A method for alloy welding of power chip on T-shaped tube shell

Through the eutectic sintering welding and hydrogen reduction of lead-indium silver solder sheets, combined with the special heating mold design, the problems of heat dissipation difference and insufficient bonding strength of power chips on T-shaped shells in the prior art are solved, and high Strength welding and good heat dissipation effect meet the high-quality reliability requirements in the military aerospace field.

CN115172190BActive Publication Date: 2024-12-06JINZHOU 777 MICROELECTRONICS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210687016.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-17
Publication Date
2024-12-06
Estimated Expiration
2042-06-17

AI Technical Summary

Technical Problem

The bonding method of existing power chips on T-shaped shells has poor heat dissipation effect and average bonding strength, which cannot meet the high-quality reliability requirements of electronic components in the military aerospace field.

Method used

Lead-indium silver solder sheets are used for eutectic sintering and welding. By raising the temperature multiple times in the eutectic welding furnace, hydrogen is generated by heating the constant temperature and decomposing it into the eutectic welding furnace. Combined with the design of a special heating mold, it ensures that the solder is fully melted and has high bonding strength.

Benefits of technology

It achieves high-strength welding and good heat dissipation effects, is suitable for long-term storage requirements in the military aerospace field, and improves the quality reliability of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115172190B_ABST
    Figure CN115172190B_ABST
Patent Text Reader

Abstract

A method for alloy welding of a power chip on a T-shaped tube shell comprises the following steps: placing the T-shaped tube shell in acetone for ultrasonic cleaning for 15 minutes to remove oil and impurities on the surface of the tube shell, then dehydrating it with anhydrous ethanol, and drying it for standby use; selecting a lead-indium-silver solder sheet as solder, the size of which is consistent with the size of the power chip to be welded; inserting the T-shaped tube shell to be welded into the mounting holes of a special heating mold respectively, embedding the positioning end of the outer edge of the upper end of the T-shaped tube shell into the positioning notch at the upper end of the mounting hole, placing a lead-indium-silver solder sheet of appropriate size on the chip bonding area on the top surface of the T-shaped tube shell, and placing the power chip to be welded on the lead-indium-silver solder sheet; placing the special heating mold with the T-shaped tube shell, the lead-indium-silver solder sheet and the power chip placed in a programmable eutectic welding furnace for sintering welding. The device prepared by this method has high welding strength, good heat dissipation, and long storage time, and can meet the requirements of electronic components in the military aerospace field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electronic component manufacturing, and in particular to an alloy welding method for a power chip on a T-shaped tube shell. Background Art

[0002] In recent years, electronic components, as an important basic resource for the quality reliability of the whole machine, have been highly valued. For some special purposes such as the whole machine system in the military and aerospace fields, due to their special working environment, the requirements for the long-term quality reliability of electronic components are becoming higher and higher. Some power devices have higher and higher requirements for heat dissipation, and also put forward higher requirements for the miniaturization of packaging.

[0003] At present, power chips are usually fixed on T-shaped tube shells using conductive organic adhesives, which have poor heat dissipation effect, general bonding strength, and short storage time, and are not suitable for the requirements of electronic components in the military aerospace field. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an alloy welding method for a power chip on a T-shaped tube shell. The device prepared by this method has high welding strength, good heat dissipation, and long storage time, and can meet the requirements of the military aerospace field for electronic components.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for alloy welding of a power chip on a T-shaped tube shell comprises the following steps:

[0007] 1. Place the T-shaped tube shell in acetone and ultrasonically clean it for 15 minutes to remove the oil and impurities on the surface of the tube shell, then dehydrate it with anhydrous ethanol and blow it dry for later use;

[0008] 2. Select lead-indium-silver solder sheet as solder, and the size of the solder should be consistent with the size of the power chip to be soldered;

[0009] 3. Insert the T-shaped tube shells to be welded into the mounting holes of the special heating mold respectively, embed the positioning end of the upper outer edge of the T-shaped tube shell into the positioning notch at the upper end of the mounting hole, place the lead-indium-silver solder sheet of appropriate size on the chip bonding area on the top surface of the T-shaped tube shell, and place the power chip to be welded on the lead-indium-silver solder sheet;

[0010] 4. Place the dedicated heating mold with the T-shaped tube shell, lead-indium-silver solder sheet and power chip into the programmable eutectic soldering furnace for sintering and welding. The specific operations are as follows:

[0011] 4.1. First, evacuate the furnace for 80 to 120 seconds to make the vacuum degree less than 500Pa; then fill the eutectic furnace with nitrogen for 100 to 120 seconds, and control the nitrogen filling volume to 15 to 20 slm; repeat this process twice to replace the air in the eutectic furnace with nitrogen;

[0012] 4.2. Start heating and heating for 120s until the temperature in the furnace reaches 220℃. At the same time, control the nitrogen filling volume to 15slm. After reaching 220℃, keep the temperature constant for 60s. At this time, introduce formic acid at a flow rate of 10slm to decompose the formic acid to produce hydrogen. The reduction effect of hydrogen is used to improve the quality of eutectic welding.

[0013] 4.3. Restart heating and keep the temperature constant for 200 seconds after the temperature reaches 350℃, while continuing to introduce formic acid; after the temperature is constant, heat again until the temperature reaches 410℃, and keep the temperature constant for 30-50 seconds to fully melt the lead-indium-silver solder sheet; then stop introducing formic acid, evacuate, and keep the temperature constant for another 60 seconds to complete the eutectic welding;

[0014] 4.4. After welding, introduce nitrogen to start cooling. When the temperature drops below 70 degrees, open the chamber door of the eutectic welding furnace and take out the welded components.

[0015] As a further preference, the dedicated heating mold includes a heat-conducting block with a rectangular shape, the thickness of the heat-conducting block is slightly larger than the length of the T-shaped tube shell, and a plurality of the mounting holes are evenly distributed on the heat-conducting block. The mounting holes are stepped, and the major diameter of the upper end thereof is matched with the diameter clearance of the outer edge of the upper end of the T-shaped tube shell. The positioning notches are respectively arranged at the inner edge of the upper end of the mounting hole to realize the positioning and placement of the T-shaped tube shell.

[0016] As a further preference, the heat-conducting block is an aluminum block to facilitate processing and heat conduction.

[0017] As a further preference, the number of mounting holes on the heat conducting block is five.

[0018] As a further preference, in step 4.3, the heating is restarted for 150 to 200 seconds to reach a temperature of 350°C; and the heating is repeated for 80 to 100 seconds to reach a temperature of 410°C.

[0019] The beneficial effects of the present invention are:

[0020] 1. The power chip is welded to the T-shaped tube shell by using the eutectic sintering method using the lead-indium-silver solder sheet. By heating and maintaining the temperature three times in the eutectic soldering furnace, the special heating mold can fully absorb the heat to ensure that the lead-indium-silver solder sheet placed on the T-shaped tube shell is fully melted; the formic acid introduced during the heating process in the eutectic soldering furnace decomposes to produce hydrogen, and the reducing effect of hydrogen can improve the eutectic welding quality; the process is reasonable and the operation is simple, which solves the problem of eutectic sintering of the T-shaped tube shell and the power chip together, is suitable for industrial production, and greatly improves the quality reliability of military products.

[0021] 2. Compared with traditional organic adhesives, the chips welded by this method have high bonding strength, good heat dissipation, and can be stored for a long time without failure, which can meet the requirements of electronic components in the military aerospace field. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the structure of the T-shaped tube shell after welding the power chip of the present invention;

[0023] Figure 2 yes Figure 1 A top view of

[0024] Figure 3 It is a structural schematic diagram of the special heating mold of the present invention.

[0025] Figure 4 yes Figure 3 AA section view. DETAILED DESCRIPTION

[0026] The specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings.

[0027] The present invention relates to an alloy welding method for a power chip on a T-shaped tube shell, comprising the following steps:

[0028] 1. Place the T-shaped tube shell 1 in acetone for ultrasonic cleaning for 15 minutes to remove oil and impurities on the surface of the tube shell, then dehydrate it with anhydrous ethanol, blow dry it and set it aside;

[0029] 2. Select lead-indium-silver solder sheet as solder, and the size of the solder should be consistent with the size of the power chip 3 to be soldered;

[0030] 3. Insert the pins 101 of the T-shaped tube shell 1 to be welded into the mounting holes of the special heating mold respectively, embed the positioning end of the upper outer edge of the T-shaped tube shell 1 into the positioning notch at the upper end of the mounting hole, place the lead indium silver solder sheet 2 of appropriate size on the chip bonding area on the top surface of the T-shaped tube shell 1, and place the power chip 3 to be welded on the lead indium silver solder sheet 2;

[0031] 4. Place the dedicated heating mold with the T-shaped tube shell 1, lead-indium-silver solder sheet 2 and power chip 3 into the programmable eutectic soldering furnace for sintering and soldering. The specific operations are as follows:

[0032] 4.1. First, evacuate the furnace for 80 to 120 seconds to make the vacuum less than 500Pa; then fill the eutectic furnace with nitrogen for 100 to 120 seconds, and control the nitrogen filling volume to 15 to 20 slm; repeat this process twice to replace the air in the eutectic furnace with nitrogen to ensure welding quality and improve heat transfer efficiency;

[0033] 4.2. Start heating up, heating up time 120s, make the temperature in the furnace reach 220℃, and control the nitrogen filling volume to 15slm; after reaching 220℃, keep the temperature constant for 60s, at this time, introduce formic acid, the flow rate is 10slm, so that the formic acid decomposes to produce hydrogen, and the reduction effect of hydrogen is used to make the eutectic welding quality better;

[0034] 4.3. Restart heating for 150-200 seconds. After heating to 350℃, keep the temperature constant for 200 seconds to allow the special heating mold to gradually absorb heat, while keeping the formic acid flowing in. After the constant temperature ends, heat again for 80-100 seconds until the temperature reaches 410℃. Keep the temperature constant for 30-50 seconds to fully melt the lead-indium-silver solder sheet. Then stop passing formic acid, evacuate, and keep the temperature constant for another 60 seconds to complete the eutectic welding.

[0035] 4.4. After welding, introduce nitrogen to start cooling. When the temperature drops below 70 degrees, open the eutectic welding furnace chamber door and take out the welded components. Figure 1 and Figure 2 shown.

[0036] like Figure 3 and Figure 4 As shown, the special heating mold includes a heat conducting block 4 with a rectangular shape, the thickness of which is slightly greater than the length of the T-shaped tube shell 1, and a plurality of mounting holes 401 are evenly processed on the heat conducting block 4. Five mounting holes 401 are used as an example in this embodiment. The mounting holes 401 are stepped, and the large diameter of the upper end thereof is matched with the diameter clearance of the outer edge of the upper end of the T-shaped tube shell 1. The positioning notches 402 are respectively provided at the inner edges of the upper ends of the mounting holes 401 to realize the positioning and placement of the T-shaped tube shell 1. The heat conducting block 4 is an aluminum block for easy processing and heat conduction.

[0037] Five devices were selected for shear force testing after the power chips were soldered using this method. The test data were completely qualified. Under a 30x microscope, 100% of the solder remained. The test data is shown in the following table.

[0038] serial number <![CDATA[Chip area (mm 2 )]]> Shear strength(kg) in conclusion 1# 4.1 12.1 qualified 2# 4.1 13.9 qualified 3# 4.1 11.1 qualified 4# 4.1 12.6 qualified 5# 4.1 12.9 qualified

[0039] It can be seen from the above table that the shear force data of the present invention fully complies with the standard requirements of GJB 548B-2005 "Test Methods and Procedures for Microelectronic Devices".

[0040] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for alloy welding of a power chip on a T-shaped tube shell, It is characterized in that The steps are as follows: (1) Place the T-shaped tube shell in acetone for ultrasonic cleaning for 15 minutes to remove oil and impurities on the surface of the tube shell, then dehydrate it with anhydrous ethanol, blow dry it and set it aside; (2) Select lead-indium-silver solder sheet as solder, and the size of the solder should be consistent with the size of the power chip to be soldered; (3) Insert the T-shaped tube shells to be welded into the mounting holes of the special heating mold respectively, insert the positioning end of the upper outer edge of the T-shaped tube shell into the positioning notch at the upper end of the mounting hole, place the lead indium silver solder sheet of appropriate size on the chip bonding area on the top surface of the T-shaped tube shell, and place the power chip to be welded on the lead indium silver solder sheet; (4) Place the dedicated heating mold with the T-shaped tube shell, lead-indium-silver solder sheet and power chip in a programmable eutectic soldering furnace for sintering and soldering. The specific operations are as follows: 4.

1. First, evacuate the furnace for 80 to 120 seconds to make the vacuum degree less than 500Pa; then fill the eutectic furnace with nitrogen for 100 to 120 seconds, and control the nitrogen filling volume to 15 to 20 slm; repeat this process twice to replace the air in the eutectic furnace with nitrogen; 4.

2. Start heating and heating for 120s until the temperature in the furnace reaches 220℃. At the same time, control the nitrogen filling volume to 15slm. After reaching 220℃, keep the temperature constant for 60s. At this time, introduce formic acid at a flow rate of 10slm to decompose the formic acid to produce hydrogen. The reduction effect of hydrogen is used to improve the quality of eutectic welding. 4.

3. Restart heating and keep the temperature constant for 200 seconds after the temperature reaches 350℃, while continuing to introduce formic acid; after the temperature is constant, heat again until the temperature reaches 410℃, and keep the temperature constant for 30-50 seconds to fully melt the lead-indium-silver solder sheet; then stop introducing formic acid, evacuate, and keep the temperature constant for another 60 seconds to complete the eutectic welding; 4.

4. After welding, introduce nitrogen to start cooling. When the temperature drops below 70 degrees, open the chamber door of the eutectic welding furnace and take out the welded components.

2. The alloy welding method for a power chip on a T-shaped tube shell according to claim 1, Features: The special heating mold includes a heat-conducting block with a rectangular shape. The thickness of the heat-conducting block is slightly larger than the length of the T-shaped tube shell. A plurality of the mounting holes are evenly distributed on the heat-conducting block. The mounting holes are stepped. The large diameter of the upper end thereof is matched with the diameter clearance of the outer edge of the upper end of the T-shaped tube shell. The positioning notches are respectively arranged at the inner edges of the upper ends of the mounting holes to realize the positioning and placement of the T-shaped tube shell.

3. The alloy welding method for a power chip on a T-shaped tube shell according to claim 2, Features: The heat conducting block is an aluminum block for ease of processing and heat conduction.

4. The alloy welding method for a power chip on a T-shaped tube shell according to claim 2 or 3, Features: The number of mounting holes on the heat conducting block is five.

5. The alloy welding method for a power chip on a T-shaped tube shell according to claim 1, Features: In step 4.3, the heating is restarted for 150 to 200 seconds to reach a temperature of 350°C; the heating is repeated for 80 to 100 seconds to reach a temperature of 410°C.

Citation Information

Patent Citations

  • Automatic eutectic welding method of power chip and pickup suction head

    CN111987010A

  • Method for solving SMD tube shell bonding point gold-aluminum system

    CN112151400A

  • Chip low-vacuum alloy welding method for nickel-plated tube base

    CN112687555A