Artificial anti-ferroelectric capacitor with high energy storage density and design method thereof

By introducing a built-in electric field into the dielectric layer, using work function differences to build artificial antiferroelectric capacitors, the problem of insufficient existing antiferroelectric materials is solved, and the capacitor design with high energy storage density and high efficiency utilization is realized .

CN119069261APending Publication Date: 2024-12-03INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411435679.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

There are few antiferroelectric materials in existing, resulting in the research on high energy storage density artificial antiferroelectric capacitors in a vacant stage, and it is difficult to achieve high energy storage density and high energy storage efficiency.

Method used

By introducing a built-in electric field with opposite directions into the dielectric layer, high-energy storage density artificial antiferroelectric capacitors are constructed using the difference in work functions of different materials, including the bottom electrode layer, the middle layer and the top electrode layer, and the electrode layer is optimized by the phase field simulation method. The distribution and dielectric layer thickness are used to achieve double hysteresis loop characteristics.

Benefits of technology

The energy storage density and energy storage efficiency of the capacitor are significantly improved, and high energy storage density and high efficiency utilization are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069261A_ABST
    Figure CN119069261A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of capacitors, and particularly relates to a high-energy-storage-density artificial anti-ferroelectric capacitor and a design method thereof.The high-energy-storage-density artificial anti-ferroelectric capacitor comprises a bottom electrode layer, a first dielectric layer, a middle layer, a second dielectric layer and a top electrode layer; a bottom electrode layer, a first dielectric layer, an intermediate layer, a second dielectric layer, and a top electrode layer sequentially stacked in a first direction; the first direction is perpendicular to the plane where the bottom electrode layer is located and points to the top electrode layer from the bottom electrode layer. By introducing opposite built-in electric fields into the two dielectric layers, the artificial anti-ferroelectric film is obtained to serve as a dielectric of the capacitor, and by designing the sizes of the built-in electric fields, the thicknesses of the electrode layers and the dielectric layers and the strain of the dielectric layers, the energy storage density and efficiency of the anti-ferroelectric film are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of capacitors, in particular to an artificial antiferroelectric capacitor with high energy storage density and a design method thereof. Background Art

[0002] Compared with other energy storage devices such as batteries and electrochemical capacitors, dielectric capacitors have the advantages of fast charging and discharging speed, high power density, and long cycle life, which makes dielectric capacitors widely used in medical devices, pulse electronic equipment, etc. According to the differences in dielectric structure and properties, dielectrics can be divided into linear dielectrics, paraelectrics, ferroelectrics, antiferroelectrics, and relaxor ferroelectrics. Ferroelectrics can quickly reach saturation after the electric field is applied, but have a certain residual polarization after the electric field is removed and cannot return to the initial state. Therefore, the dielectric loss is large and it is not suitable for high energy storage density applications. Antiferroelectrics are different from ferroelectrics. The arrangement of adjacent dipoles in anti-ferroelectrics is opposite to each other. In the macroscopic state, the polarization is zero. When an external electric field is applied, the orientation of adjacent dipoles becomes consistent and transforms into a ferroelectric. Antiferroelectrics have double hysteresis loops and zero residual polarization, which is conducive to the improvement of energy storage density. Compared with ferroelectric materials, the reversibility of field-induced phase transition in antiferroelectric materials reduces the energy loss during the charging and discharging process. However, there are currently few known antiferroelectric materials and this field is in a vacant stage. Therefore, it is necessary to vigorously carry out research on the realization of artificial antiferroelectric capacitors with high energy storage density. Summary of the invention

[0003] The present invention provides a high energy storage density artificial antiferroelectric capacitor and a design method thereof. The bottom electrode layer, the middle layer and the top electrode layer are made of materials with different work functions, and a built-in electric field with opposite directions is introduced into the first dielectric layer and the second dielectric layer through work function engineering to form a capacitor with antiferroelectric characteristics of double hysteresis loops. The high energy storage density artificial antiferroelectric capacitor constructed by introducing a built-in electric field using the work function difference of different materials improves the energy storage density and energy storage efficiency of the capacitor.

[0004] The technical solution adopted by the present invention to achieve the above-mentioned purpose is: an artificial antiferroelectric capacitor with high energy storage density, comprising: a bottom electrode layer, a first dielectric layer, an intermediate layer, a second dielectric layer and a top electrode layer;

[0005] A bottom electrode layer, a first dielectric layer, an intermediate layer, a second dielectric layer, and a top electrode layer sequentially stacked in a first direction;

[0006] The first direction is perpendicular to the plane where the bottom electrode layer is located, and points from the bottom electrode layer to the top electrode layer.

[0007] The first dielectric layer and the second dielectric layer are made of any one of ferroelectric materials, relaxor ferroelectric materials or antiferroelectric materials.

[0008] The thickness of the bottom electrode layer, the middle layer and the top electrode layer ranges from 2 nm to 500 nm;

[0009] The thickness range of the first dielectric layer and the second dielectric layer is 2nm-1μm, and the in-plane strain range of the film is -2%-2%.

[0010] The intermediate layer is a material having a work function difference with the bottom electrode layer and the top electrode layer, that is, any one of an electrode or a dielectric material.

[0011] A design method for an artificial antiferroelectric capacitor with high energy storage density comprises the following steps:

[0012] 1) Selecting materials of the bottom electrode layer, the middle layer and the top electrode layer with different work functions; and ensuring that the work function of the middle layer material is greater than or less than the work function of the two electrode layer materials;

[0013] 2) Selecting materials for the first dielectric layer and the second dielectric layer; and establishing built-in electric fields in the first dielectric layer and the second dielectric layer respectively according to the difference in work function between the intermediate layer and the electrode layer materials, determining the thickness range of the dielectric layer in combination with the breakdown field strength of the dielectric layer materials, and selecting a suitable strain size for the dielectric layer;

[0014] 3) stacking a bottom electrode layer, a first dielectric layer, an intermediate layer, a second dielectric layer and a top electrode layer in sequence along a first direction to complete the structural design of the antiferroelectric capacitor;

[0015] 4) simulating the antiferroelectric capacitor by phase field simulation method to obtain the polarization distribution of the first dielectric layer, the middle layer and the second dielectric layer;

[0016] 5) drawing a PE hysteresis loop according to the polarization distribution of the first dielectric layer, the middle layer and the second dielectric layer, and integrating the polarization distribution to obtain the energy storage density and energy storage efficiency of the artificial antiferroelectric capacitor;

[0017] 6) Determine whether the energy storage density and energy storage efficiency of the antiferroelectric capacitor meet the set required values. If not, return to step 1) to step 2), reselect intermediate layer and electrode layer materials with different work functions, adjust the thickness and strain of the dielectric layer, and execute steps 3) to step 6). Otherwise, determine that the antiferroelectric capacitor meets the design requirements.

[0018] In step 2), a built-in electric field is established in the first dielectric layer and the second dielectric layer, respectively, specifically:

[0019] The material of the bottom electrode is selected to have the same work function as the material of the top electrode and greater than the work function of the material of the intermediate layer;

[0020] Generate a built-in electric field in the first dielectric layer directed from the middle layer to the bottom electrode, and generate a built-in electric field in the second dielectric layer directed from the middle layer to the top electrode;

[0021] The built-in electric field is the work function difference divided by the thickness of the corresponding dielectric layer;

[0022] The polarization directions of the built-in electric fields in the first dielectric layer and the second dielectric layer are completely opposite, and the overall polarization of the first dielectric layer, the intermediate layer, and the second dielectric layer is 0;

[0023] When an external electric field is applied, the variation of polarization with the electric field exhibits the characteristics of a double hysteresis loop of an artificial antiferroelectric.

[0024] The step 4) is specifically:

[0025] The artificial antiferroelectric capacitor is simulated by the phase field simulation method. The three components of polarization are used as order parameters to solve the TDGL equation with time t as the independent variable to obtain the polarization conditions of the first dielectric layer, the middle layer and the second dielectric layer, namely:

[0026]

[0027] Where L is the kinetic coefficient, F is the total free energy of the artificial antiferroelectric capacitor structure, and P i (x, t) is the polarization vector;

[0028] By solving equation (1), the polarization distribution of the artificial antiferroelectric capacitor structure is obtained.

[0029] In step 5), the polarization distribution is integrated to obtain the energy storage density and energy storage efficiency of the artificial antiferroelectric capacitor, specifically:

[0030] The energy density during the charge and discharge process is obtained by integrating the PE curve, that is:

[0031]

[0032]

[0033] Among them, W tot and W re are the total energy density and recoverable energy density, respectively, integrated over the charge and discharge paths, P max , P r , E and P are the maximum polarization intensity, residual polarization intensity, applied electric field and polarization intensity corresponding to the PE curve respectively;

[0034] The energy storage efficiency η is calculated by the following formula:

[0035]

[0036] The present invention has the following beneficial effects and advantages:

[0037] 1. The present invention introduces opposite built-in electric fields in two dielectric layers to obtain an artificial antiferroelectric film as the dielectric of the capacitor. By designing the size of the built-in electric field, the thickness of the electrode layer and the dielectric layer, and the strain of the dielectric layer, the energy storage density and efficiency of the antiferroelectric film are greatly improved.

[0038] 2. In the present invention, there is a work function difference between the electrode materials selected for the middle layer and the bottom electrode layer, and the middle layer and the top electrode layer, so that opposite built-in electric fields exist inside the two dielectric layers, and the polarization directions inside the two dielectric layers are opposite. By selecting appropriate materials and parameters, a capacitor with higher energy storage density and energy storage efficiency can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 Schematic diagram of the energy band structure of a capacitor when the work functions of the top electrode and the bottom electrode are different;

[0040] Figure 2 A schematic diagram of the structure of a high energy storage density artificial antiferroelectric capacitor conceived by the present invention;

[0041] 1 is the bottom electrode, 2 is the first dielectric layer, 3 is the middle layer, 4 is the second dielectric layer, and 5 is the top electrode.

[0042] Figure 3 A schematic diagram of the energy band structure of the artificial antiferroelectric capacitor with high energy storage density conceived by the present invention;

[0043] Figure 4 1 is a hysteresis loop diagram of Example 1 of the present invention;

[0044] Figure 5 1 is a hysteresis loop diagram of Example 2 of the present invention;

[0045] Figure 6 This is the hysteresis loop diagram of comparative example 1 of the present invention. DETAILED DESCRIPTION

[0046] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0047] The antiferroelectric thin film material provided by the present invention is composed of a bottom electrode layer, a first dielectric layer, an intermediate layer, a second dielectric layer, and a top electrode layer stacked in sequence. Since there is a certain work function difference between the materials selected for the intermediate layer and the bottom electrode layer and the top electrode layer, there will be a built-in electric field in the two dielectric layers, resulting in a preferred polarization orientation of the dielectric layer, and the polarization directions of the two dielectric layers are opposite. In the process of applying an external electric field, it is necessary to first flip the dielectric layer with a polarization direction opposite to the external field direction to a polarization direction identical to the external field direction, thereby forming a double hysteresis polarization-electric field curve with antiferroelectric characteristics. By introducing opposite built-in electric fields in the two dielectric layers, an artificial antiferroelectric thin film is obtained as a dielectric of a capacitor, and by designing the size of the built-in electric field, the thickness of the electrode layer and the dielectric layer, and the strain of the dielectric layer, the energy storage density and efficiency of the antiferroelectric thin film are greatly improved.

[0048] like Figure 2 , which is a schematic diagram of the structure of the artificial antiferroelectric capacitor with high energy storage density conceived by the present invention, the artificial antiferroelectric capacitor with high energy storage density of the present invention comprises: a bottom electrode layer 1, a first dielectric layer 2, an intermediate layer 3, a second dielectric layer 4 and a top electrode layer 5;

[0049] A bottom electrode layer 1, a first dielectric layer 2, an intermediate layer 3, a second dielectric layer 4 and a top electrode layer 5 are sequentially stacked in a first direction;

[0050] The first direction is perpendicular to the plane where the bottom electrode layer 1 is located, and points from the bottom electrode layer 1 to the top electrode layer 5 .

[0051] The first dielectric layer and the second dielectric layer are made of any one of ferroelectric materials, relaxor ferroelectric materials or antiferroelectric materials.

[0052] The thickness of the bottom electrode layer 1, the middle layer 3 and the top electrode layer 5 ranges from 2 nm to 500 nm;

[0053] The thickness of the first dielectric layer 2 and the second dielectric layer 4 is in the range of 2 nm to 1 μm, and the in-plane strain of the film is in the range of -2% to 2%.

[0054] The intermediate layer 3 is a material having a work function difference with the bottom electrode layer and the top electrode layer, that is, any one of an electrode or a dielectric material.

[0055] like Figure 1 As shown, it is a schematic diagram of the energy band structure of a capacitor when the work functions of the top electrode and the bottom electrode are different. The design principle of the present invention is:

[0056] The energy storage density of a material generally refers to the effective energy storage density, that is, the recoverable energy density (W re ). It can be obtained by integrating the PE (polarization-electric field) curve, Where P max is the maximum polarization intensity, P r is the residual polarization intensity after the electric field is removed, and E is the applied electric field intensity. When there is a built-in electric field in the dielectric layer that is opposite to the external electric field, a larger external electric field needs to be applied to the dielectric to achieve the same polarization state as when there is no built-in electric field. Therefore, the introduction of the built-in electric field will cause the PE curve to shift to the right, and the maximum electric field that can be applied, E max Increase, thereby increasing the energy storage density.

[0057] In a capacitor, when the work functions of the electrodes on both sides of the dielectric are different, a built-in electric field is generated inside the dielectric, such as Figure 1 When the work function of electrode 1 (W1) is greater than the work function of electrode 2 (W2), a built-in electric field ( Where d is the thickness of the dielectric), when the built-in electric field is large enough, the polarization direction of the dielectric will be exactly the same as the direction of the built-in electric field.

[0058] The design method of the high energy storage density artificial antiferroelectric capacitor of the present invention is as follows:

[0059] 1) Selecting materials of the bottom electrode layer 1, the middle layer 3 and the top electrode layer 5 with different work functions; and ensuring that the work function of the middle layer material is greater than or less than the work function of the two electrode layer materials;

[0060] 2) Selecting materials for the first dielectric layer 2 and the second dielectric layer 4; and establishing built-in electric fields in the first dielectric layer 2 and the second dielectric layer 4 respectively according to the difference in work function between the intermediate layer and the electrode layer materials, determining the thickness range of the dielectric layer in combination with the breakdown field strength of the dielectric layer materials, and selecting a suitable strain size for the dielectric layer;

[0061] The structure of the artificial antiferroelectric capacitor with high energy storage density of the present invention has an energy band structure as shown in FIG. Figure 3 As shown, a built-in electric field is established in the first dielectric layer 2 and the second dielectric layer 4, respectively, which specifically includes the following steps:

[0062] When the work function of the material of the bottom electrode 1 is the same as that of the material of the top electrode 5 and is greater than the work function of the material of the intermediate layer 3, a built-in electric field (E b ), a built-in electric field (E b ), resulting in the polarization directions in the first dielectric layer 2 and the second dielectric layer 4 being completely opposite, and the overall polarization of the first dielectric layer, the intermediate layer, and the second dielectric layer is 0. When an external electric field is applied, the change of polarization with the electric field will show the characteristics of the double hysteresis loop of the antiferroelectric.

[0063] 3) A bottom electrode layer 1, a first dielectric layer 2, an intermediate layer 3, a second dielectric layer 4 and a top electrode layer 5 are sequentially stacked along a first direction to complete the structural design of the antiferroelectric capacitor;

[0064] 4) simulating the antiferroelectric capacitor by phase field simulation method to obtain the polarization distribution of the first dielectric layer 2, the intermediate layer 3 and the second dielectric layer 4;

[0065] The structure is simulated using the phase field simulation method to obtain the polarization distribution of the first dielectric layer, the middle layer, and the second dielectric layer. The PE hysteresis loop is drawn and integrated to obtain the energy storage density and energy storage efficiency.

[0066] Phase field simulation uses the three components of polarization as order parameters and obtains the polarization of the film by solving the Ginzburg-Landau (TDGL) equation with time t as the independent variable:

[0067]

[0068] Where L is the kinetic coefficient, F is the total free energy of the artificial antiferroelectric capacitor structure, and P i (x, t) is the polarization vector;

[0069] By solving equation (1), the polarization distribution of the artificial antiferroelectric capacitor structure of the present invention can be obtained, and the PE hysteresis loop can be drawn according to the polarization magnitude under different electric field strengths.

[0070] 5) drawing a PE hysteresis loop according to the polarization distribution of the first dielectric layer 2, the intermediate layer 3 and the second dielectric layer 4, and integrating the polarization distribution to obtain the energy storage density and energy storage efficiency of the artificial antiferroelectric capacitor;

[0071] The energy density during the charge and discharge process can be calculated by integrating the PE curve:

[0072]

[0073]

[0074] Among them, W tot and W re are the total energy density and recoverable energy density, respectively, and need to integrate the charging and discharging paths respectively, P max , P r , E and P are the maximum polarization intensity, remnant polarization intensity, applied electric field and polarization intensity, respectively.

[0075] The energy storage efficiency can be calculated by the following formula:

[0076]

[0077] 6) Determine whether the energy storage density and energy storage efficiency of the antiferroelectric capacitor meet the set required values. If not, return to step 1) to step 2), reselect intermediate layer and electrode layer materials with different work functions, adjust the thickness and strain of the dielectric layer, and execute steps 3) to step 6). Otherwise, determine that the antiferroelectric capacitor meets the design requirements.

[0078] The following further examples are given to explain the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field according to the following contents of the present invention belong to the scope of protection of the present invention. In the description of the specification, many specific details are provided in order to enable readers to have a more complete understanding of the present invention; however, the present invention may still be implemented under the premise of omitting some or all of these specific details.

[0079] Embodiment 1:

[0080] The simulation parameters are selected as follows:

[0081] The in-plane dimensions of the model are 64 × 64 nm;

[0082] A potential of 3.0 V is set on the upper surface of the first dielectric layer and the lower surface of the second dielectric layer, and the potential of the lower surface of the first dielectric layer and the upper surface of the second dielectric layer is 0 V to simulate the potential difference between the upper and lower surfaces of the dielectric layer caused by the different work functions of the materials of the middle layer, the bottom electrode layer, and the top electrode layer. The thickness of the bottom electrode layer, the middle layer, and the top electrode layer are all selected to be 2 nm;

[0083] The first dielectric layer and the second dielectric layer are both selected as ferroelectric PbTiO3 films, and the thickness is both selected as 6nm. The in-plane strain of the lead titanate film is selected as 0.4%.

[0084] The PE curve of the artificial antiferroelectric film composed of the first dielectric layer, the middle layer and the second dielectric layer of this embodiment obtained by the phase field simulation method is as follows: Figure 4 As shown, it has obvious double hysteresis antiferroelectric characteristics.

[0085] According to formulas (2)-(4), Figure 4 By integrating the hysteresis loop shown in FIG. 1 , the recoverable energy density of the artificial antiferroelectric film of this embodiment is obtained to be 365.4 J / cm 3 , the energy storage efficiency is 89.0%.

[0086] Embodiment 2:

[0087] The simulation parameters are selected as follows:

[0088] The in-plane dimensions of the model are 64 × 64 nm;

[0089] A potential of 3.0 V is set on the upper surface of the first dielectric layer and the lower surface of the second dielectric layer, and the potential of the lower surface of the first dielectric layer and the upper surface of the second dielectric layer is 0 V to simulate the potential difference between the upper and lower surfaces of the dielectric layer caused by the different work functions of the materials of the middle layer, the bottom electrode layer, and the top electrode layer. The thickness of the bottom electrode layer, the middle layer, and the top electrode layer are all selected to be 2 nm;

[0090] The first dielectric layer and the second dielectric layer are both selected as ferroelectric PbTiO3 films, and the thickness is both selected as 6nm. The strain of the lead titanate film is selected as -1.3%.

[0091] The PE curve of the artificial antiferroelectric film composed of the first dielectric layer, the middle layer and the second dielectric layer of this embodiment obtained by the phase field simulation method is as follows: Figure 5 As shown, it has obvious double hysteresis antiferroelectric characteristics.

[0092] According to formulas (2)-(4), Figure 5 By integrating the hysteresis loop shown in FIG. 1 , the recoverable energy density of the artificial antiferroelectric film of this embodiment is obtained to be 288.0 J / cm 3 , the energy storage efficiency is 53.6%.

[0093] Comparative Example 1:

[0094] The simulation parameters are selected as follows:

[0095] The in-plane dimensions of the model are 64 × 64 nm;

[0096] The electric potentials of the upper and lower surfaces of the first dielectric layer and the second dielectric layer are both 0V, that is, the middle layer and the bottom electrode and the top electrode are made of materials with the same work function, and no built-in electric field is generated in the first dielectric layer and the second dielectric layer;

[0097] The thickness of the bottom electrode layer, the middle layer, and the top electrode layer are all selected to be 2 nm;

[0098] The first dielectric layer and the second dielectric layer are both selected as ferroelectric PbTiO3 films, and the thickness is both selected as 6nm. The strain of the lead titanate film is selected as -1.3%.

[0099] The PE curve of the film composed of the first dielectric layer, the middle layer and the second dielectric layer of this comparative example obtained by the phase field simulation method is as follows: Figure 6 As shown, since no built-in electric field is introduced, the characteristics of the ferroelectric hysteresis loop are still maintained.

[0100] According to formulas (2)-(4), Figure 6The hysteresis loop shown in FIG. 1 is integrated to obtain a recoverable energy density of 83.1 J / cm 3 , the energy storage efficiency is 62.5%.

[0101] The above description is only a suitable embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high energy storage density artificial antiferroelectric capacitor, characterized in that: include: A bottom electrode layer (1), a first dielectric layer (2), an intermediate layer (3), a second dielectric layer (4) and a top electrode layer (5); A bottom electrode layer (1), a first dielectric layer (2), an intermediate layer (3), a second dielectric layer (4) and a top electrode layer (5) stacked sequentially in a first direction; The first direction is perpendicular to the plane where the bottom electrode layer (1) is located, and points from the bottom electrode layer (1) to the top electrode layer (5).

2. The high energy storage density artificial antiferroelectric capacitor according to claim 1, characterized in that: The first dielectric layer and the second dielectric layer are made of any one of ferroelectric materials, relaxor ferroelectric materials or antiferroelectric materials.

3. The high energy storage density artificial antiferroelectric capacitor according to claim 1, characterized in that: The thickness of the bottom electrode layer, the middle layer and the top electrode layer ranges from 2 nm to 500 nm; The thickness range of the first dielectric layer and the second dielectric layer is 2nm-1μm, and the in-plane strain range of the film is -2%-2%.

4. The high energy storage density artificial antiferroelectric capacitor according to claim 1, characterized in that: The intermediate layer is a material having a work function difference with the bottom electrode layer and the top electrode layer, that is, any one of an electrode or a dielectric material.

5. The design method of a high energy storage density artificial antiferroelectric capacitor according to claim 1, characterized in that: The following steps are involved: 1) selecting materials of the bottom electrode layer (1), the middle layer (3) and the top electrode layer (5) with different work functions; and determining whether the work function of the middle layer material is greater than or less than the work functions of the two electrode layer materials; 2) selecting materials for the first dielectric layer (2) and the second dielectric layer (4); According to the difference in work function between the intermediate layer and the electrode layer material, a built-in electric field is established in the first dielectric layer (2) and the second dielectric layer (4), respectively, and the thickness range of the dielectric layer is determined in combination with the breakdown field strength of the dielectric layer material, and a suitable strain size is selected for the dielectric layer; 3) a bottom electrode layer (1), a first dielectric layer (2), an intermediate layer (3), a second dielectric layer (4) and a top electrode layer (5) are sequentially stacked along a first direction to complete the structural design of the antiferroelectric capacitor; 4) simulating the antiferroelectric capacitor by a phase field simulation method to obtain the polarization distribution of the first dielectric layer (2), the intermediate layer (3) and the second dielectric layer (4); 5) drawing a PE hysteresis loop according to the polarization distribution of the first dielectric layer (2), the intermediate layer (3) and the second dielectric layer (4), and integrating the polarization distribution to obtain the energy storage density and energy storage efficiency of the artificial antiferroelectric capacitor; 6) Determine whether the energy storage density and energy storage efficiency of the antiferroelectric capacitor meet the set required values. If not, return to step 1) to step 2), reselect intermediate layer and electrode layer materials with different work functions, adjust the thickness and strain of the dielectric layer, and execute steps 3) to step 6). Otherwise, determine that the antiferroelectric capacitor meets the design requirements.

6. The design method of a high energy storage density artificial antiferroelectric capacitor according to claim 5, characterized in that: In step 2), a built-in electric field is established in the first dielectric layer (2) and the second dielectric layer (4), respectively, specifically: The material of the bottom electrode (1) is selected to have a work function that is the same as that of the material of the top electrode (5) and greater than the work function of the material of the intermediate layer (3); A built-in electric field is generated in the first dielectric layer (2) and directed from the middle layer (3) to the bottom electrode (1), and a built-in electric field is generated in the second dielectric layer (4) and directed from the middle layer to the top electrode (5); The built-in electric field is the work function difference divided by the thickness of the corresponding dielectric layer; The polarization directions of the built-in electric fields in the first dielectric layer (2) and the second dielectric layer (4) are completely opposite, and the overall polarization of the first dielectric layer (2), the intermediate layer (3) and the second dielectric layer (4) is 0; When an external electric field is applied, the variation of polarization with the electric field exhibits the characteristics of a double hysteresis loop of an artificial antiferroelectric.

7. The design method of a high energy storage density artificial antiferroelectric capacitor according to claim 5, characterized in that: The step 4) is specifically: The artificial antiferroelectric capacitor is simulated by the phase field simulation method. The three components of polarization are used as order parameters to solve the TDGL equation with time t as the independent variable, and the polarization conditions of the first dielectric layer (2), the middle layer (3) and the second dielectric layer (4) are obtained respectively, that is: Where L is the kinetic coefficient, F is the total free energy of the artificial antiferroelectric capacitor structure, and P i (x, t) is the polarization vector; By solving equation (1), the polarization distribution of the artificial antiferroelectric capacitor structure is obtained.

8. The design method of a high energy storage density artificial antiferroelectric capacitor according to claim 5, characterized in that: In step 5), the polarization distribution is integrated to obtain the energy storage density and energy storage efficiency of the artificial antiferroelectric capacitor, specifically: The energy density during the charge and discharge process is obtained by integrating the PE curve, that is: Among them, W tot and W re are the total energy density and recoverable energy density, respectively, integrated over the charge and discharge paths, P max , P r , E and P are the maximum polarization intensity, residual polarization intensity, applied electric field and polarization intensity corresponding to the PE curve respectively; The energy storage efficiency η is calculated by the following formula:

Citation Information

Cited By

  • Phase field simulation method and device for relaxor ferroelectric dielectric property and storage medium

    CN120387326A