A method for preparing carbon paper for fuel cell gas diffusion layer

By combining acrylonitrile pulp and modified micronized expanded graphite with carbon fiber, the problems of low strength and difficult porosity control of carbon paper for fuel cells were solved, and carbon paper with high strength, high conductivity and uniform pore structure was prepared, which improved the electron transmission efficiency and output power of fuel cells.

CN115172767BActive Publication Date: 2024-11-01ZHEJIANG SCI-TECH UNIV

Patent Information

Application Number
CN202210876559.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-25
Publication Date
2024-11-01
Estimated Expiration
2042-07-25

AI Technical Summary

Technical Problem

Existing fuel cell gas diffusion layer carbon paper has low strength, high brittleness, and difficult-to-control porosity, resulting in low electron transport efficiency and insufficient output power.

Method used

High-strength, high-conductivity carbon paper was prepared by combining acrylonitrile pulp and modified micro-refined expanded graphite with carbon fiber, through high-pressure reaction, subcritical liquid-phase oxidation technology, and latex modification.

Benefits of technology

It significantly improved the strength and conductivity of carbon paper, regulated the pore structure, enhanced its flexibility and toughness, and improved the overall performance of carbon paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003762595220000101
    Figure BDA0003762595220000101
Patent Text Reader

Abstract

The invention relates to a method for preparing carbon paper for a fuel cell gas diffusion layer. In the method, acrylic pulp is first configured into a slurry, reacted with a modifying liquid under certain conditions, and washed and dried with a weak acid and clean water after the reaction is completed to obtain modified acrylic pulp. Afterwards, an expanded graphite floating liquid is configured, and it is cut by a high-speed disperser to obtain micronized expanded graphite. Oxidation is performed under subcritical conditions, and washing and filtering are performed to obtain modified micronized expanded graphite. Modified acrylic pulp and carbon fiber are configured into a mixed slurry, and modified micronized expanded graphite, polyethylene oxide, aluminum sulfate and latex are added to obtain a stabilized mixed slurry. The mixed slurry is sheet-formed and dried to obtain a carbon paper precursor. The carbon paper precursor is then immersed in a phenolic resin ethanol solution and dried, and finally hot pressed and carbonized to obtain carbon paper. The carbon paper prepared by the present invention has the advantages of ultra-high strength, excellent conductivity and uniform pore structure, and the preparation method is fast and stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cell preparation, and in particular relates to a method for preparing carbon paper for a fuel cell gas diffusion layer. Background Art

[0002] A fuel cell is a device that converts the chemical energy of a fuel into clean electrical energy through an electrochemical reaction. Unlike traditional batteries, it cannot store energy, but is similar to a generator in that it converts the chemical energy of a fuel into electrical energy. It is an energy conversion device. Fuel cells have many advantages, such as higher energy conversion efficiency, lower pollution and noise, higher operating reliability, and more fuel options.

[0003] As a type of fuel cell, the proton exchange membrane fuel cell has the advantages of small size and weight, high energy density, fast startup speed, safe and reliable operation, etc. It is the most promising type of fuel cell. It consists of bipolar plates, gaskets, gas diffusion layers, catalyst layers and proton exchange membranes. The gas diffusion layer is usually composed of porous conductive materials. Its function is to transport reaction gases, discharge product water, support the catalyst layer, collect current, etc., to achieve the redistribution of product water and reaction gases. At present, common gas diffusion layers include carbon cloth, carbon paper and carbon black paper, especially carbon paper as a gas diffusion layer is more common.

[0004] Carbon paper needs to have the following properties in proton exchange membrane fuel cells: (1) Certain strength. It needs to have high mechanical strength and appropriate flexibility to provide structural support for the fuel cell. (2) Appropriate pore size structure. It is used for gas transport during fuel cell operation and the discharge of water after electrochemical reaction to ensure the smooth progress of electrochemical reaction. (3) Low resistivity. It is conducive to electron transport in carbon paper, reduces the contact resistance between carbon paper and other components, and ensures the output power of the fuel cell. (4) Appropriate thickness and apparent density. Improve the ability of carbon paper to transport gas and water. (5) Smooth surface. Reduce the contact resistance between the gas diffusion layer and the catalyst layer to ensure the stable output power of the proton exchange membrane fuel cell.

[0005] Chinese patent CN1185736C describes a method for preparing carbon paper, in which the raw material used is pure carbon fiber, which is then dispersed in an aqueous phase using a dispersant, and then directly made into paper. Although this method can greatly retain the content of carbon fiber, the strength of the resulting carbon paper is extremely low and cannot be applied in practice. According to patent CN110512459B, the raw materials used are viscose fiber, cellulose nanofibrils and carbon fiber. The strength of the carbon paper precursor can be improved by coordinating with other additives such as surfactants, polyethylene oxide and polyvinyl alcohol solution, but the strength of the carbon paper is not significantly improved due to the low residual carbon rate of viscose fiber and cellulose nanofibrils, and the porosity of the carbon paper is not easy to adjust. Although Chinese patent CN113066996B proposes a method for preparing porous carbon paper, and the porosity and mechanical properties of the carbon paper are adjusted, due to the introduction of natural inorganic mineral fibers, the resistivity of the carbon paper is greatly improved, which reduces the electron transmission efficiency and fuel cell output power in the carbon paper.

[0006] Therefore, developing a method for manufacturing fuel cell gas diffusion layer carbon paper with high strength, high conductivity, good air permeability, stable quality and simple process has become a key issue that needs to be solved urgently. Summary of the invention

[0007] The technical problem to be solved by the present invention is as follows: In view of the problems that the carbon paper used for the gas diffusion layer of fuel cells is currently brittle, has low strength and is difficult to control the gaps, a method for preparing the carbon paper for the gas diffusion layer of fuel cells is proposed.

[0008] The technical solution adopted by the present invention to solve the technical problem is:

[0009] (1) Add acrylic pulp to water to prepare a slurry with a concentration of 2%-20%, then beat it to prepare a slurry with a beating degree of 30-80°SR, and then dehydrate it for standby use. Prepare an alkali solution with a concentration of 2%-12%, and then add 10%-30% of anhydrous ethanol relative to the mass of the alkali solution to prepare a modified liquid. Add the prepared modified liquid to the beaten acrylic pulp, and react it in a high-pressure reactor at a pressure of 50-200kPa and a temperature of 50℃-80℃ for 5-20min. Finally, wash it with weak acid and clean water and dry it to obtain modified acrylic pulp.

[0010] (2) Mixing the expanded graphite with water to prepare an expanded graphite floating liquid with a mass ratio of 1%-5%, cutting it with a high-speed disperser to obtain micronized expanded graphite. Then, adding 15-25 times of concentrated sulfuric acid and 1-5 times of oxide relative to the mass of the expanded graphite to the expanded graphite floating liquid, reacting for 10-30 minutes under subcritical conditions to obtain an expanded graphite suspension. Finally, washing and filtering with hydrogen peroxide, sodium hydroxide and water to obtain modified micronized expanded graphite.

[0011] (3) Add modified acrylic pulp and carbon fiber into water to prepare a mixed slurry with a concentration of 0.05%-0.2%. Then add 2%-10% of modified micronized expanded graphite relative to the mass of carbon fiber, 0.1%-0.2% of polyethylene oxide, 3%-15% of aluminum sulfate and 5%-25% of latex relative to the total fiber mass. Stir evenly to obtain a stabilized mixed slurry. Sheet the mixed slurry into a mold and dry it to obtain a carbon paper precursor. Then, immerse the carbon paper precursor in a phenolic resin ethanol solution and dry it, and finally obtain a carbon paper for fuel cells through hot pressing and carbonization.

[0012] Furthermore, the alkali solution in step (1) is one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide.

[0013] Furthermore, the weak acid in step (1) is one or more of formic acid, acetic acid and citric acid.

[0014] Furthermore, the expanded graphite described in step (2) is prepared from expandable graphite of 200-2000 mesh.

[0015] Furthermore, the size of the micronized expanded graphite in step (2) is between 500 nanometers and 70 micrometers.

[0016] Furthermore, the oxide in step (2) is one or more of potassium permanganate and potassium dichromate.

[0017] Furthermore, the subcritical temperature of step (2) is 493-593K and the pressure is 5-15MPa.

[0018] Furthermore, the carbon fiber described in step (3) is one or more of polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber and viscose-based carbon fiber.

[0019] Furthermore, the carbon fiber described in step (3) has a diameter of 3-15 μm and a length of 1-7 mm.

[0020] Furthermore, the ratio of the modified acrylic pulp to carbon fiber in step (3) is 1:1-20.

[0021] Furthermore, the latex described in step (3) is one or more of styrene-butadiene latex, nitrile-butadiene latex and natural latex.

[0022] Furthermore, the hot pressing treatment temperature in step (3) is 120°C-180°C, the pressure is 2-15MPa, and the time is 5-25min.

[0023] Furthermore, the carbonization conditions in step (3) are in an inert atmosphere, the carbonization temperature is 800° C.-1600° C., and the carbonization time is 20-200 min.

[0024] Furthermore, the carbonization conditions in step (3) are one or more of nitrogen and argon.

[0025] Furthermore, the carbon paper in step (3) has a basis weight of 30-150 g / m 2 .

[0026] Beneficial effects of the present invention:

[0027] (1) The reinforcing fiber used in the present invention is acrylic pulp, and the modified acrylic pulp is prepared by hydrophilic modification on its surface. The modified acrylic pulp overcomes the hydrophobicity of the original fiber, enhances water wettability, improves its suspension stability in water, and also improves the bonding strength between fibers.

[0028] (2) The present invention uses subcritical liquid phase oxidation technology to prepare modified micronized expanded graphite, and the preparation method used is simple and efficient. It not only retains the molecular structure of natural graphite and the porous characteristics of expanded graphite, but also improves its water-wetting dispersibility.

[0029] (3) The present invention utilizes the branching structure and bending properties of acrylic pulp to form an interwoven interconnected state between carbon fibers, and uses modified micronized expanded graphite to increase locking binding sites between fibers, thereby significantly increasing the strength of carbon paper.

[0030] (4) The present invention introduces modified micronized expanded graphite to increase the pore channels between carbon papers, making it easy to regulate the pore structure and water vapor management ability of carbon paper.

[0031] (5) The present invention adsorbs modified expanded graphite on acrylic pulp, and after carbonization, the surface resistance and contact resistance of carbon paper are greatly reduced, and the conductive performance is greatly improved.

[0032] (6) The present invention significantly improves the softness of carbon paper by introducing the self-slip properties of expanded graphite layers and latex, making it less likely to be bent and damaged during preparation and transportation.

[0033] (7) The carbon paper of the present invention has the advantages of ultra-high strength, excellent conductivity and uniform pore structure, and the preparation method is fast and stable, and has good practical application value. DETAILED DESCRIPTION

[0034] Technical solution of the present invention:

[0035] (1) Add acrylic pulp to water to prepare a slurry with a concentration of 2%-20%, then beat it to prepare a slurry with a beating degree of 30-80°SR, and then dehydrate it for standby use. Prepare an alkali solution with a concentration of 2%-12% (which can be sodium hydroxide, potassium hydroxide and lithium hydroxide), and then add 10%-30% of anhydrous ethanol relative to the mass of the alkali solution to prepare a modified liquid. Add the prepared modified liquid to the beaten acrylic pulp, and react it in a high-pressure reactor at a pressure of 50-200kPa and a temperature of 50℃-80℃ for 5-20min. Finally, wash it with a weak acid (which can be formic acid, acetic acid and citric acid) and clean water and dry it to obtain a modified acrylic pulp.

[0036] (2) Mixing the expanded graphite with water to form an expanded graphite floating liquid with a mass ratio of 1%-5%, cutting it with a high-speed disperser to obtain a micronized expanded graphite with a size of 500 nanometers-70 micrometers. Then, adding 15-25 times of concentrated sulfuric acid and 1-5 times of oxide (potassium permanganate and potassium dichromate) relative to the mass of the expanded graphite to the expanded graphite floating liquid, reacting for 10-30 minutes under subcritical conditions of a temperature of 493-593K and a pressure of 5-15MPa to obtain an expanded graphite suspension. Finally, washing and filtering with hydrogen peroxide, sodium hydroxide and water to obtain modified micronized expanded graphite.

[0037] (3) Add modified acrylic pulp and carbon fibers with a diameter of 3-15 μm and a length of 1-7 mm (which may be polyacrylonitrile-based carbon fibers, asphalt-based carbon fibers and viscose-based carbon fibers) to water at a ratio of 1:1-20 to prepare a mixed slurry with a concentration of 0.05%-0.2%. Then add 2%-10% of modified micronized expanded graphite relative to the mass of the carbon fibers. Then add 0.1%-0.2% of polyethylene oxide, 3%-15% of aluminum sulfate and 5%-25% of latex (which may be styrene-butadiene latex, nitrile latex and natural latex) relative to the mass of the total fibers (modified acrylic pulp + carbon fibers). Stir evenly to obtain a stabilized mixed slurry. Sheet the mixed slurry into a mold and dry it to obtain a carbon paper precursor. The carbon paper precursor is then immersed in a phenolic resin ethanol solution and dried, and finally subjected to hot pressing at a temperature of 120°C-180°C, a pressure of 2-15 MPa, a time of 5-25 min, and carbonization at a temperature of 800°C-1600°C, a time of 20-200 min, to obtain a carbon paper with a weight of 30-150 g / m 2 A carbon paper for use in fuel cells.

[0038] Principle of the method of the present invention:

[0039] Acrylic pulp is formed by using acrylonitrile as the main comonomer, has a highly fibrillated structure, a high proportion of branched structure, and contains a large number of cyano groups (-CN) on its surface, so acrylic pulp is a hydrophobic fiber. The present invention converts the hydrophobic group cyano group into a hydrophilic group carboxyl group (-COH), amide group (-CONH2), etc. by hydrophilic modification of acrylic pulp, thereby giving acrylic pulp hydrophilic properties. The fiber increases its specific surface area through surface etching, improves hydrophilicity, and further enhances its dispersion stability in water.

[0040] Expanded graphite is composed of the same elements as graphite, which are carbon atoms, and the structure is that six carbon atoms form a regular hexagon in the same plane and stretch into sheets. Since the surface mineralization of graphite is very high, it is neither hydrophilic nor oleophilic, which causes expanded graphite to be difficult to disperse and easily agglomerate in water. The present invention adopts subcritical liquid phase oxidation technology to prompt the oxidant to attack the oxidation active sites affected by steric hindrance between the surface and the sheets of expanded graphite, so that the expanded graphite is endowed with hydrophilic groups such as hydroxyl and carboxyl in all directions and 360 degrees. Adding hydrophilic groups on the surface of expanded graphite makes it easier to be wetted by water, further enhancing its water dispersibility.

[0041] Traditional carbon paper is mainly made of carbon fiber and uses a single phenolic resin as a binder, so it has poor strength, is brittle, and has difficult gap adjustment. The present invention utilizes the extremely high carbon storage rate and morphological characteristics of acrylic pulp - fiber extension tree-like, clustered fluffy microfibers, combined with a hydrophilic modification process, so that acrylic pulp and carbon fiber are interwoven to form a "hook-like" structure, which firmly locks the carbon fiber. This improves the mechanical meshing between carbon fiber and carbon fiber, and between carbon fiber and resin, enhances the interface performance between the two, and improves the strength of carbon fiber paper.

[0042] The modified micronized expanded graphite and acrylic pulp are combined through hydrogen bonds and intermolecular forces, acting as a "lock" in the "hook-like" structure, further enhancing the strength of the carbon paper. In addition, the modified micronized expanded graphite also retains the microstructure of expanded graphite - loose and porous. The void structure of the carbon paper can be adjusted by adjusting the proportion of the modified micronized expanded graphite in the carbon paper.

[0043] The brittleness of carbon paper is improved by adding latex to the slurry. Since there is no hydrophilic group on the surface of conventional carbon fiber, acrylic pulp and expanded graphite, the addition of latex will cause a large amount of loss. Active groups are introduced by modifying acrylic pulp and expanded graphite of the present invention, and then combined with aluminum sulfate, latex is retained in carbon paper through electrostatic adsorption and flocculation, further improving the toughness of carbon paper. In addition, since expanded graphite has its own graphite lamella structure, sliding surfaces are formed between the lamellae, making carbon paper difficult to break during bending. Therefore, modified micronized expanded graphite can not only enhance its own hydrophilicity but also enhance the strength of carbon paper, regulate porosity, improve conductivity and improve brittleness. Compared with traditional carbon paper, the present invention improves the strength of carbon paper, improves the brittleness of carbon paper, and regulates the porosity of carbon paper.

[0044] Example 1

[0045] Step 1: Add acrylic pulp to water to prepare a slurry with a concentration of 2%, then beat it to prepare a slurry with a beating degree of 30°SR, and then dehydrate it for use. Prepare sodium hydroxide with a concentration of 2%, and then add anhydrous ethanol with a mass of 10% relative to the mass of sodium hydroxide to prepare a modified liquid. Add the prepared modified liquid to the beaten acrylic pulp and react it in a high-pressure reactor at a pressure of 50kPa and a temperature of 50°C for 5 minutes. Finally, wash it with formic acid and clean water and dry it to obtain modified acrylic pulp.

[0046] Step 2: Mix the expanded graphite with water to prepare a 1% expanded graphite floating liquid, cut it with a high-speed disperser, and obtain a micronized expanded graphite with a size of 500 nanometers. Then add 15 times the mass of the expanded graphite and 1 times the mass of potassium permanganate to the expanded graphite floating liquid, react for 10 minutes under subcritical conditions of a temperature of 493K and a pressure of 5MPa to obtain an expanded graphite suspension. Finally, wash and filter with hydrogen peroxide, sodium hydroxide and water to obtain modified micronized expanded graphite.

[0047] Step 3: Add modified acrylic pulp and polyacrylonitrile-based carbon fiber with a diameter of 3mm and a length of 1mm into water in a ratio of 1:1 to prepare a mixed slurry with a concentration of 0.05%. Then add 2% of modified micronized expanded graphite relative to the mass of carbon fiber. Then add 0.1% of polyethylene oxide, 3% of aluminum sulfate and 5% of styrene-butadiene latex relative to the total fiber mass. Stir evenly to obtain a stabilized mixed slurry. The mixed slurry is sheet-formed and dried to obtain a carbon paper precursor. The carbon paper precursor is then immersed in a phenolic resin ethanol solution and dried. Finally, it is hot-pressed at a temperature of 120°C, a pressure of 2MPa, and a time of 5min, and carbonized at a temperature of 800°C and a time of 20min to obtain a quantitative of 30g / m 2 A carbon paper for use in fuel cells.

[0048] Example 2

[0049] Step 1: Add acrylic pulp to water to prepare a slurry with a concentration of 20%, then beat it to prepare a slurry with a beating degree of 80°SR, and then dehydrate it for use. Prepare potassium hydroxide with a concentration of 12%, and then add 30% anhydrous ethanol relative to the mass of potassium hydroxide to prepare a modified liquid. Add the prepared modified liquid to the beaten acrylic pulp and react it in a high-pressure reactor at a pressure of 200kPa and a temperature of 80°C for 20 minutes. Finally, wash it with acetic acid and clean water and dry it to obtain modified acrylic pulp.

[0050] Step 2: Mix the expanded graphite with water to prepare a 5% expanded graphite floating liquid, cut it with a high-speed disperser, and obtain a micronized expanded graphite with a size of 70 microns. Then add 25 times the mass of concentrated sulfuric acid and 5 times the mass of potassium dichromate to the expanded graphite floating liquid, and react for 30 minutes under subcritical conditions of a temperature of 593K and a pressure of 15MPa to obtain an expanded graphite suspension. Finally, wash and filter with hydrogen peroxide, sodium hydroxide and water to obtain modified micronized expanded graphite.

[0051] Step 3: Add modified acrylic pulp and asphalt-based carbon fiber with a diameter of 15μm and a length of 7mm into water at a ratio of 1:20 to prepare a mixed slurry with a concentration of 0.2%. Then add 10% of modified micronized expanded graphite relative to the mass of carbon fiber. Then add 0.2% of polyethylene oxide, 15% of aluminum sulfate and 25% of nitrile latex relative to the total fiber mass. Stir evenly to obtain a stabilized mixed slurry. The mixed slurry is sheet-formed and dried to obtain a carbon paper precursor. The carbon paper precursor is then immersed in a phenolic resin ethanol solution and dried. Finally, it is hot-pressed at a temperature of 180°C, a pressure of 15MPa, and a time of 25min, and carbonized at a temperature of 1600°C and a time of 200min to obtain a quantitative 150g / m 2 A carbon paper for use in fuel cells.

[0052] Example 3

[0053] Step 1: Add acrylic pulp to water to prepare a slurry with a concentration of 10%, then beat it to make a slurry with a beating degree of 50°SR, and then dehydrate it for use. Prepare lithium hydroxide with a concentration of 8%, and then add 20% anhydrous ethanol relative to the mass of lithium hydroxide to prepare a modified liquid. Add the prepared modified liquid to the beaten acrylic pulp and react it in a high-pressure reactor at a pressure of 100kPa and a temperature of 60°C for 10 minutes. Finally, wash it with citric acid and clean water and dry it to obtain modified acrylic pulp.

[0054] Step 2: Mix the expanded graphite with water to prepare a 3% expanded graphite floating liquid, cut it with a high-speed disperser to obtain a micronized expanded graphite with a size of 5 microns. Then add 20 times the mass of concentrated sulfuric acid and 3 times the mass of potassium permanganate to the expanded graphite floating liquid, react for 20 minutes under subcritical conditions of a temperature of 553K and a pressure of 10MPa to obtain an expanded graphite suspension. Finally, wash and filter with hydrogen peroxide, sodium hydroxide and water to obtain modified micronized expanded graphite.

[0055] Step 3: Add modified acrylic pulp and viscose-based carbon fiber with a diameter of 10μm and a length of 3mm into water at a ratio of 1:10 to prepare a mixed slurry with a concentration of 0.1%. Then add 8% of modified micronized expanded graphite relative to the mass of carbon fiber. Then add 0.15% of polyethylene oxide, 6% of aluminum sulfate and 15% of natural latex relative to the total fiber mass. Stir evenly to obtain a stabilized mixed slurry. The mixed slurry is sheet-formed and dried to obtain a carbon paper precursor. The carbon paper precursor is then immersed in a phenolic resin ethanol solution and dried. Finally, it is hot-pressed at a temperature of 150°C, a pressure of 8MPa, and a time of 15min, and carbonized at a temperature of 1200°C and a time of 60min to obtain a quantitative 60g / m 2 A carbon paper for use in fuel cells.

[0056] Comparative Example 1

[0057] Step 1: Add acrylic pulp to water to prepare a slurry with a concentration of 10%, then beat it to make a slurry with a beating degree of 50°SR, and then dehydrate it for use. Prepare lithium hydroxide with a concentration of 8%, and then add 20% anhydrous ethanol relative to the mass of lithium hydroxide to prepare a modified liquid. Add the prepared modified liquid to the beaten acrylic pulp and react it in a high-pressure reactor at a pressure of 100kPa and a temperature of 60°C for 10 minutes. Finally, wash it with citric acid and clean water and dry it to obtain modified acrylic pulp.

[0058] Step 2: Add modified acrylic pulp and viscose-based carbon fiber with a diameter of 10μm and a length of 3mm into water at a ratio of 1:10 to prepare a mixed slurry with a concentration of 0.1%. Then add 0.15% polyethylene oxide, 6% aluminum sulfate and 15% natural latex relative to the total fiber mass. Stir evenly to obtain a stabilized mixed slurry. The mixed slurry is sheet-formed and dried to obtain a carbon paper precursor. The carbon paper precursor is then immersed in a phenolic resin ethanol solution and dried. Finally, it is hot-pressed at a temperature of 150°C, a pressure of 8MPa, and a time of 15min, and carbonized at a temperature of 1200°C and a time of 60min to obtain a quantitative 60g / m 2 A carbon paper for use in fuel cells.

[0059] Comparative Example 2

[0060] The first step is to mix the expanded graphite with water to prepare a 3% expanded graphite floating liquid, and cut it with a high-speed disperser to obtain a micronized expanded graphite with a size of 5 microns. Then, 20 times the mass of concentrated sulfuric acid and 3 times the mass of potassium permanganate are added to the expanded graphite floating liquid, and the expanded graphite suspension is obtained by reacting at a temperature of 553K and a pressure of 10MPa under subcritical conditions for 20 minutes. Finally, the expanded graphite is washed and filtered with hydrogen peroxide, sodium hydroxide and water to obtain a modified micronized expanded graphite.

[0061] Step 2: Add viscose-based carbon fibers with a diameter of 10 μm and a length of 3 mm into water to prepare a slurry with a concentration of 0.1%. Then add 8% of modified micronized expanded graphite relative to the mass of carbon fiber. Then add 0.15% of polyethylene oxide, 6% of aluminum sulfate and 15% of natural latex relative to the total fiber mass. Stir evenly to obtain a stabilized mixed slurry. The mixed slurry is sheet-formed and dried to obtain a carbon paper precursor. The carbon paper precursor is then immersed in a phenolic resin ethanol solution and dried. Finally, it is hot-pressed at a temperature of 150°C, a pressure of 8 MPa, and a time of 15 minutes, and carbonized at a temperature of 1200°C and a time of 60 minutes to obtain a quantitative 60g / m 2 A carbon paper for use in fuel cells.

[0062] Comparative Example 3

[0063] Add viscose-based carbon fibers with a diameter of 10 μm and a length of 3 mm into water to prepare a slurry with a concentration of 0.1%. Then add 0.15% polyethylene oxide, 6% aluminum sulfate and 15% natural latex relative to the total fiber mass. Stir evenly to obtain a stabilized mixed slurry. The mixed slurry is sheet-formed and dried to obtain a carbon paper precursor. The carbon paper precursor is then immersed in a phenolic resin ethanol solution and dried, and finally subjected to hot pressing at a temperature of 150°C, a pressure of 8 MPa, and a time of 15 minutes, and carbonization at a temperature of 1200°C and a time of 60 minutes to obtain a quantitative 60g / m 2 A carbon paper for use in fuel cells.

[0064] Gas diffusion layer carbon paper performance test:

[0065] The carbon papers prepared in the above examples and comparative examples were tested for tensile strength, porosity, resistivity, air permeability, bending stiffness and other properties. The test results are shown in Table 1.

[0066] Table 1 Comparison of gas diffusion layer carbon paper properties

[0067]

[0068] As shown in Table 1, the addition of modified expanded graphite can significantly improve the porosity and air permeability of carbon paper, and the tensile strength and bendability are improved. As shown in Table 1, modified acrylic pulp can significantly improve the tensile strength of carbon paper, but the porosity and air permeability are reduced. As shown in Examples 1-3 and Comparative Examples 1-3, by introducing modified acrylic pulp and modified expanded graphite on carbon paper, the tensile strength of carbon paper can be significantly improved and the resistivity can be reduced, and the porosity and air permeability are kept good. In addition, the anti-bending deformation ability of carbon paper is improved. In summary, the carbon paper of the present invention has excellent comprehensive performance, not only has the advantages of high strength, excellent conductivity and uniform void structure, but also has improved bending deformation ability and toughness, and has good practical application value.

[0069] The above is only a preferred embodiment of the present invention and is not intended to limit the invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing carbon paper for a fuel cell gas diffusion layer, characterized in that: (1) Adding acrylic fiber pulp into water to prepare a pulp with a concentration of 2%-20%, then beating the pulp to prepare a pulp with a beating degree of 30-80°SR, and then dehydrating the pulp for standby use; Prepare a 2%-12% alkali solution, add 10%-30% of anhydrous ethanol relative to the mass of the alkali solution, and prepare a modified solution; Add the prepared modified liquid to the beaten acrylic pulp, and react for 5-20 minutes in a high-pressure reactor at a pressure of 50-200 kPa and a temperature of 50° C.-80° C.; The modified acrylic fiber pulp is prepared by washing with weak acid and clean water and drying; (2) Mixing expanded graphite with water to prepare an expanded graphite floating liquid with a mass ratio of 1% to 5%, and cutting it with a high-speed disperser to obtain micronized expanded graphite; Adding concentrated sulfuric acid in an amount of 15-25 times the mass of the expanded graphite and an oxide in an amount of 1-5 times the mass of the expanded graphite to the expanded graphite floating liquid, and reacting for 10-30 minutes under subcritical conditions to obtain an expanded graphite suspension; The modified micronized expanded graphite is prepared by washing and filtering with hydrogen peroxide, sodium hydroxide and water; (3) adding modified acrylic pulp and carbon fiber into water to prepare a mixed slurry with a concentration of 0.05%-0.2%; Add 2%-10% of modified micronized expanded graphite relative to the mass of carbon fiber, add 0.1%-0.2% of polyethylene oxide, 3%-15% of aluminum sulfate and 5%-25% of latex relative to the mass of total fiber; stir evenly to obtain a stabilized mixed slurry; sheet-form the mixed slurry and dry it to obtain a carbon paper precursor; then impregnate the carbon paper precursor in a phenolic resin ethanol solution and dry it, and finally obtain a fuel cell gas diffusion layer carbon paper through hot pressing and carbonization.

2. The method for preparing a fuel cell gas diffusion layer carbon paper according to claim 1, characterized in that: The alkaline solution in step (1) is one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide; the weak acid is one or more of formic acid, acetic acid and citric acid.

3. The method for preparing a fuel cell gas diffusion layer carbon paper according to claim 1, characterized in that: The expanded graphite in step (2) is prepared from expandable graphite of 200-2000 mesh; the size of the micronized expanded graphite is between 500 nanometers and 70 micrometers.

4. The method for preparing a fuel cell gas diffusion layer carbon paper according to claim 1, characterized in that: The oxide in step (2) is one or more of potassium permanganate and potassium dichromate.

5. The method for preparing a fuel cell gas diffusion layer carbon paper according to claim 1, characterized in that: The subcritical temperature of step (2) is 493-593K and the pressure is 5-15MPa.

6. The method for preparing a fuel cell gas diffusion layer carbon paper according to claim 1, characterized in that: The carbon fiber described in step (3) is one or more of polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber and viscose-based carbon fiber; the carbon fiber has a diameter of 3-15 μm and a length of 1-7 mm.

7. The method for preparing a fuel cell gas diffusion layer carbon paper according to claim 1, characterized in that: The mass ratio of the modified acrylic pulp to the carbon fiber in step (3) is 1:1-20.

8. The method for preparing a fuel cell gas diffusion layer carbon paper according to claim 1, characterized in that: The latex described in step (3) is one or more of styrene-butadiene latex, nitrile-butadiene latex and natural latex.

9. The method for preparing a fuel cell gas diffusion layer carbon paper according to claim 1, characterized in that: The hot pressing treatment temperature in step (3) is 120°C-180°C, the pressure is 2-15MPa, and the time is 5-25min; the carbonization condition is in an inert atmosphere, the carbonization temperature is 800°C-1600°C, and the carbonization time is 20-200min.

10. The method for preparing carbon paper for a fuel cell gas diffusion layer according to claim 1, characterized in that: The carbonization conditions in step (3) are one or more of nitrogen and argon.

Citation Information

Patent Citations

  • A high-performance carbon paper for fuel cells, its preparation method and application

    CN110512459B

  • A PEM fuel cell, a porous carbon paper with a gas diffusion layer, and a method for preparing the same.

    CN113066996B

  • Carbon fiber paper material for gas diffusing layer of fuel cell electrode and its prepn

    CN1185736C

  • Carbonized silk fabric / transition metal oxide composite material for flexible lithium ion battery negative electrode and preparation method thereof

    CN109713261A

  • High-performance carbon paper for fuel cell and preparation method and application thereof

    CN110512459A

Cited By

  • Preparation method of carbon fiber paper

    CN121896753A