Methods for improving etching defects
By performing baking heat treatment before etching of the metal layer and strengthening drying treatment after etching, the rat bite defect caused by wet etching is solved, and the yield and quality of the product are improved.
Patent Information
- Application Number
- CN202210876118.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-07-25
AI Technical Summary
In the prior art, wet etching of Taichung aluminum by metal etching can easily cause "rat bite defects", reduce the critical dimension of line width and lead to product yield loss.
Baking heat treatment is carried out before etching of the metal layer to release thermal stress, and drying is strengthened after etching to remove residual acid in the cavity caused by the reaction between metal layers, and inter-metallic inter-metallic by adjusting the photoresist removal machine temperature is formed Compounds, residual solution is removed using isopropanol vapor dryer and ashing process.
It effectively improves the rat bite defects, improves the product yield, and prevents further defects caused by acid etching.
Smart Images

Figure CN115159449B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a method for improving etching defects. Background Art
[0002] MEMS sensor, or Microelectro Mechanical Systems, is a multidisciplinary frontier research field developed on the basis of microelectronics technology. After more than 40 years of development, it has become one of the major scientific and technological fields that has attracted worldwide attention. It involves multiple disciplines and technologies such as electronics, mechanics, materials, physics, chemistry, biology, and medicine, and has broad application prospects. At present, hundreds of products including micro pressure sensors, accelerometers, micro inkjet print heads, and digital micromirror displays have been developed, among which MEMS sensors account for a considerable proportion. MEMS sensors are new sensors manufactured using microelectronics and micromachining technology. Compared with traditional sensors, it has the characteristics of small size, light weight, low cost, low power consumption, high reliability, suitable for mass production, easy integration, and intelligent realization. At the same time, the characteristic size in the micrometer range enables it to complete functions that some traditional mechanical sensors cannot achieve.
[0003] For MEMS accelerometer products, in the prior art, a layer of photoresist is formed on the aluminum layer on the substrate, and the pattern on the aluminum layer is defined by photolithography. Then, the photoresist layer is opened and the exposed aluminum layer is removed by wet etching. Then, the wet-etched substrate is subjected to an ashing process and water-based cleaning. The wet etching of aluminum in the metal etching station is prone to cause the following problems: Figure 1 , 2 The “rat bite defect” shown here will reduce the critical dimension of line width and cause product yield loss.
[0004] In order to solve the above problems, a new method for improving etching defects is needed. Summary of the invention
[0005] In view of the shortcomings of the prior art described above, the purpose of the present invention is to provide a method for improving etching defects, which is used to solve the problem that wet etching of aluminum in a metal etching station in the prior art is prone to cause "rat bite defects", which will reduce the critical dimension of the line width and cause loss of product yield.
[0006] To achieve the above objectives and other related objectives, the present invention provides a method for improving etching defects, comprising:
[0007] Step 1: providing a substrate, on which a first metal layer and a second metal layer formed on the first metal layer are formed;
[0008] Step 2, forming a photoresist layer on the second metal layer, photolithographically opening a portion of the photoresist layer so that the second metal layer thereunder is exposed, and then adjusting the temperature of the photoresist removal machine so that an intermetallic compound is formed at the contact surface between the exposed second metal layer and the first metal layer thereunder;
[0009] Step 3, removing the exposed second metal layer by wet etching, and then drying the substrate to remove the solution on the first and second metal layers;
[0010] Step 4: removing the photoresist layer by an ashing process, so that the residual solution on the first and second metal layers is removed;
[0011] Step five: cleaning the substrate, and then drying the substrate.
[0012] Preferably, the substrate in step one is a silicon substrate.
[0013] Preferably, in step 1, the material of the first metal layer is titanium.
[0014] Preferably, in step 1, the material of the second metal layer is aluminum.
[0015] Preferably, the intermetallic compound in step 2 is TiAL3.
[0016] Preferably, the photoresist removal machine in step 2 is a deep ultraviolet light processing machine.
[0017] Preferably, in step 2, the temperature of the deep ultraviolet light processing machine is adjusted to 150 to 180 degrees Celsius.
[0018] Preferably, in step three, the solution is removed by using an isopropanol vapor dryer, and then nitrogen is introduced into the isopropanol vapor dryer to exhaust the gas therein.
[0019] Preferably, the temperature of the electric furnace used in the ashing process in step 4 is 250 degrees Celsius.
[0020] Preferably, the gases introduced into the electric furnace used in the ashing process in step 4 are H2N2 and O2.
[0021] Preferably, in step 4, 200 to 400 SCCM of H2N2 and 2500 to 3500 SCCM of O2 are introduced into the electric furnace.
[0022] Preferably, the power of the electric furnace used in the ashing process in step 4 is 1000 to 1400 watts.
[0023] As described above, the method for improving etching defects of the present invention has the following beneficial effects:
[0024] The present invention performs baking heat treatment before etching the metal layer to release thermal stress; and strengthens drying treatment after etching to remove residual acid in the cavity generated by the reaction between the metal layers, preventing further etching reaction of the residual acid, thereby improving mouse bite defects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Shown is a schematic diagram of a rat bite defect in the prior art;
[0026] Figure 2 Shown is a schematic diagram of a rat bite defect in the prior art;
[0027] Figure 3 Shown is a schematic diagram of the improvement of rat bite defects according to the present invention;
[0028] Figure 4 Shown is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION
[0029] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0030] See also Figure 4 The present invention provides a method for improving etching defects, comprising:
[0031] Step 1, providing a substrate, on which a first metal layer and a second metal layer formed on the first metal layer are formed;
[0032] In an embodiment of the present invention, the substrate in step 1 is a silicon substrate.
[0033] In an embodiment of the present invention, the material of the first metal layer in step 1 is titanium.
[0034] In an embodiment of the present invention, the material of the second metal layer in step 1 is aluminum.
[0035] Step 2: using a photoresist removal machine to form a photoresist layer on the second metal layer, photolithography to open part of the photoresist layer, and then through exposure, film erection, development, baking and other steps, the second metal layer below is exposed, and then the substrate after photolithography is transferred to the photoresist removal machine, and the temperature of the photoresist removal machine is adjusted to form an intermetallic compound at the contact surface of the first and second metal layers at the exposed part, that is, before the second metal layer is etched, the thermal stress of the metal layer can be released by baking heat treatment;
[0036] In an embodiment of the present invention, the intermetallic compound in step 2 is TiAL3, which is formed by the reaction of a titanium metal layer and an aluminum metal layer.
[0037] In an embodiment of the present invention, the photoresist removal machine in step 2 is a deep ultraviolet light processing (UV curing) machine. The UV curing machine is a device that uses a UV light source to cure UV coatings, reacts chemically with the photosensitizer in the UV coating, and dries and cures instantly.
[0038] In an embodiment of the present invention, in step 2, the temperature of the deep ultraviolet light processing machine is adjusted to 150 to 180 degrees Celsius.
[0039] Step 3: Remove the exposed second metal layer by wet etching. Drying is the last step of wet cleaning and greatly affects the yield of the wafer. Since the reaction between the metal layers will form voids, the acid remaining in the voids will continue to etch to form mouse bite defects. After that, the substrate is dried to remove the solution on the first and second metal layers to prevent the acid from continuing to react.
[0040] In an embodiment of the present invention, the wet cleaning below 0.35 μm in the wafer factory adopts the drying method of heated isopropyl alcohol vapor mist, which is commonly referred to as the IPA drying method. IPA drying uses intermolecular forces to remove water molecules. Isopropyl alcohol is atomized to form mist, and its molecules are more easily carried into the channel of the device by hot nitrogen, thereby taking away the water molecules in the channel to achieve the effect of drying. This method not only greatly reduces the occurrence of water vapor residue, but also reduces the adsorption of particles on the surface of the wafer. In step three, an isopropyl alcohol vapor dryer is used to remove the solution, and then nitrogen is introduced into the isopropyl alcohol vapor dryer to discharge the gas therein. Hot N2 and IPA pass through the IPA atomizer to quickly form IPA vapor and spray it onto the surface of the wafer to achieve drying. This method has sufficient IPA concentration to form an IPA vapor block, without high temperature danger, and dries faster.
[0041] Step 4, removing the photoresist layer by an ashing process, and adjusting the parameters of the electric furnace in the ashing process so that the residual solution on the first and second metal layers is removed in this step;
[0042] In an embodiment of the present invention, the temperature of the electric furnace used in the ashing process in step 4 is 250 degrees Celsius.
[0043] In an embodiment of the present invention, the gases introduced into the electric furnace used for the ashing process in step 4 are H2N2 and O2.
[0044] In an embodiment of the present invention, in step 4, 200 to 400 SCCM of H2N2 and 2500 to 3500 SCCM of O2 are introduced into the electric furnace.
[0045] In an embodiment of the present invention, the power of the electric furnace used in the ashing process in step 4 is 1000 to 1400 watts.
[0046] Step five: cleaning the substrate and then drying the substrate.
[0047] In an embodiment of the present invention, the substrate after wet cleaning may be dried in an electric furnace.
[0048] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner. Therefore, the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0049] In summary, the present invention performs a baking heat treatment before etching the metal layer to release thermal stress; and strengthens the drying process after etching to remove the residual acid in the cavity generated by the reaction between the metal layers, and prevents the further etching reaction of the residual acid, thereby improving the mouse bite defect. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.
[0050] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for improving etching defects, characterized in that: At least: Step 1: providing a substrate, on which a first metal layer and a second metal layer formed on the first metal layer are formed; Step 2: forming a photoresist layer on the second metal layer, photolithographically opening a portion of the photoresist layer so that the second metal layer thereunder is exposed, and then adjusting the temperature of the photoresist removal machine to 150 to 180 degrees Celsius so that an intermetallic compound is formed at the contact surface between the exposed second metal layer and the first metal layer thereunder; Step 3, removing the exposed second metal layer by wet etching, and then drying the substrate to remove the solution on the first and second metal layers; Step 4: removing the photoresist layer by an ashing process, wherein the gases introduced into the electric furnace in the ashing process are H2N2 and O2, 200 to 400 SCCM of H2N2 and 2500 to 3500 SCCM of O2 are introduced into the electric furnace, and the power of the electric furnace in the ashing process is 1000 to 1400 watts, so that the residual solution on the first and second metal layers is removed; Step five: cleaning the substrate, and then drying the substrate.
2. The method for improving etching defects according to claim 1, characterized in that: The substrate in step one is a silicon substrate.
3. The method for improving etching defects according to claim 1, characterized in that: In step 1, the material of the first metal layer is titanium.
4. The method for improving etching defects according to claim 3, characterized in that: In step 1, the material of the second metal layer is aluminum.
5. The method for improving etching defects according to claim 4, characterized in that: The intermetallic compound in step 2 is TiAL3.
6. The method for improving etching defects according to claim 1, characterized in that: The photoresist removal machine in step 2 is a deep ultraviolet light processing machine.
7. The method for improving etching defects according to claim 1, characterized in that: In step 3, the solution is removed by using an isopropanol vapor dryer, and then nitrogen is introduced into the isopropanol vapor dryer to exhaust the gas therein.
8. The method for improving etching defects according to claim 1, characterized in that: The temperature of the electric furnace used in the ashing process in step 4 is 250 degrees Celsius.
Citation Information
Patent Citations
Isopropanol steam cleaning and drying device
CN101844140A
Method for drying wafer
CN101957124A
Method for removing photoinduced resist layer on semiconductor device structure
CN102386088A
Method for effectively reducing water mark defects
CN102437037A
Metal wet etching method without metal wire cut problem
CN103426750A