Cement-based energy storage structure and preparation method thereof

By setting up a diaphragm and epoxy resin encapsulation layer in the cement-based energy storage structure, using the double layer effect of electrodes and carbon fiber activated carbon powder, the problem of low energy storage efficiency in existing energy storage technologies is solved, and high-efficiency electrical energy storage is achieved , and provides low-cost, safe and durable new energy storage methods.

CN118983192APending Publication Date: 2024-11-19KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411026214.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the existing energy storage technology, energy storage efficiency is low, and untreated cement matrix seriously affects ion transmission, making it difficult to meet the needs of the power system.

Method used

Adopt a cement-based energy storage structure, including a cement matrix, a diaphragm, an epoxy resin encapsulation layer and an electrode. The diaphragm is arranged inside the cement matrix to separate it into two areas, and an epoxy resin encapsulation layer is arranged on the outside. Located between the cement matrix and the epoxy resin encapsulation layer, the cations and anions in the electrolyte are moved by applying voltage and adsorbed on the electrodes and carbon fibers and activated carbon powder surfaces to form an electric double layer to store electrical energy.

Benefits of technology

It significantly improves energy storage efficiency, is low cost, has good mechanical performance, simple structural composition, high durability and safety, provides a technology that integrates structure and energy storage, and provides a new way for the safe storage of new energy. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983192A_ABST
    Figure CN118983192A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of cement-based composite material electrochemistry, in particular to a cement-based energy storage structure and a preparation method thereof.The cement-based energy storage structure comprises a cement matrix, a diaphragm, an epoxy resin packaging layer and an electrode; a diaphragm is arranged in the cement base body, and the interior of the cement base body is divided into two areas by the diaphragm; the cement base body is sleeved with an epoxy resin packaging layer. The electrodes are located between the cement base body and the epoxy resin packaging layer and arranged on the outer wall of the cement base body. According to the cement-based energy storage structure, electric energy can be stored, and the energy storage efficiency can be greatly improved through conductive filler distribution and a communicating hole structure in the cement matrix, so that the problem that the energy storage efficiency is low in an existing energy storage technology is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement-based composite electrochemical technology, and in particular to a cement-based energy storage structure and a preparation method thereof. Background Art

[0002] With the continuous development of new energy technologies, the importance of energy storage technology has become increasingly prominent. New energy power generation (wind power and photovoltaic power, etc.) and user power load demand show seasonal and climatic changes, and the peak power consumption period is often inconsistent with the peak power generation period of new energy in terms of time and space. Therefore, energy storage technology must be used to provide guarantees for the safe and stable operation of new energy consumption and power systems.

[0003] Energy storage technology plays an indispensable role in improving energy efficiency, ensuring energy supply security, and promoting the development of renewable energy. It is an important part of building a sustainable energy system in the future. Battery energy storage is one of the energy storage technologies. Battery energy storage has high energy density and can respond to rapid charge and discharge. It has become the most widely used energy storage method in life. However, the cost, life and number of charge and discharge times of batteries seriously restrict their application. At the same time, their pollution and recycling issues are also important problems that are difficult to solve.

[0004] Existing energy storage technologies still cannot meet the needs of the power system. For example, a cement-based electrochemical energy storage device and its preparation method disclosed in patent number CN202211405404.X provide a new energy storage method for new energy storage, but its energy storage efficiency is low, and the untreated cement matrix seriously affects ion transmission.

[0005] Therefore, it is urgent to explore and develop new energy storage technologies to solve the problem of low energy storage efficiency in existing energy storage technologies. Summary of the invention

[0006] The purpose of the present invention is to provide a cement-based energy storage structure and a preparation method thereof, so as to solve the problem of low energy storage efficiency in existing energy storage technologies.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0008] A cement-based energy storage structure comprises a cement matrix, a diaphragm, an epoxy resin encapsulation layer and an electrode; the diaphragm is arranged inside the cement matrix, and the diaphragm divides the inside of the cement matrix into two areas; the epoxy resin encapsulation layer is sleeved outside the cement matrix; the electrode is located between the cement matrix and the epoxy resin encapsulation layer, and the electrodes are respectively arranged on the outer wall of the cement matrix.

[0009] Preferably, the electrode is a metal electrode, and the thickness of the metal electrode is 0.5-2 mm.

[0010] Preferably, the diaphragm is a battery diaphragm, and the material of the battery diaphragm is either polyethylene or polypropylene.

[0011] Preferably, the cement matrix comprises the following raw materials in parts by weight:

[0012] 40-70 parts of cement, 20-30 parts of sand, 15-30 parts of water, 0.5-2 parts of carbon fiber, 1-10 parts of activated carbon powder, and 0.1-1 parts of foaming agent.

[0013] Preferably, the cement is any one of ordinary Portland cement, slag Portland cement, pozzolanic Portland cement, fly ash Portland cement, composite Portland cement, rapid hardening Portland cement, aluminate cement or sulphoaluminate cement.

[0014] Preferably, the sand is any one of river sand or artificial sand, and the sand fineness modulus is 2.3-3.0.

[0015] Preferably, the carbon fiber length is 3-9 mm, the carbon fiber diameter is 7-10 μm, and the activated carbon powder particle size is 0.01-0.5 mm.

[0016] Preferably, the cement matrix further comprises an electrolyte solution, and the electrolyte solution is any one of potassium hydroxide, lithium hydroxide and potassium chloride, or a mixed solution of any several of potassium hydroxide, lithium hydroxide and potassium chloride.

[0017] The present application also provides a method for preparing a cement-based energy storage structure, which specifically comprises the following steps:

[0018] 1) Insert the diaphragm in the middle of the test mold;

[0019] 2) Pour cement matrix slurry into the test mold with the diaphragm inserted, remove the test mold after one day, obtain the cement matrix-diaphragm solidified product, and then perform standard curing on the cement matrix-diaphragm assembly for 28-60 days;

[0020] 3) Pasting electrodes on the outer wall of the cement matrix in the cement matrix-diaphragm assembly, and connecting the electrodes with two wires to obtain a cement matrix-diaphragm-electrode assembly;

[0021] 4) Dry the cement matrix-diaphragm-electrode assembly at a temperature of 60°C for 24 hours, and then place the dried cement matrix-diaphragm-electrode assembly in an electrolyte solution and soak it for 48 hours;

[0022] 5) Take out the cement matrix-diaphragm-electrode assembly from the electrolyte solution, use epoxy resin to encapsulate the outside of the cement matrix in the cement matrix-diaphragm-electrode assembly after being soaked in the electrolyte solution, and then cool the cement matrix-diaphragm-electrode assembly encapsulated with epoxy resin to obtain a cement-based energy storage structure.

[0023] Preferably, the cement matrix slurry preparation process specifically comprises the following steps:

[0024] a) Weigh cement, sand and activated carbon powder according to the mass ratio, and then mix the weighed cement, sand and activated carbon powder evenly to obtain a mixture of cement-sand-activated carbon powder;

[0025] b) weighing water, carbon fiber and foaming agent according to the mass ratio, pouring the weighed foaming agent into the weighed foaming agent and stirring evenly to obtain a foaming agent solution, and then pouring the weighed carbon fiber into the foaming agent solution and stirring evenly to obtain a mixed solution of water-carbon fiber-foaming agent;

[0026] c) Slowly pour the mixture of cement-sand-activated carbon powder in a) into the mixed solution of water-carbon fiber-foaming agent in b) and stir thoroughly for 2-3 minutes to obtain a cement matrix slurry.

[0027] Energy storage principle of cement matrix energy storage structure, charging process: by applying voltage to the cement matrix, the cations and anions in the electrolyte in the cement matrix move to the negative electrode and the positive electrode respectively, and adsorb on the surface of the electrode and the carbon fiber and activated carbon powder in the cement matrix. At the same time, the charge opposite to the ion will appear on the electrode surface and be stored on the electrode surface to form a double electrical layer.

[0028] Discharge process: The charge stored on the electrode surface migrates, forming a current released to the outside, and the ions on the electrode surface migrate back into the electrolyte.

[0029] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0030] 1. The cement-based energy storage structure of the present invention can not only store electrical energy, but also the distribution of the conductive filler and the interconnecting pore structure in the cement matrix can greatly improve the energy storage efficiency, thereby solving the problem of low energy storage efficiency in existing energy storage technologies.

[0031] 2. The cement-based energy storage structure of the present invention is not only low in cost, but also has good mechanical properties, simple structural composition, good durability, good stability and high safety.

[0032] 3. The cement-based energy storage structure of the present invention provides a technology that integrates structure and energy storage, and provides a new way for the safe storage of new energy, which is of great significance to ensuring my country's energy security. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the structure of the present invention.

[0034] Figure 2 is a cyclic voltammetry test curve diagram of the cement-based energy storage structure in an embodiment of the present invention;

[0035] Figure 3 is a charge and discharge curve diagram of the cement-based energy storage structure in an embodiment of the present invention; Figure 4 is an AC impedance spectrum curve diagram of the cement-based energy storage structure in an embodiment of the present invention; Figure 5 It is the compressive strength curve of the cement-based energy storage structure in the embodiment of the present invention. In the figure, 1-cement matrix, 2-diaphragm, 3-epoxy resin packaging layer, 4-electrode. DETAILED DESCRIPTION

[0036] like Figure 1-5 In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0037] Existing energy storage technologies still cannot meet the needs of the power system. For example, a cement-based electrochemical energy storage device and its preparation method disclosed in patent number CN202211405404.X provide a new energy storage method for new energy storage, but its energy storage efficiency is low, and the untreated cement matrix seriously affects ion transmission.

[0038] Therefore, it is urgent to explore and develop new energy storage technologies to solve the problem of low energy storage efficiency of existing energy storage technologies; for details, refer to Example 1, Example 2 and Example 3.

[0039] Embodiment 1

[0040] A method for preparing a cement-based energy storage structure comprises the following steps:

[0041] The first step: insert the diaphragm (diaphragm: battery diaphragm) into the middle of the rectangular test mold, so that the inside of the test mold is divided into two left and right areas by the diaphragm;

[0042] Step 2: When the diaphragm and the test mold are assembled, first weigh 40 parts of ordinary Portland cement, 20 parts of river sand with a fineness modulus of 2.5, 20 parts of laboratory tap water, 0.05 parts of 6mm long carbon fiber, 0.5 parts of activated carbon powder with a diameter of 0.1mm and 0.1 parts of concrete chemical foaming agent, and then mix the weighed cement, sand and activated carbon powder evenly to obtain a mixture of cement-sand-activated carbon powder;

[0043] After the mixture of cement-sand-activated carbon powder is prepared, pour the weighed foaming agent into the weighed foaming agent and stir evenly to obtain a foaming agent solution, then pour the weighed carbon fiber into the foaming agent solution and stir evenly to obtain a mixed solution of water-carbon fiber-foaming agent;

[0044] After the mixed solution of water-carbon fiber-foaming agent is prepared, slowly pour the previously prepared mixture of cement-sand-activated carbon powder into the mixed solution of water-carbon fiber-foaming agent and stir thoroughly for 2-3 minutes to obtain cement matrix slurry;

[0045] When the cement matrix slurry is prepared, the cement matrix slurry is poured into the test mold with the diaphragm inserted, and the cement matrix slurry and the test mold with the diaphragm inserted are solidified. The solidification time can be one day, and then the test mold is removed to obtain a cement matrix-diaphragm combination. The cement matrix-diaphragm combination is then subjected to standard curing. The standard curing time can be 28-60 days.

[0046] Step 3: After the cement matrix-diaphragm assembly is cured, the two electrodes (copper electrodes) are first polished, the electrode polishing thickness can be 0.5-2mm, and the electrode polishing roughness can be 0.01-0.1mm. Then, the two polished electrodes are respectively bonded to the outer wall of the cement matrix in the cement matrix-diaphragm assembly, and two wires are used to connect the electrodes respectively to obtain a cement matrix-diaphragm-electrode assembly;

[0047] Step 4: Dry the cement matrix-diaphragm-electrode assembly at 60°C for 24 hours, and then soak the dried cement matrix-diaphragm-electrode assembly in a 3 mol / L potassium chloride solution for 48 hours, so that the 3 mol / L potassium chloride solution enters the cement matrix of the cement matrix-diaphragm-electrode assembly by infiltration;

[0048] Step 5: After the cement matrix-diaphragm-electrode assembly is immersed in a potassium chloride solution with a concentration of 3 mol / L for 48 hours, the cement matrix-diaphragm-electrode assembly is taken out from the potassium chloride solution, and the outside of the cement matrix in the cement matrix-diaphragm-electrode assembly immersed in the potassium chloride solution is first encapsulated with epoxy resin, and then the cement matrix-diaphragm-electrode assembly encapsulated with epoxy resin is cooled to finally obtain a cement-based energy storage structure.

[0049] The cement-based energy storage structure prepared by the above preparation method is as follows Figure 1 As shown, specifically, the cement-based energy storage structure includes a cement matrix 1, a diaphragm 2, an epoxy resin encapsulation layer 3 and an electrode 4; wherein the cement matrix 1 serves as a matrix for installing the diaphragm 2, the epoxy resin encapsulation layer 3 and the electrode 4; the diaphragm 2 is inserted into the cement matrix 1, and the diaphragm is used to separate the interior of the cement matrix 1 into two left and right areas; the electrode 4 is used to be connected to a wire connected to an external power supply; the epoxy resin encapsulation layer 3 is used to encapsulate the cement matrix 1 and the electrode 4.

[0050] More specifically, a diaphragm 2 is vertically arranged inside the cement matrix 1. The diaphragm 2 is a battery diaphragm. The material of the battery diaphragm is either polyethylene or polypropylene. The diaphragm 2 divides the interior of the cement matrix 1 into two left and right areas. The pores in the left and right areas of the cement matrix 1 are filled with electrolyte solutions with anions and cations. An epoxy resin encapsulation layer 3 is provided on the outside of the cement matrix 1. The electrode 4 is located between the cement matrix 1 and the epoxy resin encapsulation layer 3. The electrode 4 is a metal electrode. The thickness of the metal electrode 4 is 0.5-2mm. The electrodes 4 are respectively arranged on the outer walls on both sides of the cement matrix 1.

[0051] It should be noted that the energy storage principle of the cement-based energy storage structure is: Charging process: by applying an external voltage to the cement matrix, the cations and anions in the electrolyte in the cement matrix move to the negative electrode and the positive electrode respectively, and are adsorbed on the surface of the electrode and the carbon fiber and activated carbon powder in the cement matrix. At the same time, an electric charge opposite to the ion will appear on the electrode surface and be stored on the electrode surface to form a double electrical layer.

[0052] Discharge process: The charge stored on the electrode surface migrates, forming a current released to the outside, and the ions on the electrode surface migrate back into the electrolyte.

[0053] Next, the cement-based energy storage structure in this embodiment is subjected to cyclic voltammetry test, charge and discharge test, AC impedance spectroscopy test and compressive strength test in sequence.

[0054] Specifically, the cement-based energy storage structure was tested by cyclic voltammetry. The test results are as follows: Figure 2 As shown, Figure 2 The horizontal axis in is the external voltage value applied. Figure 2 The vertical axis is the current density.

[0055] from Figure 2 It can be seen that the CV curve integral area of ​​the cement-based energy storage structure of the present invention is large, has a large specific capacitance, can store a certain amount of charge, and has the function of storing electrical energy.

[0056] Specifically, the cement-based energy storage structure was charged and discharged, and the test results were as follows: Figure 3 As shown, Figure 3 The horizontal axis is the time used for charging and discharging. Figure 3 The vertical axis is the charging and discharging voltage.

[0057] from Figure 3 It can be seen that the cement-based energy storage structure of the present invention has good electrochemical cycle reversibility and stability; in addition, from the perspective of the time used for charging and discharging, the energy density and power density of the cement-based energy storage structure are relatively high, which can meet the requirements of energy storage.

[0058] Specifically, the cement-based energy storage structure was tested for AC impedance spectroscopy. The test results are as follows: Figure 4 As shown, Figure 4 The horizontal axis in is the real part of the AC impedance voltage. Figure 4 The ordinate in is the imaginary part of the flow impedance voltage.

[0059] from Figure 4 It can be seen that the cement-based energy storage structure of the present invention has good conductivity and exhibits good conductivity under different alternating current frequencies. The conductive filler in the cement matrix can provide more places for ion attachment, thereby improving the energy storage efficiency.

[0060] Specifically, the compressive strength test of the cement-based energy storage structure after 60 days of curing was carried out. The test results are as follows: Figure 5 As shown, Figure 5 The horizontal axis is the number of each embodiment. Figure 5 The vertical axis is the compressive strength of the cement-based energy storage structure.

[0061] from Figure 5 It can be seen that the 60-day compressive strength of the cement-based energy storage structure of the present invention is above 30 MPa, and it can play a mechanical support role. This is mainly because the bridging effect of some carbon fibers and the filling effect of activated carbon powder can effectively improve the compressive strength of the structure. Although a large number of interconnected pores are created by the foaming agent, the compressive strength of the structure is still good.

[0062] Embodiment 2

[0063] The remaining steps of this embodiment are the same as those of the first embodiment, with the only difference being that in the process of preparing the cement-based energy storage structure, the amount of carbon fiber in the cement matrix is ​​0.1 parts and the amount of activated carbon powder is 0.7 parts.

[0064] Specifically, a method for preparing a cement-based energy storage structure comprises the following steps:

[0065] The first step: insert the diaphragm (diaphragm: battery diaphragm) into the middle of the rectangular test mold, so that the inside of the test mold is divided into two left and right areas by the diaphragm;

[0066] Step 2: When the diaphragm and the test mold are assembled, first weigh 40 parts of ordinary Portland cement, 20 parts of river sand with a fineness modulus of 2.5, 20 parts of laboratory tap water, 0.1 part of 6mm long carbon fiber, 0.7 part of activated carbon powder with a diameter of 0.1mm and 0.1 part of concrete chemical foaming agent, and then mix the weighed cement, sand and activated carbon powder evenly to obtain a mixture of cement-sand-activated carbon powder;

[0067] After the mixture of cement-sand-activated carbon powder is prepared, pour the weighed foaming agent into the weighed foaming agent and stir evenly to obtain a foaming agent solution, then pour the weighed carbon fiber into the foaming agent solution and stir evenly to obtain a mixed solution of water-carbon fiber-foaming agent;

[0068] After the mixed solution of water-carbon fiber-foaming agent is prepared, slowly pour the previously prepared mixture of cement-sand-activated carbon powder into the mixed solution of water-carbon fiber-foaming agent and stir thoroughly for 2-3 minutes to obtain cement matrix slurry;

[0069] When the cement matrix slurry is prepared, the cement matrix slurry is poured into the test mold with the diaphragm inserted, and the cement matrix slurry and the test mold with the diaphragm inserted are solidified. The solidification time can be one day, and then the test mold is removed to obtain a cement matrix-diaphragm combination. The cement matrix-diaphragm combination is then subjected to standard curing. The standard curing time can be 28-60 days.

[0070] Step 3: After the cement matrix-diaphragm assembly is cured, the two electrodes (copper electrodes) are first polished, the electrode polishing thickness can be 0.5-2mm, and the electrode polishing roughness can be 0.01-0.1mm. Then, the two polished electrodes are respectively bonded to the outer wall of the cement matrix in the cement matrix-diaphragm assembly, and two wires are used to connect the electrodes respectively to obtain a cement matrix-diaphragm-electrode assembly;

[0071] Step 4: Dry the cement matrix-diaphragm-electrode assembly at 60°C for 24 hours, and then soak the dried cement matrix-diaphragm-electrode assembly in a 3 mol / L potassium chloride solution for 48 hours, so that the 3 mol / L potassium chloride solution enters the cement matrix of the cement matrix-diaphragm-electrode assembly by infiltration;

[0072] Step 5: After the cement matrix-diaphragm-electrode assembly is immersed in a potassium chloride solution with a concentration of 3 mol / L for 48 hours, the cement matrix-diaphragm-electrode assembly is taken out from the potassium chloride solution, and the outside of the cement matrix in the cement matrix-diaphragm-electrode assembly immersed in the potassium chloride solution is first encapsulated with epoxy resin, and then the cement matrix-diaphragm-electrode assembly encapsulated with epoxy resin is cooled to finally obtain a cement-based energy storage structure.

[0073] Next, the cement-based energy storage structure in this embodiment is subjected to cyclic voltammetry test, charge and discharge test, AC impedance spectroscopy test and compressive strength test in sequence.

[0074] Specifically, the cement-based energy storage structure was tested by cyclic voltammetry. The test results are as follows: Figure 2 As shown, Figure 2 The horizontal axis in is the external voltage value applied. Figure 2 The vertical axis is the current density.

[0075] from Figure 2 It can be seen that the increase of conductive fillers can increase the energy storage capacity of cement-based energy storage structures to a certain extent.

[0076] Specifically, the cement-based energy storage structure was charged and discharged, and the test results were as follows: Figure 3 As shown, Figure 3 The horizontal axis is the time used for charging and discharging. Figure 3 The vertical axis is the charging and discharging voltage.

[0077] from Figure 3 It can be seen that the increase of conductive fillers can, to a certain extent, make the cement-based energy storage structure have better electrochemical cycle reversibility and stability, and the time required for charging and discharging is reduced, and the energy storage efficiency is improved.

[0078] Specifically, the cement-based energy storage structure was tested for AC impedance spectroscopy. The test results are as follows: Figure 4 As shown, Figure 4 The horizontal axis in is the real part of the AC impedance voltage. Figure 4 The ordinate in is the imaginary part of the flow impedance voltage.

[0079] from Figure 4 It can be seen that the increase in conductive fillers leads to a decrease in structural resistivity, which enhances the conductivity of the cement-based energy storage structure and is beneficial to ion transport and adsorption.

[0080] Specifically, the compressive strength test of the cement-based energy storage structure after 60 days of curing was carried out. The test results are as follows: Figure 5 As shown, Figure 5The horizontal axis is the number of each embodiment. Figure 5 The vertical axis is the compressive strength of the cement-based energy storage structure.

[0081] from Figure 5 It can be seen that the compressive strength of the cement-based energy storage structure after curing for 60 days is slightly lower than 30MPa, indicating that the increase in carbon fiber and activated carbon powder introduces more porosity and defects, and the compressive strength of the cement-based energy storage structure decreases.

[0082] Embodiment 3

[0083] The remaining steps of this embodiment are the same as those of Embodiment 1, except that the ratio of the cement matrix raw materials is 30 parts of ordinary Portland cement, 30 parts of river sand with a fineness modulus of 2.5, 20 parts of laboratory tap water, 0.1 parts of carbon fiber, 1 part of activated carbon powder, and 0.05 parts of concrete chemical foaming agent.

[0084] Specifically, a method for preparing a cement-based energy storage structure comprises the following steps:

[0085] The first step: insert the diaphragm (diaphragm: battery diaphragm) into the middle of the rectangular test mold, so that the inside of the test mold is divided into two left and right areas by the diaphragm;

[0086] Step 2: When the diaphragm and the test mold are assembled, first weigh 3 parts of ordinary Portland cement, 3 parts of river sand with a fineness modulus of 2.5, 2 parts of laboratory tap water, 0.1 parts of carbon fiber, 1 part of activated carbon powder, and 0.05 parts of concrete chemical foaming agent, and then mix the weighed cement, sand and activated carbon powder evenly to obtain a mixture of cement-sand-activated carbon powder;

[0087] After the mixture of cement-sand-activated carbon powder is prepared, pour the weighed foaming agent into the weighed foaming agent and stir evenly to obtain a foaming agent solution, then pour the weighed carbon fiber into the foaming agent solution and stir evenly to obtain a mixed solution of water-carbon fiber-foaming agent;

[0088] After the mixed solution of water-carbon fiber-foaming agent is prepared, slowly pour the previously prepared mixture of cement-sand-activated carbon powder into the mixed solution of water-carbon fiber-foaming agent and stir thoroughly for 2-3 minutes to obtain cement matrix slurry;

[0089] When the cement matrix slurry is prepared, the cement matrix slurry is poured into the test mold with the diaphragm inserted, and the cement matrix slurry and the test mold with the diaphragm inserted are solidified. The solidification time can be one day, and then the test mold is removed to obtain a cement matrix-diaphragm combination. The cement matrix-diaphragm combination is then subjected to standard curing. The standard curing time can be 28-60 days.

[0090] Step 3: After the cement matrix-diaphragm assembly is cured, the two electrodes (copper electrodes) are first polished, the electrode polishing thickness can be 0.5-2mm, and the electrode polishing roughness can be 0.01-0.1mm. Then, the two polished electrodes are respectively bonded to the outer wall of the cement matrix in the cement matrix-diaphragm assembly, and two wires are used to connect the electrodes respectively to obtain a cement matrix-diaphragm-electrode assembly;

[0091] Step 4: Dry the cement matrix-diaphragm-electrode assembly at 60°C for 24 hours, and then soak the dried cement matrix-diaphragm-electrode assembly in a 3 mol / L potassium chloride solution for 48 hours, so that the 3 mol / L potassium chloride solution enters the cement matrix of the cement matrix-diaphragm-electrode assembly by infiltration;

[0092] Step 5: After the cement matrix-diaphragm-electrode assembly is immersed in a potassium chloride solution with a concentration of 3 mol / L for 48 hours, the cement matrix-diaphragm-electrode assembly is taken out from the potassium chloride solution, and the outside of the cement matrix in the cement matrix-diaphragm-electrode assembly immersed in the potassium chloride solution is first encapsulated with epoxy resin, and then the cement matrix-diaphragm-electrode assembly encapsulated with epoxy resin is cooled to finally obtain a cement-based energy storage structure.

[0093] Next, the cement-based energy storage structure in this embodiment is subjected to cyclic voltammetry test, charge and discharge test, AC impedance spectroscopy test and compressive strength test in sequence.

[0094] Specifically, the cement-based energy storage structure was tested by cyclic voltammetry. The test results are as follows: Figure 2 As shown, Figure 2 The horizontal axis in is the external voltage value applied. Figure 2 The vertical axis is the current density.

[0095] from Figure 2 It can be seen that with the decrease of cement content and the increase of activated carbon powder, the porosity of the cement-based energy storage structure increases, the current density increases, the specific capacitance increases, and the energy storage capacity increases.

[0096] Specifically, the cement-based energy storage structure was charged and discharged, and the test results were as follows: Figure 3 As shown, Figure 3 The horizontal axis is the time used for charging and discharging. Figure 3 The vertical axis is the charging and discharging voltage.

[0097] from Figure 3 It can be seen that with the increase of activated carbon powder, more adsorption sites are provided for ion migration, resulting in faster charging and discharging rates of the cement-based energy storage structure and increased energy storage efficiency.

[0098] Specifically, the cement-based energy storage structure was tested for AC impedance spectroscopy. The test results are as follows: Figure 4 As shown, Figure 4 The horizontal axis in is the real part of the AC impedance voltage. Figure 4 The ordinate in is the imaginary part of the flow impedance voltage.

[0099] from Figure 4 It can be seen that the AC impedance spectrum shows a lower resistivity, indicating that the increase of activated carbon powder leads to a decrease in the resistivity and an increase in the conductivity of the cement-based energy storage structure.

[0100] Specifically, the compressive strength test of the cement-based energy storage structure after 60 days of curing was carried out. The test results are as follows: Figure 5 As shown, Figure 5 The horizontal axis is the number of each embodiment. Figure 5 The vertical axis is the compressive strength of the cement-based energy storage structure.

[0101] from Figure 5 It can be seen that due to the reduction of cementitious material and the increase of activated carbon powder, the porosity of the matrix increases, which reduces the compressive strength of the energy storage structure.

[0102] The cement-based energy storage structure of the present invention can not only store electrical energy, but also the distribution of conductive fillers and interconnected pore structure in the cement matrix can greatly improve the energy storage efficiency; the cement-based energy storage structure of the present invention is not only low in cost, but also has good mechanical properties, simple structural composition, good durability, good stability and high safety; the cement-based energy storage structure of the present invention also provides a technology that integrates structure and energy storage, provides a new way for the safe storage of new energy, and is of great significance to ensuring my country's energy security

[0103] Although the present invention is described herein with reference to a number of illustrative embodiments of the present invention, it will be appreciated that those skilled in the art may devise many other modifications and implementations that fall within the scope and spirit of the principles disclosed herein. More specifically, within the scope of the present disclosure, drawings, and claims, a variety of variations and modifications may be made to the components and / or layout of the subject combination layout. In addition to the variations and modifications made to the components and / or layout, other uses will also be apparent to those skilled in the art.

Claims

1. A cement-based energy storage structure, characterized in that: include Cement matrix (1); A diaphragm (2), wherein the cement matrix (1) is provided with the diaphragm (2), and the diaphragm (2) divides the cement matrix (1) into two areas; An epoxy resin encapsulation layer (3), wherein the cement matrix (1) is provided with an epoxy resin encapsulation layer (3) on its exterior; Electrodes (4), the electrodes (4) are located between the cement matrix (1) and the epoxy resin packaging layer (3), and the electrodes (4) are respectively arranged on the outer wall of the cement matrix (1).

2. A cement-based energy storage structure according to claim 1, characterized in that: The electrode (4) is a metal electrode, and the thickness of the metal electrode (4) is 0.5-2 mm.

3. A cement-based energy storage structure according to claim 1, characterized in that: The diaphragm (2) is a battery diaphragm, and the material of the battery diaphragm is any one of polyethylene and polypropylene.

4. A cement-based energy storage structure according to claim 1, characterized in that: The cement matrix comprises the following raw materials in parts by weight: 40-70 parts of cement, 20-30 parts of sand, 15-30 parts of water, 0.5-2 parts of carbon fiber, 1-10 parts of activated carbon powder, and 0.1-1 parts of foaming agent.

5. A cement-based energy storage structure according to claim 4, characterized in that: The cement is any one of ordinary silicate cement, slag silicate cement, pozzolanic silicate cement, fly ash silicate cement, composite silicate cement, rapid hardening silicate cement, aluminate cement or sulphoaluminate cement.

6. A cement-based energy storage structure according to claim 4, characterized in that: The sand is any one of river sand and artificial sand, and the sand fineness modulus is 2.3-3.

0.

7. A cement-based energy storage structure according to claim 4, characterized in that: The length of the carbon fiber is 3-9 mm, the diameter of the carbon fiber is 7-10 μm, and the particle size of the activated carbon powder is 0.01-0.5 mm.

8. The cement-based energy storage structure according to claim 1, characterized in that: The cement matrix (1) further comprises an electrolyte solution (5) therein, and the electrolyte solution (5) is any one of potassium hydroxide, lithium hydroxide and potassium chloride, or a mixed solution of any several of potassium hydroxide, lithium hydroxide and potassium chloride.

9. A method for preparing a cement-based energy storage structure according to any one of claims 1 to 8, characterized in that: The method for preparing a cement-based energy storage structure comprises the following steps: 1) Insert the diaphragm in the middle of the test mold; 2) Pour cement matrix slurry into the test mold with the diaphragm inserted. After one day, remove the test mold to obtain the cement matrix-diaphragm assembly, and then perform standard curing on the cement matrix-diaphragm assembly for 28-60 days; 3) Electrodes are respectively attached to the outer wall of the cement matrix in the cement matrix-diaphragm assembly, and are respectively connected to the electrodes with two wires to obtain a cement matrix-diaphragm-electrode assembly; 4) Dry the cement matrix-diaphragm-electrode assembly for 24 hours at a temperature of 60°C, then place the dried cement matrix-diaphragm-electrode assembly in an electrolyte solution and soak it for 48 hours; 5) Take out the cement matrix-diaphragm-electrode assembly from the electrolyte solution, use epoxy resin to encapsulate the outside of the cement matrix in the cement matrix-diaphragm-electrode assembly soaked in the electrolyte solution, and then cool the cement matrix-diaphragm-electrode assembly encapsulated with epoxy resin to obtain a cement-based energy storage structure.

10. The method for preparing a cement-based energy storage structure according to claim 9, characterized in that: The cement matrix slurry preparation process specifically includes the following steps: a) Weigh cement, sand and activated carbon powder according to the mass ratio, and then mix the weighed cement, sand and activated carbon powder evenly to obtain a mixture of cement-sand-activated carbon powder; b) weighing water, carbon fiber and foaming agent according to the mass ratio, pouring the weighed foaming agent into the weighed foaming agent and stirring evenly to obtain a foaming agent solution, and then pouring the weighed carbon fiber into the foaming agent solution and stirring evenly to obtain a mixed solution of water-carbon fiber-foaming agent; c) Slowly pour the mixture of cement-sand-activated carbon powder in a) into the mixed solution of water-carbon fiber-foaming agent in b), and stir thoroughly for 2-3 minutes to obtain a cement matrix slurry.

Citation Information

Cited By

  • Cement-based zinc battery with low interface impedance as well as preparation method and application of cement-based zinc battery

    CN119695302A

  • Flexible aluminoferrite cement-based supercapacitor and preparation method thereof

    CN120199623A

  • A flexible iron aluminate cement-based supercapacitor and its preparation method

    CN120199623B

  • Method for regulating and controlling pore structure of cement-based supercapacitor

    CN120933081A

  • Thermoelectric power generation-energy storage concrete material system as well as preparation method and application thereof

    CN122444489A