blending each grade of aggregates, which is beneficial to improving the comprehensive mechanical properties of cement concrete after molding and improving the economic applicability of cement concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of civil engineering application, and in particular to an aggregate gradation design method for forming a cement concrete skeleton. Background Art

[0002] The mix design of cement concrete is one of the key factors affecting the quality of cement concrete pavement projects. A large number of practices have proved that under the premise of using the same raw materials, if there is a lack of reasonable mix design, cement concrete pavements are prone to various early damage phenomena, including corner fractures, broken plates and other problems, which seriously affect the road quality and service life of the pavement. The traditional mix design of cement concrete pavement is mainly based on the orthogonal design method, which analyzes the effects of four parameters, namely cement dosage, water dosage, sand ratio and admixture, on the slump, compressive strength and flexural strength of cement concrete, and determines the best combination of the four parameters that can meet the slump and strength technical requirements from a large amount of test data, thereby determining the best mix ratio of cement concrete for subsequent large-scale implementation.

[0003] Cement concrete is generally composed of two types of aggregates: coarse aggregate and fine aggregate. Coarse aggregate is used to form the skeleton of cement concrete, and fine aggregate is used to fill the skeleton formed by coarse aggregate, thereby making cement concrete more compact. However, coarse aggregate, as the most used component in cement concrete, has not received sufficient attention in traditional design methods.

[0004] In the process of cement concrete mix design, engineering technicians generally ignore the changes in density, mud content, needle-like shape and gradation of coarse aggregates from different sources, and carry out relevant mix design and test analysis after determining the blending ratio of each grade of coarse aggregate based on previous design experience. However, for coarse aggregates, the changes in density, mud content, needle-like shape and gradation of coarse aggregates often affect their density and mechanical properties as the skeleton of cement concrete, and also greatly affect the workability and strength of cement concrete. Summary of the invention

[0005] The purpose of the present invention is to propose an aggregate gradation design method for forming a cement concrete skeleton. By blending each grade of aggregate, the optimal proportion of each grade of aggregate when the aggregate density is maximum and the uniaxial penetration pressure of the skeleton is optimal is obtained, so as to provide an accurate and reliable coarse aggregate blending ratio before conducting an orthogonal design test of cement concrete mix ratio, which is beneficial to improving the comprehensive mechanical properties of cement concrete after molding and improving the economic applicability of cement concrete, so as to overcome the shortcomings of the prior art.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] A method for designing aggregate gradation for forming a cement concrete skeleton comprises the following steps:

[0008] Determine the particle size of aggregates used to prepare cement concrete; classify the aggregates according to a preset particle size range, and sort and number them from large to small according to the particle size; wherein the aggregate with the largest particle size is numbered A, the aggregate with the second largest particle size is numbered B, the aggregate with the third largest particle size is numbered C, and so on;

[0009] Calculate by mass ratio, mix aggregate A and aggregate B in a preset mixing ratio, and then measure the tap density, draw a tap density-mixing ratio relationship curve, and take the mixing ratio corresponding to the maximum tap density point as the optimal mixing ratio of aggregate A and aggregate B;

[0010] Aggregate A and aggregate B are blended according to the above-mentioned optimal mixing ratio, and the two together form aggregate (A+B); according to the mass ratio, aggregate (A+B) and aggregate C are mixed according to the preset mixing ratio and then the tap density is measured, and a tap density-mixing ratio relationship curve is drawn. The mixing ratio corresponding to the maximum tap density point is taken as the optimal mixing ratio, and the optimal mixing ratio of aggregate A, aggregate B and aggregate C under the optimal mixing ratio of aggregate (A+B) and aggregate C is obtained by conversion; and so on, until the optimal mixing ratios of aggregates with other numbers except the last number have been determined;

[0011] Aggregates with numbers other than the last number are mixed according to the optimal mixing ratio to form a mixed aggregate. The mixed aggregate and the last numbered aggregate are mixed according to the preset mixing ratio calculated by mass ratio, and then the skeleton penetration pressure is measured. A skeleton penetration pressure-mixing ratio relationship curve is drawn, and the mixing ratio corresponding to the maximum point of skeleton penetration pressure is taken as the optimal mixing ratio. The optimal mixing ratio of all numbered aggregates under the optimal mixing ratio of the mixed aggregate and the last numbered aggregate is obtained by conversion.

[0012] Preferably, the number of preset mixing ratios of A aggregate and B aggregate, the preset mixing ratio of (A+B) aggregate and C aggregate, and the preset mixing ratio of the mixed aggregate and the last numbered aggregate are all set to at least 5 groups.

[0013] Preferably, there are 7 groups of preset mixing ratios of aggregate A and aggregate B, which are 2:8, 3:7, 4:6, 5:5, 6:4, 7:3 and 8:2 calculated by mass ratio.

[0014] Preferably, there are five preset mixing ratios of (A+B) aggregate and C aggregate, which are 6:1, 5:1, 4:1, 3:1 and 2:1 calculated by mass ratio.

[0015] Preferably, there are five preset mixing ratios of the mixed aggregate and the last numbered aggregate, which are 6:1, 5:1, 4:1, 3:1 and 2:1 calculated by mass ratio.

[0016] Preferably, the tap density is measured at least three times, and the arithmetic mean of the three tap densities is taken to draw a tap density-mixing ratio relationship curve.

[0017] Preferably, the tap density is measured at least 3 times, and after removing the abnormal values, the arithmetic mean of the remaining tap density is taken to draw a tap density-mixing ratio relationship curve;

[0018] The absolute value of the difference between the abnormal value and the average value of the three tap densities is greater than 1.15 times the first preset difference.

[0019] Preferably, the skeleton penetration pressure is measured at least three times, and the arithmetic mean of the three skeleton penetration pressures is taken to draw a skeleton penetration pressure-mixing ratio relationship curve.

[0020] Preferably, the skeleton penetration pressure is measured at least three times, and after removing the abnormal values, the arithmetic mean of the remaining skeleton penetration pressures is taken to draw a skeleton penetration pressure-mixing ratio relationship curve;

[0021] The absolute value of the difference between the abnormal value and the average value of the three skeleton penetration pressures is greater than 1.15 times the second preset difference.

[0022] The technical solution provided by the embodiments of the present application may have the following beneficial effects:

[0023] This scheme proposes a theory based on the step-by-step blending of the skeleton, with the design goal of achieving the maximum compacted density of the mixture and the optimal mechanical properties of the skeleton. By blending a series of particles from coarse to fine, the optimal proportion of each grade of aggregate when the aggregate compacted density is maximum and the uniaxial penetration pressure of the skeleton is optimal is obtained, which can effectively improve the mechanical properties of cement concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is the relationship curve of the tap density-mixing ratio of the A aggregate and the B aggregate in the embodiments of the present invention and the comparative examples.

[0025] Figure 2 It is the skeleton penetration pressure-mixing ratio relationship curve of (A+B) aggregate and C aggregate in the embodiment of the present invention.

[0026] Figure 3 It is the relationship curve between the tap density and the mixing ratio of the (A+B) aggregate and the C aggregate in the embodiment of the present invention. DETAILED DESCRIPTION

[0027] A method for designing aggregate gradation for forming a cement concrete skeleton comprises the following steps:

[0028] Determine the particle size of aggregates used to prepare cement concrete; classify the aggregates according to a preset particle size range, and sort and number them from large to small according to the particle size; wherein the aggregate with the largest particle size is numbered A, the aggregate with the second largest particle size is numbered B, the aggregate with the third largest particle size is numbered C, and so on;

[0029] Calculate by mass ratio, mix aggregate A and aggregate B in a preset mixing ratio, and then measure the tap density, draw a tap density-mixing ratio relationship curve, and take the mixing ratio corresponding to the maximum tap density point as the optimal mixing ratio of aggregate A and aggregate B;

[0030] Aggregate A and aggregate B are blended according to the above-mentioned optimal mixing ratio, and the two together form aggregate (A+B); according to the mass ratio, aggregate (A+B) and aggregate C are mixed according to the preset mixing ratio and then the tap density is measured, and a tap density-mixing ratio relationship curve is drawn. The mixing ratio corresponding to the maximum tap density point is taken as the optimal mixing ratio, and the optimal mixing ratio of aggregate A, aggregate B and aggregate C under the optimal mixing ratio of aggregate (A+B) and aggregate C is obtained by conversion; and so on, until the optimal mixing ratios of aggregates with other numbers except the last number have been determined;

[0031] Aggregates with numbers other than the last number are mixed according to the optimal mixing ratio to form a mixed aggregate. The mixed aggregate and the last numbered aggregate are mixed according to the preset mixing ratio calculated by mass ratio, and then the skeleton penetration pressure is measured. A skeleton penetration pressure-mixing ratio relationship curve is drawn, and the mixing ratio corresponding to the maximum point of skeleton penetration pressure is taken as the optimal mixing ratio. The optimal mixing ratio of all numbered aggregates under the optimal mixing ratio of the mixed aggregate and the last numbered aggregate is obtained by conversion.

[0032] Since the changes in density, mud content, needle-like shape and gradation of coarse aggregate often affect its density and mechanical properties as a cement concrete skeleton, it also greatly affects the workability and strength of cement concrete. Therefore, before conducting orthogonal design experiments, coarse aggregates of different specifications are reasonably blended to make the skeleton they form more tightly embedded and obtain a skeleton with higher density and better mechanical properties, which is conducive to improving the comprehensive mechanical strength of cement concrete. It can effectively reduce the amount of cement or admixtures under the premise of meeting the same mechanical strength, and improve its economic applicability.

[0033] Therefore, in order to solve the technical problem of rapid and reasonable blending of aggregates of different specifications in cement concrete mix design, this scheme proposes an aggregate gradation design method for forming a cement concrete skeleton. Based on the theory of step-by-step blending of the skeleton, the design goal is to achieve the maximum compacted density of the mixture and the optimal mechanical properties of the skeleton. By blending a series of particles from coarse to fine, the optimal proportion of each grade of aggregate is obtained when the aggregate tap density is maximum and the uniaxial penetration pressure of the skeleton is optimal.

[0034] Specifically, the aggregate gradation design method of this scheme includes the following steps:

[0035] Determine the particle size of aggregate used to prepare cement concrete. In one embodiment of the present solution, crushed stone is used as coarse aggregate to be mixed into cement concrete, so it is necessary to first determine the particle size of the crushed stone used to prepare cement concrete.

[0036] The aggregates are classified into grades according to a preset particle size range, and are sorted and numbered from large to small according to the particle size; among them, the aggregate with the largest particle size is numbered A, the aggregate with the second largest particle size is numbered B, the aggregate with the third largest particle size is numbered C, and so on. In the above embodiment, if it can be known from step A that the particle size of the gravel is 5-25 mm, in one embodiment of the present scheme, the gravel can be screened and graded step by step according to the particle size ranges of 21-25 mm, 10-20 mm and 5-9 mm, and the 21-25 mm gravel is numbered A, the 10-20 mm gravel is numbered B and the 5-9 mm gravel is numbered C; in another embodiment of the present scheme, the 5-25 mm gravel is graded and sold in the particle size ranges of 16-25 mm, 10-20 mm and 5-10 mm, then the design method of the present scheme can also grade and number the 5-25 gravel according to the particle size ranges of 16-25 mm, 10-20 mm and 5-10 mm according to the selling rules, and the 16-25 mm gravel is numbered A, the 10-20 mm gravel is numbered B and the 5-10 mm gravel is numbered C. There is no limitation on the grading rules of aggregates in this scheme, and testers can grade aggregates according to actual conditions and experience.

[0037] According to the mass ratio, the tap density of aggregate A and aggregate B is measured after mixing them in the preset mixing ratio, and the tap density-mixing ratio relationship curve is drawn. The mixing ratio corresponding to the maximum tap density point is taken as the optimal mixing ratio of aggregate A and aggregate B. Then, this scheme measures the tap density of each aggregate in the order of large to small particle size, draws a scatter plot of tap density and preset mixing ratio and performs numerical regression, and selects the mixing ratio corresponding to the point with the maximum tap density as the optimal ratio when aggregate A and aggregate B are used together. In one embodiment of the present scheme, the 5-25 crushed stone will be graded and numbered according to the particle size ranges of 16-25mm, 10-20mm and 5-10mm according to the selling rules, and the 16-25mm crushed stone will be numbered A, the 10-20mm crushed stone will be numbered B and the 5-10mm crushed stone will be numbered C. The test personnel can mix according to the preset mixing ratio such as A aggregate: B aggregate = 3:7, 4:6 or 5:5. The preset mixing ratio of the two grades of aggregate is not limited, and the test personnel can set the mixing ratio according to actual conditions and experience.

[0038] Aggregate A and aggregate B are blended according to the above-mentioned optimal mixing ratio, and the two together form aggregate (A+B); according to the mass ratio, aggregate (A+B) and aggregate C are mixed according to the preset mixing ratio and then the tap density is measured, and the tap density-mixing ratio relationship curve is drawn. The mixing ratio corresponding to the maximum tap density point is taken as the optimal mixing ratio, and the optimal mixing ratio of aggregate A, aggregate B and aggregate C under the optimal mixing ratio of aggregate (A+B) and aggregate C is obtained by conversion. After the optimal mixing ratio of the first two grades with the largest particle size is determined, the first two grades are blended into a new grade of aggregate, recorded as (A+B) aggregate, and then the tap density is measured with aggregate C to obtain the optimal mixing ratio of aggregate (A+B) and aggregate C, and then after conversion, the optimal mixing ratio of aggregate A, aggregate B and aggregate C can be obtained. Similarly, when (A+B) aggregate and C aggregate are mixed according to a preset mixing ratio, the preset mixing ratio of the two grades of aggregate is not limited, and the test personnel can set the mixing ratio according to actual conditions and experience.

[0039] And so on, until the optimal mixing ratio of aggregates with other numbers except the last number has been determined; the aggregate gradation design method in this scheme is based on the skeleton step-by-step mixing theory. First, the maximum compacted density of the mixed aggregate is taken as the design goal, and the optimal mixing ratio of aggregates with other numbers except the last number is obtained. That is, if there are four grades of aggregate, ABCD, the maximum compacted density of the mixed aggregate is taken as the design goal, and the optimal mixing ratio of three grades of aggregate, ABC, is obtained.

[0040] Aggregates with numbers other than the last number are mixed according to the optimal mixing ratio to form a mixed aggregate. The mixed aggregate and the last numbered aggregate are mixed according to the preset mixing ratio calculated by mass ratio, and then the skeleton penetration pressure is measured. A skeleton penetration pressure-mixing ratio relationship curve is drawn, and the mixing ratio corresponding to the maximum point of skeleton penetration pressure is taken as the optimal mixing ratio. The optimal mixing ratio of all numbered aggregates under the optimal mixing ratio of the mixed aggregate and the last numbered aggregate is obtained by conversion.

[0041] The quality of the mechanical properties of the aggregate skeleton is positively correlated with the skeleton tap density, but is affected by factors such as the aggregate needle-like shape (particle shape), the gradation of single-grade aggregate, and the mud content. The mechanical properties of the aggregate skeleton are not optimal when the maximum skeleton tap density is reached. Therefore, in order to make the aggregate gradation design achieve both the maximum tap density and the optimal mechanical properties, this solution adds step F to ensure that the mixing ratio of the aggregate is obtained when the maximum tap density and the optimal mechanical properties are achieved. It should be noted that when the mixed aggregate and the last numbered aggregate are mixed according to the preset mixing ratio, the preset mixing ratio of the two grades of aggregate is not limited, and the test personnel can set the mixing ratio according to actual conditions and experience.

[0042] It should be noted that the method for measuring the tap density in this scheme is a conventional measurement method in the field of highway engineering technology, and the method for measuring the skeleton penetration pressure is also a conventional measurement method in the field of highway engineering technology. Therefore, the specific steps of the two measurement methods are not described in detail here.

[0043] To further illustrate, the number of preset mixing ratios of A aggregate and B aggregate, the preset mixing ratio of (A+B) aggregate and C aggregate, and the preset mixing ratio of the mixed aggregate and the last numbered aggregate are all set to at least 5 groups.

[0044] In one embodiment of the present technical solution, at least 5 groups of mixing ratios are set for two grades of aggregate to measure the compacted density and skeleton penetration pressure, so as to improve the fitting accuracy of the compacted density-mixing ratio relationship curve and the skeleton penetration pressure-mixing ratio relationship curve.

[0045] To further explain, there are 7 groups of preset mixing ratios of A aggregate and B aggregate, which are 2:8, 3:7, 4:6, 5:5, 6:4, 7:3 and 8:2 calculated by mass ratio.

[0046] To further illustrate, there are five preset mixing ratios of (A+B) aggregate and C aggregate, which are 6:1, 5:1, 4:1, 3:1 and 2:1 calculated by mass ratio.

[0047] To further explain, there are five groups of preset mixing ratios of the mixed aggregate and the final numbered aggregate, which are 6:1, 5:1, 4:1, 3:1 and 2:1 calculated by mass ratio.

[0048] To further illustrate, the tap density is measured at least three times, and the arithmetic mean of the three tap densities is taken to draw a tap density-mixing ratio relationship curve.

[0049] In another embodiment of the present technical solution, the tap density is measured at least three times, and the arithmetic mean of the three tap densities is taken to draw the tap density-mixing ratio relationship curve, which is beneficial to further improve the fitting accuracy of the relationship curve and avoid the impact of a single accidental situation on the fitting accuracy of the curve.

[0050] It is further explained that the tap density is measured at least 3 times, and after removing the abnormal values, the arithmetic mean of the remaining tap density is taken to draw a tap density-mixing ratio relationship curve;

[0051] The absolute value of the difference between the abnormal value and the average value of the three tap densities is greater than 1.15 times the first preset difference.

[0052] In a more preferred embodiment of the present technical solution, the tap density is measured at least three times, and after eliminating the outliers, the arithmetic mean of the remaining tap densities is taken to draw a tap density-mixing ratio relationship curve; the absolute value of the difference between the outlier and the average of the three tap densities is greater than 1.15 times the first preset difference.

[0053] For example, the results of three tap density measurements are x, y and z respectively, and the first preset difference is p. If |x-(x+y+z) / 3|≤1.15p, then x is a normal measurement value; if |x-(x+y+z) / 3|>1.15p, then x is an abnormal value. In order to avoid the abnormal tap density measurement value affecting the accuracy of the fitting curve, it needs to be eliminated. It should be noted that the first preset difference p is not limited, and the tester can set the first preset difference p according to actual conditions and experience.

[0054] To further illustrate, the skeleton penetration pressure is measured at least three times, and the arithmetic mean of the three skeleton penetration pressures is taken to draw a skeleton penetration pressure-mixing ratio relationship curve.

[0055] In another embodiment of the present technical solution, the skeleton penetration pressure is measured at least three times, and the arithmetic mean of the three skeleton penetration pressures is taken to draw the skeleton penetration pressure-mixing ratio relationship curve, which is beneficial to further improve the fitting accuracy of the relationship curve and avoid the impact of a one-time accidental situation on the fitting accuracy of the curve.

[0056] It is further explained that the skeleton penetration pressure is measured at least three times, and after eliminating abnormal values, the arithmetic mean of the remaining skeleton penetration pressures is taken to draw a skeleton penetration pressure-mixing ratio relationship curve;

[0057] The absolute value of the difference between the abnormal value and the average value of the three skeleton penetration pressures is greater than 1.15 times the second preset difference.

[0058] In a more preferred embodiment of the present technical solution, the skeleton penetration pressure is measured at least three times. After eliminating the abnormal values, the arithmetic mean of the remaining skeleton penetration pressures is taken to draw a skeleton penetration pressure-mixing ratio relationship curve; the absolute value of the difference between the abnormal value and the average value of the three skeleton penetration pressures is greater than 1.15 times the second preset difference.

[0059] For example, the results of three skeleton penetration pressure measurements are m, n and l respectively, and the first preset difference is q. If |m-(m+n+l) / 3|≤1.15q, then m is a normal measurement value; if |m-(m+n+l) / 3|>1.15q, then m is an abnormal value. In order to avoid the abnormal skeleton penetration pressure measurement value affecting the accuracy of the fitting curve, it needs to be eliminated. It should be noted that the second preset difference q is not limited, and the tester can set the second preset difference q according to actual conditions and experience.

[0060] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, taking a newly built cement concrete pavement project of a high-speed tunnel in Guangdong as an example.

[0061] Comparison Example

[0062] Relying on a new cement concrete pavement project of a highway tunnel in Guangdong, the orthogonal design method was used to optimize the original cement concrete mix ratio. The project used 16-25mm, 10-20mm and 5-10mm crushed stones produced by a stone quarry in Yingde City as coarse aggregates. Based on the orthogonal design method, the cement concrete mix ratio was obtained as follows: cement: sand: 16-25mm crushed stone: 10-20mm crushed stone: 5-10mm crushed stone: water: water reducer = 370:705:480:480:240:145:4.1. The conversion ratio of coarse aggregate alone was obtained as follows: 16-25mm crushed stone: 10-20mm crushed stone: 5-10mm crushed stone = 4:4:2.

[0063] Example

[0064] (1) Determine the particle size of crushed stone used to prepare cement concrete;

[0065] (2) The aggregates are classified into grades according to a preset particle size range, and are sorted and numbered from large to small according to the particle size; wherein 16-25 mm crushed stone is numbered A, 10-20 mm crushed stone is numbered B, and 5-10 mm crushed stone is numbered C;

[0066] (3) According to the mass ratio, the A aggregate and the B aggregate were mixed in the mixing ratio of 2:8, 3:7, 4:6, 5:5, 6:4, 7:3 and 8:2, and the tap density was measured. The results are shown in Table 1 below. The tap density-mixing ratio relationship curve was drawn, as shown in Figure 1 As shown, the mixing ratio corresponding to the maximum point of tap density is taken as the optimal mixing ratio of aggregate A and aggregate B, and the optimal mixing ratio of aggregate A and aggregate B is 1.9, that is, 16-25mm crushed stone: 10-20mm crushed stone = 1.9:1;

[0067] Table 1 The tap density test results of different mixing ratios of aggregate A and aggregate B

[0068]

[0069] (4) Aggregate A and aggregate B were mixed according to the above-mentioned optimal mixing ratio of 1.9:1, and the two together formed (A+B) aggregate; (A+B) aggregate and aggregate C were mixed in mixing ratios of 6:1, 5:1, 4:1, 3:1 and 2:1 according to the mass ratio, and the skeleton penetration pressure was measured. The results are shown in Table 2 below, and the skeleton penetration pressure-mixing ratio relationship curve was drawn, as shown in Figure 2 As shown in the figure, the mixing ratio corresponding to the maximum point of skeleton penetration pressure is taken as the optimal mixing ratio. The optimal mixing ratio of aggregate A, aggregate B and aggregate C under the optimal mixing ratio of (A+B) aggregate and aggregate C is obtained by conversion. The optimal mixing ratio of (A+B) aggregate and aggregate C is 4.3, that is, (A+B) aggregate: aggregate C = 4.3:1. After conversion, aggregate A: aggregate B and aggregate C = 2.82:1.48:1.

[0070] Table 2 Test results of skeleton penetration pressure of different mixing ratios of (A+B) aggregate and C aggregate

[0071]

[0072] Comparative Example

[0073] (1) Determine the particle size of crushed stone used to prepare cement concrete;

[0074] (2) The aggregates are classified into grades according to a preset particle size range, and are sorted and numbered from large to small according to the particle size; wherein 16-25 mm crushed stone is numbered A, 10-20 mm crushed stone is numbered B, and 5-10 mm crushed stone is numbered C;

[0075] (3) According to the mass ratio, the A aggregate and the B aggregate were mixed in the mixing ratio of 2:8, 3:7, 4:6, 5:5, 6:4, 7:3 and 8:2, and the tap density was measured. The results are shown in Table 1 above. The tap density-mixing ratio relationship curve was plotted, as shown in Figure 1 As shown, the mixing ratio corresponding to the maximum point of tap density is taken as the optimal mixing ratio of aggregate A and aggregate B, and the optimal mixing ratio of aggregate A and aggregate B is 1.9, that is, 16-25mm crushed stone: 10-20mm crushed stone = 1.9:1;

[0076] (4) Aggregate A and aggregate B were mixed according to the above-mentioned optimal mixing ratio of 1.9:1, and the two together formed aggregate (A+B); (A+B) aggregate and aggregate C were mixed in mixing ratios of 6:1, 5:1, 4:1, 3:1 and 2:1 according to the mass ratio, and the tap density was measured. The results are shown in Table 3 below, and the tap density-mixing ratio relationship curve was drawn, as shown in Figure 3 As shown, the mixing ratio corresponding to the maximum point of compacted density is taken as the optimal mixing ratio. The optimal mixing ratio of aggregate A, aggregate B and aggregate C under the optimal mixing ratio of (A+B) aggregate and aggregate C is obtained by conversion. The optimal mixing ratio of (A+B) aggregate and aggregate C is 4.3, that is, (A+B) aggregate: aggregate C = 3.8:1. After conversion, aggregate A: aggregate B and aggregate C = 2.48:1.31:1.

[0077] Table 3. Test results of tap density of (A+B) aggregate and C aggregate at different mixing ratios

[0078]

[0079] Cement concrete specimens were prepared according to the cement dosage, water dosage, sand ratio and admixture dosage of the control example gradation and the preparation method, and the slump (measured according to T0522JTG E30-2005), the compressive strength on the 7th day and the 28th day (measured according to T0558 JTG E30-2005) and the flexural strength on the 7th day and the 28th day (measured according to T0555 JTG E30-2005) of the cement concrete of the control example, the embodiment and the comparative example were measured. The results are shown in Table 4 below.

[0080] Table 4 Performance test results of cement concrete of control example, embodiment and comparative example

[0081]

[0082] From the slump test results of cement concrete specimens, it can be seen that the slump of the cement concrete specimens prepared in the embodiments and comparative examples is 15-20mm, and the slump of the cement concrete specimens prepared in the control example is 20-25mm. Although the increase in the skeleton embedding effect leads to a decrease in the slump of the embodiments and comparative examples, it still meets the basic slump requirement (10-30mm) for slipform paving.

[0083] The mechanical properties test results of cement concrete specimens were analyzed and found that in terms of 7-day compressive strength, the comparative example > the embodiment > the control example; in terms of 28-day compressive strength, the embodiment > the comparative example > the control example, indicating that the enhanced skeleton embedding effect can effectively improve the compressive strength of cement concrete materials. In terms of 7-day flexural strength, the control example > the comparative example > the embodiment; in terms of 28-day compressive strength, the embodiment > the comparative example > the control example. It can be seen that although the flexural strength of the embodiment on the 7th day is lower than that of the control example gradation, after 28 days of curing, the final flexural strength of the embodiment gradation is higher than that of the control gradation, indicating that it has better bending and tensile properties. In addition, it can be found that both the 28-day compressive strength and the 28-day flexural strength of the embodiment are better than the control group, indicating that the quality of the aggregate skeleton mechanical properties is positively correlated with the skeleton packing density, but when the mechanical properties of cement concrete and its skeleton reach the best, the corresponding tap density is not the largest (this is mainly due to the influence of factors such as aggregate particle shape, single-grade aggregate grading, mud content, etc.), which further verifies the rationality and importance of verifying the mechanical properties in the last mixing of this scheme.

[0084] The results of mechanical property tests show that the aggregate gradation design method of this scheme can achieve the stable embedding effect of coarse aggregate in cement concrete and the optimal skeleton mechanical properties, and the final mechanical strength (flexural and compressive strength) of cement concrete after molding can be improved, which has good application significance. In the subsequent implementation process, if the mechanical strength is required to be consistent with the gradation of the control example, the purpose of improving the economic applicability of this scheme can be achieved by reducing the cement dosage of the embodiment.

[0085] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A method for designing aggregate gradation for forming a cement concrete skeleton, characterized in that: The following steps are involved: Determine the particle size of aggregates used to prepare cement concrete; classify the aggregates according to a preset particle size range, and sort and number them from large to small according to the particle size; wherein the aggregate with the largest particle size is numbered A, the aggregate with the second largest particle size is numbered B, the aggregate with the third largest particle size is numbered C, and so on; Calculate by mass ratio, mix aggregate A and aggregate B in a preset mixing ratio, and then measure the tap density, draw a tap density-mixing ratio relationship curve, and take the mixing ratio corresponding to the maximum tap density point as the optimal mixing ratio of aggregate A and aggregate B; Aggregate A and aggregate B are blended according to the above-mentioned optimal mixing ratio, and the two together form aggregate (A+B); according to the mass ratio, aggregate (A+B) and aggregate C are mixed according to the preset mixing ratio and then the tap density is measured, and a tap density-mixing ratio relationship curve is drawn. The mixing ratio corresponding to the maximum tap density point is taken as the optimal mixing ratio, and the optimal mixing ratio of aggregate A, aggregate B and aggregate C under the optimal mixing ratio of aggregate (A+B) and aggregate C is obtained by conversion; and so on, until the optimal mixing ratios of aggregates with other numbers except the last number have been determined; Aggregates with other numbers except the last number are mixed according to the best mixing ratio to form mixed aggregates; after the mixed aggregates and the last numbered aggregates are mixed according to the preset mixing ratio according to the mass ratio, the skeleton penetration pressure is measured, and a skeleton penetration pressure-mixing ratio relationship curve is drawn. The mixing ratio corresponding to the maximum point of the skeleton penetration pressure is taken as the best mixing ratio, and the best mixing ratio of all numbered aggregates under the best mixing ratio of the mixed aggregates and the last numbered aggregates is obtained by conversion; There are 7 groups of preset mixing ratios of aggregate A and aggregate B, which are 2:8, 3:7, 4:6, 5:5, 6:4, 7:3 and 8:2 calculated by mass ratio.

2. A method for designing aggregate gradation for forming a cement concrete skeleton according to claim 1, characterized in that: The number of preset mixing ratios of (A+B) aggregate and C aggregate and the number of preset mixing ratios of mixed aggregate and last numbered aggregate are both set to at least 5 groups.

3. A method for designing aggregate gradation for forming a cement concrete skeleton according to claim 2, characterized in that: There are five groups of preset mixing ratios of (A+B) aggregate and C aggregate, which are 6:1, 5:1, 4:1, 3:1 and 2:1 calculated by mass ratio.

4. The aggregate gradation design method for forming a cement concrete skeleton according to claim 2, characterized in that: There are five groups of preset mixing ratios of mixed aggregate and final numbered aggregate, which are 6:1, 5:1, 4:1, 3:1 and 2:1 calculated by mass ratio.

5. The aggregate gradation design method for forming a cement concrete skeleton according to claim 1, characterized in that: The tap density is measured at least three times, and the arithmetic mean of the three tap densities is taken to draw a tap density-mixing ratio relationship curve.

6. A method for designing aggregate gradation for forming a cement concrete skeleton according to claim 5, characterized in that: The tap density is measured at least 3 times, and after removing the abnormal values, the arithmetic mean of the remaining tap density is taken to draw a tap density-mixing ratio relationship curve; The absolute value of the difference between the abnormal value and the average value of the three tap densities is greater than 1.15 times the first preset difference.

7. The aggregate gradation design method for forming a cement concrete skeleton according to claim 1, characterized in that: The skeleton penetration pressure is measured at least three times, and the arithmetic mean of the three skeleton penetration pressures is taken to draw a skeleton penetration pressure-mixing ratio relationship curve.

8. The aggregate gradation design method for forming a cement concrete skeleton according to claim 7, characterized in that: The skeleton penetration pressure is measured at least 3 times, and after removing abnormal values, the arithmetic mean of the remaining skeleton penetration pressures is taken to draw a skeleton penetration pressure-mixing ratio relationship curve; Among them, the absolute value of the difference between the abnormal value and the average value of the three skeleton penetration pressures is greater than 1.15 times the second preset difference.

Citation Information

Patent Citations

  • Porous concrete mix proportion design method

    CN106294973A

  • Method for determining aggregate proportion of sand grain type asphalt concrete

    CN111965071A