Non-inverted bonded dual-band quantum dot pixels, focal plane arrays, their fabrication methods and applications

By using a non-flip-bonded dual-band quantum dot pixel structure, the problems of thermal stress mismatch and high cost in flip-bonding technology are solved, achieving efficient visible light and infrared detection with the advantages of high yield and low cost.

CN115188889BActive Publication Date: 2026-11-17XINIR TECHNOLOGY(BEIJING) CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210753491.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-28
Publication Date
2026-11-17
Estimated Expiration
2042-06-28

AI Technical Summary

Technical Problem

Existing flip-chip bonding technology suffers from problems such as high chip power density, heat dissipation, and thermal stress mismatch when fabricating visible light and infrared detectors, leading to bonding failure. In addition, the equipment cost is high and the yield is low.

Method used

A non-inverted bonded dual-band quantum dot pixel structure is adopted, including a bottom electrode, a top electrode, and a hole transport layer, an infrared photosensitive film layer, and a visible light photosensitive film layer located therebetween. A PNP heterojunction is formed by using a chalcogenide mercury colloidal quantum dot intrinsic layer and a chalcogenide silver colloidal quantum dot doping layer. Combined with a simple fabrication process, a detector with the advantages of visible light and infrared detection is fabricated.

Benefits of technology

The detector achieves high photoelectric conversion efficiency and high yield, possesses the dual-band advantage of visible light and infrared detection, reduces manufacturing costs, and avoids the thermal stress mismatch problem of flip-chip bonding technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115188889B_ABST
    Figure CN115188889B_ABST
Patent Text Reader

Abstract

This invention relates to a non-flip-bonded dual-band quantum dot pixel, focal plane array, its fabrication method, and its application, belonging to the field of optoelectronic sensor technology. The dual-band quantum dot pixel includes a bottom electrode, a top electrode, and a hole transport layer, an infrared photosensitive film layer, and a visible light photosensitive film layer located between the top and bottom electrodes. The infrared photosensitive film layer includes an intrinsic layer of chalcogenide mercury colloidal quantum dots and a doped layer of chalcogenide silver colloidal quantum dots. The visible light photosensitive film layer includes an electron transport layer and a cadmium telluride colloidal quantum dot layer. The chalcogenide silver colloidal quantum dot doped layer, the intrinsic layer of chalcogenide mercury colloidal quantum dots, the electron transport layer, and the cadmium telluride colloidal quantum dot layer constitute a P-N-P heterojunction. The fabrication method designed in this invention is relatively simple, low-cost, and has a high yield. Furthermore, the resulting detector not only possesses the advantages of visible light and infrared detection but also exhibits high photoelectric conversion efficiency and good device efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fabrication of dual-band quantum dots and focal plane arrays using a non-inverted bonding fabrication process, belonging to the field of optoelectronic sensor technology. Specifically, it relates to a non-inverted bonding dual-band quantum dot pixel and focal plane array, its fabrication method, and its application. Background Technology

[0002] The development of information fusion technology has made it possible for multiple sensors to work collaboratively. Information fusion technology refers to the multi-level, multi-faceted, and multi-layered processing and fusion of information acquired from the same scene at the same time, thereby obtaining more reliable, richer, more accurate, and more meaningful information. The coupling of visible light detectors and infrared detectors is currently one of the most common information fusion technologies. Visible light detectors can capture detailed information about the object being measured and have high spatial resolution, but because they operate within an atmospheric window, they are highly susceptible to weather conditions and cannot operate in all weather. Furthermore, visible light images cannot detect targets hidden in complex backgrounds. Short-wave infrared detectors, on the other hand, utilize blackbody radiation for imaging, are less affected by lighting conditions and adverse weather, and have nighttime imaging capabilities. However, due to limitations in their imaging principles, infrared images have low contrast, strong spatial correlation, and poor detail reproduction, resulting in imaging effects that do not conform to human visual perception. Coupled with visible light detectors and infrared detectors, the shortcomings of each imaging system can be compensated for, leveraging the advantages of both visible light and infrared detection. This allows the detector to possess the advantages of both, improving the system's detection and reconnaissance capabilities.

[0003] Traditionally, flip-chip bonding technology has been used to couple the fabricated detector to the readout circuit. This technology employs solder bumps to achieve the mechanical and electrical connection between the chip and the substrate. However, as the bump density and spacing of flip-chips increase, the chip's power density increases rapidly, exacerbating heat dissipation and internal thermal stress mismatch issues, making bonding failure more likely. Furthermore, because the bumps or solder balls are hidden between the chip and the substrate, thermal performance analysis and defect detection become extremely difficult. Additionally, flip-chip bonding technology requires expensive equipment, resulting in a complex process and low yield. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention discloses a non-inverted bonded dual-band quantum dot pixel, a focal plane array, its fabrication method, and its applications. The fabrication method designed in this invention is relatively simple, low-cost, and has a high yield. Furthermore, the resulting detector not only possesses the advantages of visible light and infrared detection but also exhibits high photoelectric conversion efficiency and good device efficiency.

[0005] To achieve the above technical objectives, this invention discloses a non-flip-bonded dual-band quantum dot pixel. The pixel includes a bottom electrode, a top electrode, and a hole transport layer, an infrared photosensitive film layer, and a visible light photosensitive film layer located between the top electrode and the bottom electrode. The infrared photosensitive film layer includes an intrinsic layer of chalcogenide mercury colloidal quantum dots and a doped layer of chalcogenide silver colloidal quantum dots. The visible light photosensitive film layer includes an electron transport layer and a cadmium telluride colloidal quantum dot layer. The chalcogenide silver colloidal quantum dot layer, the intrinsic layer of chalcogenide mercury colloidal quantum dots, the electron transport layer, and the cadmium telluride colloidal quantum dot layer constitute a PNP heterojunction.

[0006] Furthermore, the electron transport layer is made of any one of cadmium selenide, cadmium sulfide, or zinc oxide.

[0007] Furthermore, the hole transport layer is made of DMSO (dimethyl sulfoxide) or NiO. x (Referring to nickel oxides with oxygen vacancies) or either PEDOT:PSS.

[0008] Furthermore, the thickness of the chalcogenide silver colloidal quantum dot doped layer is smaller than that of the intrinsic chalcogenide mercury colloidal quantum dot layer, and the thickness of the electron transport layer is smaller than that of the cadmium telluride colloidal quantum dot layer.

[0009] The thickness of the chalcogenide silver colloidal quantum dot doped layer is 30–50 nm, the thickness of the chalcogenide mercury colloidal quantum dot intrinsic layer is 400–600 nm, the thickness of the electron transport layer is 30–50 nm, and the thickness of the cadmium telluride colloidal quantum dot layer is 400–600 nm.

[0010] Furthermore, the bottom electrode is made of an infrared-transparent conductive material laminated on a silicon substrate, and the top electrode is made of a metallic conductive material. Specifically, the infrared-transparent conductive material includes ITO, FTO, or AZO laminated on a silicon substrate; preferably, it is ITO laminated on a silicon substrate. The metallic conductive material is any one of gold, silver, copper, or aluminum.

[0011] Furthermore, the pixel, from bottom to top, is composed of ITO, a cadmium telluride colloidal quantum dot layer, a zinc oxide layer, a mercury telluride colloidal quantum dot intrinsic layer, a silver telluride colloidal quantum dot doped layer, a PEDOT:PSS layer, and a gold electrode, all composited on a silicon substrate. The cadmium telluride colloidal quantum dot layer has a thickness of 400–600 nm, the zinc oxide layer has a thickness of 30–50 nm, the mercury telluride colloidal quantum dot intrinsic layer has a thickness of 400–600 nm, the silver telluride colloidal quantum dot doped layer has a thickness of 30–50 nm, the PEDOT:PSS layer has a thickness of 30–50 nm, and the gold electrode has a thickness of 30–50 nm.

[0012] The second objective of this invention is to disclose a method for preparing non-inverted bonded dual-band quantum dot pixels, which includes the following steps:

[0013] 1) Select the bottom electrode;

[0014] 2) Preparation of cadmium telluride colloidal quantum dot layer: A cadmium telluride colloidal quantum dot ink is coated onto the upper surface of the bottom electrode, then placed on a hot plate for a period of time, followed by treatment in a saturated CdCl2 solution. After removal, excess CdCl2 solution is washed away with isopropanol, and the electrode is then placed on a hot plate for sintering. This process is repeated multiple times to obtain the cadmium telluride colloidal quantum dot layer. The saturated CdCl2 solution is a saturated methanol solution of CdCl2. The subsequent hot plate sintering temperature is higher than the preceding temperature. Specifically, the subsequent hot plate sintering temperature is 320–380℃, and the preceding temperature is 50–70℃.

[0015] 3) Preparation of the electron transport layer: The electron transport layer solution is coated onto the surface of the cadmium telluride colloidal quantum dot layer from step 1), and then annealed on a hot plate to obtain the electron transport layer; wherein, the electron transport layer solution includes any one of cadmium selenide, cadmium sulfide, or zinc oxide, preferably a zinc oxide solution, wherein the zinc oxide solution is a solution of zinc oxide dissolved in isopropanol, and its concentration is 15-25 mg / mL, preferably 20 mg / mL. The annealing temperature on the plate is 70-90℃.

[0016] 4) Preparation of the intrinsic layer of sulfide-based mercury colloidal quantum dots: The upper surface of the electron transport layer prepared in step 3) is coated with sulfide-based mercury colloidal quantum dot ink, and then 1,2-ethanedithiol is added dropwise for a period of time. The excess 1,2-ethanedithiol is washed away with isopropanol, and then a methanol solution of HgCl2 is added dropwise for treatment. The excess HgCl2 is washed away with isopropanol, and the excess isopropanol is removed by spin coating. The entire process is repeated multiple times to obtain the sulfide-based mercury colloidal quantum dot layer. Here, the methanol solution of HgCl2 can be any concentration of methanol solution.

[0017] 5) Preparation of chalcogenide silver colloidal quantum dot doped layer: The surface of the intrinsic chalcogenide mercury colloidal quantum dot layer prepared in step 4) is coated with chalcogenide silver colloidal quantum dot ink, then treated in a methanol solution of HgCl2, and after removal, the residual HgCl2 is washed away with isopropanol, and the excess isopropanol is removed by spin coating machine; thus, a chalcogenide silver colloidal quantum dot doped layer is obtained.

[0018] 6) Preparation of hole transport layer: A hole transport layer solution is coated on the upper surface of the chalcogenide silver colloidal quantum dot doped layer prepared in step 5), and then annealed on a hot plate to obtain the hole transport layer; the hole transport layer solution includes DMSO and NiO. x The annealing treatment can be performed using any solution of PEDOT:PSS, with PEDOT:PSS being preferred in this invention. The annealing temperature is 50–70°C.

[0019] 7) Encapsulating the top electrode: A metal conductive material is vapor-deposited on the upper surface of the hole transport layer prepared in step 6) to form the top electrode.

[0020] Furthermore, the coating method includes one or more of the following: drop coating, spray coating, spin coating, blade coating, or ink printing.

[0021] Furthermore, this invention discloses a method for preparing a non-inverted bonded dual-band quantum dot pixel, which includes the following steps:

[0022] (1) Select the bottom electrode;

[0023] (2) Preparation of cadmium telluride colloidal quantum dot layer: spin-coat cadmium telluride colloidal quantum dot ink on the upper surface of the bottom electrode. Select spin-coating mode of 800r-20s+1000r-10s, then place it on a hot plate at 60℃ for 1min, and then put it into a saturated CdCl2 solution (CdCl2 is soluble in methanol) and treat it at 60℃ for 15s. After taking it out, rinse off the excess CdCl2 solution with isopropanol, and then place it on a hot plate at 350℃ for sintering for 20s. The whole process is repeated 6 times.

[0024] (3) Preparation of electron transport layer: Take 50 μL of ZnO with a pipette and spin-coat it onto the surface of the cadmium telluride colloidal quantum dot layer. Select the spin-coating mode as 3000 r-60 s, and then place it on an 80℃ hot plate for annealing for 10 min.

[0025] (4) Preparation of the intrinsic layer of mercury telluride colloidal quantum dots: Mercury telluride colloidal quantum dot ink was spin-coated onto the upper surface of the electron transport layer. The spin-coating method was 800r-20s+1000r-10s. Then, EDT (1,2-ethylenedithiol) was dropped onto the mercury telluride film and treated for 10s. The residual EDT was washed away with isopropanol. Then, a methanol solution of HgCl2 was dropped onto the film and treated for 10s. The residual HgCl2 was washed away with isopropanol. The excess isopropanol was removed by spin-coating. The whole process was repeated 6 times.

[0026] (5) Preparation of silver telluride colloidal quantum dot doped layer: Silver telluride colloidal quantum dot ink is spin-coated onto the surface of the intrinsic layer of mercury telluride colloidal quantum dots. The spin-coating method is selected as 800r-20s+1000r-10s. Then, it is treated with methanol solution of HgCl2 for 10s, the residual HgCl2 is washed away with isopropanol, and the excess isopropanol is removed by spin-coating machine.

[0027] (6) Preparation of hole transport layer: PEDOT:PSS solution was spin-coated on the surface of the silver telluride colloidal quantum dot doped layer. The spin-coating method was 5000r-60s, and then the layer was placed on a hot plate at 60℃ for annealing for 20min.

[0028] (7) Encapsulating the top electrode: depositing nano-gold on the surface of the hole transport layer to form a top electrode with a thickness of about 40 nm.

[0029] Furthermore, the cadmium telluride colloidal quantum dot ink comprises the following preparation steps:

[0030] 1) Preparation of long-chain strong ligand coating solution: Place a magnetic ball in a three-necked flask, add a certain amount of cadmium oxide into the three-necked flask, and continue to add oleic acid and octadecene. Seal two of the three-necked flasks with a rubber stopper. Insert a thermocouple into one of the three-necked flasks, and connect a balloon to the other three-necked flask with a syringe to prevent it from bursting. Connect the last three-way tube to a vacuum pump at one end and argon gas at the other end.

[0031] 2) Preparation of thermal equilibrium solution: First, evacuate the three-necked flask in step 1), then slowly introduce argon gas to ensure that the three-necked flask is in an argon environment. Then, set the thermocouple to 220°C. After the solution is clear, set the thermocouple temperature to 270°C and allow the thermal equilibrium to be maintained for about half an hour.

[0032] 3) Preparation of tellurium source: Dissolve tellurium powder in trioctylphosphine (TOP) and stir well in a glove box at room temperature;

[0033] 4) Preparation of cadmium telluride tributyl phosphate solution: Take the solution from step 3) and quickly inject it into the three-necked flask from step 2), and let the reaction continue until completion;

[0034] 5) Preparation of cadmium telluride colloidal quantum dot ink: Remove the three-necked flask from the heating hood in step 4), cool it for a long time with an air gun, and then cool it in a water bath. After the cooling is complete, take the solution out of the three-necked flask, add toluene and anhydrous ethanol, centrifuge several times, then add n-hexane to dissolve it evenly and store it in a glove box for later use.

[0035] Furthermore, the preparation steps of the mercury telluride colloidal quantum dot ink are as follows:

[0036] 1) Preparation of thermal equilibrium solution: In a glove box under nitrogen atmosphere, take a certain amount of mercuric chloride and add oleylamine. Place the mixture on a heating plate, stir to dissolve, adjust the temperature of the heating plate to 100℃, heat at 100℃ for 1 hour until a transparent, light yellow solution is formed. Then cool the solution to 80℃ as the synthesis temperature. Thermal equilibrium takes about half an hour.

[0037] 2) Prepare the quenching solution: Take a certain amount of trioctylphosphine and trichloroethylene, put them in a glass bottle, mix them well, and then store them in a refrigerator;

[0038] 3) Preparation of tellurium source: Dissolve tellurium powder in trioctylphosphine (TOP) and stir well in a glove box at room temperature;

[0039] 4) Preparation of mercury telluride colloidal quantum dot ink: Take the thermal equilibrium solution from step 1) and quickly inject it into the solution from step 3). The mixture gradually darkens and turns black. After the reaction continues for a period of time, add the quenching solution from step 2) to cool the reaction solution. After removing the reaction solution from the glove box, cool it in a water bath. Transfer the reaction solution to a centrifuge tube and add an appropriate amount of isopropanol to mix. The amount of isopropanol added can be flexibly adjusted according to the number of centrifugations and the centrifugation effect. Place the mixed solution into a centrifuge for centrifugation to separate the precipitate. Discard the supernatant. Dry the solid precipitate with a nitrogen gun. The drying time is determined according to the actual processing conditions. The dried solid precipitate was then redispersed in hexane. A certain amount of 2-mercaptoethanol and tetrabutylammonium bromide were added, and the mixture was ultrasonically vibrated for a period of time to dissolve the mercury telluride quantum dot solid as completely as possible. N,N-dimethylformamide was then added, and ultrasonic vibration was continued to mix the mixture so that the mercury telluride red quantum dots were completely transferred from hexane to N,N-dimethylformamide. After the transfer was complete, the hexane was discarded.

[0040] Furthermore, the silver telluride colloidal quantum dot ink comprises the following preparation steps:

[0041] 1) Preparation of tellurium source: Dissolve tellurium powder in trioctylphosphine (TOP) and stir well in a glove box at room temperature;

[0042] 2) Synthesis of silver telluride colloidal quantum dots: Dissolve silver nitrate in oleylamine and oleic acid, place in a glove box and stir at 70°C. Continue to inject trioctylphosphine and heat rapidly to 160°C. The reaction solution continues to change from clear to yellow. Inject the solution from step 1), and the yellow solution immediately turns black. After the reaction is complete, the original reaction solution can be further washed and the subsequent process can be carried out. Alternatively, the original reaction solution can be placed in a -8°C environment for refrigeration. The molar ratio between silver nitrate and tellurium powder is 2:1.

[0043] 3) Cleaning silver telluride colloidal quantum dots: Take the above reaction stock solution at room temperature, add methanol and mix in a vortex mixer, continue sonication, then centrifuge. After centrifugation, discard the supernatant, take the solid precipitate and dissolve it in a mixture of dodecyl mercaptan and chlorobenzene, mix well, add methanol and mix well, continue sonication, then centrifuge. After centrifugation, discard the supernatant, take the solid precipitate and dissolve it in chlorobenzene, add methanol and mix well, continue sonication, then centrifuge. After centrifugation, discard the supernatant, take the solid precipitate and dissolve it in a 9:1 volume ratio of n-hexane + octane solution to form cleaned silver telluride colloidal quantum dot ink.

[0044] The third objective of this invention is to disclose a non-inverted bonded dual-band quantum dot focal plane array, which includes a readout circuit and a plurality of the aforementioned non-inverted bonded dual-band quantum dot pixels arranged in a row and column array on the readout circuit.

[0045] The fourth objective of this invention is to disclose the application of a non-flip-bonded dual-band quantum dot focal plane array in the visible light range of 390nm to 760nm and the short-wave infrared range of 1.5µm to 2.5µm. Specifically, it has applications in fields such as industrial inspection, autonomous driving assistance devices, surveillance, and military applications.

[0046] The technical solution provided by the embodiments of the present invention has the following advantages compared with the prior art:

[0047] The fabrication method designed in this invention is relatively simple, low in cost, and has a high yield. Moreover, the detector produced not only has the advantages of visible light detection and infrared detection, but also has high photoelectric conversion efficiency and good device efficiency. Attached Figure Description

[0048] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0049] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0050] Figure 1 This is a schematic diagram of the structure of the pixel designed for this invention;

[0051] Figure 2 A schematic diagram of the structure of a pixel in an embodiment of the present invention;

[0052] Figure 3 The spectral absorption curve of cadmium telluride was prepared for the embodiments of the present invention;

[0053] Figure 4 The absorption spectrum of mercury telluride was prepared for an embodiment of the present invention;

[0054] Figure 5 The equivalent circuit diagram of the array is designed for an embodiment of the present invention.

[0055] The component numbers in the above-mentioned attached diagram are as follows:

[0056] Top electrode 101, hole transport layer 102, chalcogenide silver colloidal quantum dot doped layer 103, chalcogenide mercury colloidal quantum dot intrinsic layer 104, electron transport layer 105, cadmium telluride colloidal quantum dot layer 106, bottom electrode 107. Detailed Implementation

[0057] To better understand the above-mentioned objectives, features, and advantages of the present invention, the solutions of the present invention will be further described below. It should be noted that, unless otherwise specified, the embodiments of the present invention and the features thereof can be combined with each other.

[0058] This invention discloses a non-flip-bonded dual-band quantum dot pixel. The pixel includes a bottom electrode, a top electrode, and a hole transport layer, an infrared photosensitive film layer, and a visible light photosensitive film layer located between the top electrode and the bottom electrode. The infrared photosensitive film layer includes an intrinsic layer of chalcogenide mercury colloidal quantum dots and a doped layer of chalcogenide silver colloidal quantum dots. The visible light photosensitive film layer includes an electron transport layer and a cadmium telluride colloidal quantum dot layer. The chalcogenide silver colloidal quantum dot layer, the intrinsic layer of chalcogenide mercury colloidal quantum dots, the electron transport layer, and the cadmium telluride colloidal quantum dot layer constitute a PNP heterojunction.

[0059] The electron transport layer is made of cadmium selenide, cadmium sulfide, or zinc oxide. The intrinsic layer of the chalcogenide mercury colloidal quantum dot is made of any one of mercury sulfide, mercury selenide, or mercury telluride. The preparation method of the intrinsic layer of the chalcogenide mercury colloidal quantum dot is described in the following embodiments. Similarly, the chalcogenide silver colloidal quantum dot doped layer is made of any one of silver sulfide, silver selenide, or silver telluride. The preparation method of the chalcogenide silver colloidal quantum dot doped layer is described in the following embodiments. The preparation method of the cadmium telluride colloidal quantum dot layer is described in the following embodiments. The hole transport layer is preferably made of PEDOT:PSS. The bottom electrode is made of an infrared transparent conductive material composited on a silicon substrate, and the top electrode is made of a metallic conductive material. Specifically, the infrared transparent conductive material includes ITO, FTO, or AZO composited on a silicon substrate; in this invention, ITO composited on a silicon substrate is preferred. The metallic conductive material is any one of gold, silver, copper, or aluminum. Gold is preferred in this invention.

[0060] At the same time, the present invention discloses a method having Figure 1The pixel of the structure, from top to bottom, includes a top electrode 101, a hole transport layer 102, a chalcogenide silver colloidal quantum dot doped layer 103, a chalcogenide mercury colloidal quantum dot intrinsic layer 104, an electron transport layer 105, a cadmium telluride colloidal quantum dot layer 106, and a bottom electrode 107. Cadmium telluride is a direct bandgap compound semiconductor with a high light absorption coefficient and an ideal bandgap. When combined with the electron transport layer, it forms an np model, which is beneficial for improving the power conversion efficiency of the target device. Photoconductive devices fabricated with the chalcogenide mercury colloidal quantum dot intrinsic layer have proven to have good application prospects in short-wave infrared detection, but limitations remain in detection speed and sensitivity. Meanwhile, photovoltaic devices fabricated with the chalcogenide mercury colloidal quantum dot intrinsic layer have achieved low-temperature background-limited infrared photodetection, with a sensitivity improvement of two orders of magnitude compared to photoconductive devices. This invention selects to stack chalcogenide silver colloidal quantum dots on the intrinsic layer of chalcogenide mercury colloidal quantum dots and utilizes the diffusion of silver ions to form stable and reliable P-type doping, which further improves the device efficiency and sensitivity.

[0061] Furthermore, the present invention also discloses a non-inverted bonded dual-band quantum dot focal plane array, which includes a readout circuit and the plurality of non-inverted bonded dual-band quantum dot pixels distributed in an array on the readout circuit.

[0062] Many specific details are set forth in the following description in order to provide a full understanding of the invention, but the invention may also be practiced in other ways different from those described herein; obviously, the embodiments in the specification are only some embodiments of the invention, and not all embodiments.

[0063] Example 1

[0064] This embodiment synthesizes cadmium telluride colloidal quantum dot ink, including the following steps:

[0065] (1) Preparation of long-chain strong ligand coating solution: Place a magnetic ball in a three-necked flask, take 1.9 g CdO (15 mmol) and put it into the three-necked flask, and continue to add 18.8 mL OA (oleic acid) and 20.3 mL ODE (octadecene). Seal two of the three-necked flasks with rubber stoppers, insert a thermocouple into one of the three-necked flasks, connect a balloon to the other three-necked flask with a syringe to prevent it from bursting, and connect the last three-way tube to a vacuum pump at one end and argon gas at the other end.

[0066] (2) Preparation of thermal equilibrium solution: First, evacuate the three-necked flask from step (1), and then slowly introduce argon gas (replace 3 times) to ensure that the three-necked flask is in an argon environment. Then, set the thermocouple to 220°C. After the solution is clear, set the thermocouple temperature to 270°C and allow it to reach thermal equilibrium for about half an hour.

[0067] (3) Preparation of tellurium source: Dissolve 10g of tellurium powder in 111mL of trioctylphosphine (TOP) in a glove box at room temperature, add magnetic stirring, and wait until the solution turns bright yellow before taking it out of the glove box;

[0068] (4) Preparation of cadmium telluride tributyl phosphate (TBP) solution: Take the solution from step (3) and quickly inject it into the three-necked flask from step (2), and let the reaction continue until the end;

[0069] (5) Preparation of cadmium telluride colloidal quantum dot ink: Remove the three-necked flask from the heating hood in step (4), cool it for a long time with an air gun, and then cool it in a water bath. After the cooling is complete, remove the solution from the three-necked flask, add toluene and anhydrous ethanol in a volume ratio of 1:2, centrifuge twice, then add n-hexane to dissolve evenly and store in a glove box for later use.

[0070] Example 2

[0071] This embodiment discloses a method for preparing chalcogenide mercury colloidal quantum dot ink, specifically taking mercury telluride as an example, including the following steps:

[0072] (1) Preparation of thermal equilibrium solution: In a glove box under nitrogen atmosphere, take 27.2 mg (0.1 mmol) of mercuric chloride, add 4 mL of oleylamine, place the mixture on a heating plate, add a magnetic stirrer to help accelerate dissolution, adjust the temperature of the heating plate to 100°C, heat at 100°C for 1 h until a transparent, light yellow solution is formed, then cool the solution to 80°C as the synthesis temperature, and thermal equilibrium is achieved in about half an hour.

[0073] (2) Preparation of quenching solution: Take 0.5 mL of trioctylphosphine and 4 mL of trichloroethylene and put them in a glass bottle, mix well, and then store in a refrigerator;

[0074] (3) Preparation of tellurium source: At room temperature, stir 0.1 mmol of tellurium powder and 0.1 mL of trioctylphosphine in a nitrogen glove box to form a bright yellow solution.

[0075] (4) Preparation of mercury telluride colloidal quantum dot ink: Take the thermal equilibrium solution from step (1) and quickly inject it into the solution from step (3). After 15-30 seconds, the mixture gradually darkens and turns black. After the reaction continues for 4 minutes, add the quenching solution from step (2) to cool the reaction solution. Remove the reaction solution from the glove box and cool it in a water bath. Transfer the reaction solution to a centrifuge tube and add an appropriate amount of isopropanol to mix. The amount of isopropanol added can be adjusted flexibly according to the number of centrifugations and the centrifugation effect. Place the mixed solution into a centrifuge for centrifugation to separate the precipitate. Control the centrifuge speed at 7500 r / min and centrifuge for 5-10 minutes. Discard the supernatant. Dry the solid precipitate with a nitrogen gun. The drying time is determined according to the actual processing conditions. The dried solid precipitate was then redispersed in 6 mL of n-hexane. 50 μL of 2-mercaptoethanol and 15 mg of tetrabutylammonium bromide were added, and the mixture was sonicated for 1 minute to dissolve the mercury telluride quantum dots as completely as possible. 2.5 mL of N,N-dimethylformamide was then added, and the mixture was sonicated for another minute to mix thoroughly and completely transfer the mercury telluride red quantum dots from the n-hexane to the N,N-dimethylformamide. After the transfer was complete, the n-hexane was discarded.

[0076] Example 3

[0077] This embodiment discloses a method for preparing chalcogenide silver colloidal quantum dot ink, specifically using silver telluride as an example, including the following steps:

[0078] (1) Preparation of tellurium source: At room temperature, 0.1 mmol of tellurium powder and 0.1 mL of trioctylphosphine were stirred in a nitrogen glove box to form a bright yellow solution;

[0079] (2) Synthesis of silver telluride colloidal quantum dots: Dissolve silver nitrate in oleylamine and oleic acid, place in a glove box and stir for 30 min at 70°C to obtain a uniformly dissolved solution, continue to inject trioctylphosphine, and heat rapidly to 160°C for 35-45 min. The solution changes from clear to yellow. Inject the solution from step (1), and the yellow solution immediately turns black. After the reaction is completed, you can choose to further clean the reaction solution and carry out subsequent processes, or you can choose to refrigerate the reaction solution in an environment of -8°C. The molar ratio between silver nitrate and tellurium powder is 2:1.

[0080] (3) Cleaning silver telluride colloidal quantum dots: Take the above reaction stock solution at room temperature, add methanol and place it in a vortex mixer to mix. Continue to sonicate for about 20 seconds, then centrifuge. After centrifugation, discard the supernatant and dissolve the solid precipitate in a mixture of dodecyl mercaptan and chlorobenzene. Mix well, add methanol and mix again. Continue to sonicate for about 20 seconds, then centrifuge. After centrifugation, discard the supernatant and dissolve the solid precipitate in chlorobenzene. Add methanol and mix again. Continue to sonicate for about 20 seconds, then centrifuge for 5 minutes. After centrifugation, discard the supernatant and dissolve the solid precipitate in a hexane + octane solution with a volume ratio of 9:1 to form cleaned silver telluride colloidal quantum dot ink.

[0081] Example 4

[0082] This embodiment discloses a feature Figure 2 The method for preparing the structural pixels shown includes the following steps:

[0083] (1) Select the bottom electrode;

[0084] (2) Preparation of cadmium telluride colloidal quantum dot layer: The cadmium telluride colloidal quantum dot ink prepared in Example 1 was spin-coated onto the bottom electrode using a spin-coating method of 800r-20s + 1000r-10s. The electrode was then placed on a hot plate at 60℃ for 1 min, followed by immersion in a saturated CdCl2 solution (CdCl2 is soluble in methanol) at 60℃ for 15 s. The electrode was then rinsed with isopropanol to remove excess CdCl2 solution, and finally sintered on a hot plate at 350℃ for 20 s. This process was repeated 6 times. The spectral absorption curve of the cadmium telluride thin film is shown below. Figure 3 As shown;

[0085] (3) Preparation of electron transport layer: Take 50 μL of ZnO with a pipette and spin-coat it on top of the cadmium telluride colloidal quantum dot layer. Select the spin-coating mode as 3000r-60s, and then place it on an 80℃ hot plate for annealing for 10 min.

[0086] (4) Preparation of the intrinsic layer of mercury telluride colloidal quantum dots: The mercury telluride colloidal quantum dot ink prepared in Example 2 above the electron transport layer was spin-coated using a spin-coating method of 1000r-20s+300r-10s. Then, EDT (1,2-ethylenedithiol) was dropped onto the mercury telluride film for 10s. The residual EDT was rinsed off with isopropanol, followed by the addition of a methanol solution of HgCl2 for 10s. The residual HgCl2 was rinsed off with isopropanol, and excess isopropanol was removed using a spin coater. The entire process was repeated 6 times. The spectral absorption curve of the mercury telluride film is shown below. Figure 4 As shown;

[0087] (5) Preparation of silver telluride colloidal quantum dot doped layer: The silver telluride colloidal quantum dot ink prepared in Example 3 above was spin-coated on the intrinsic layer of mercury telluride colloidal quantum dots. The spin-coating method was selected as 1000r-20s+300r-10s. Then, the ink was treated with a methanol solution of HgCl2 for 10s. The residual HgCl2 was rinsed with isopropanol, and the excess isopropanol was removed by spin-coating machine.

[0088] (6) Preparation of hole transport layer: PEDOT:PSS solution was spin-coated on the silver telluride colloidal quantum dot doped layer. The spin-coating method was 3000r-60s, and then the layer was placed on a hot plate at 60℃ for annealing for 20min.

[0089] (7) Encapsulating the top electrode: depositing nano-gold on top of the hole transport layer to form a top electrode with a thickness of about 40 nm.

[0090] Example 5

[0091] This embodiment discloses a focal plane array, which includes first selecting a focal plane array substrate, then fabricating a readout circuit on the substrate surface, and arranging a plurality of pixels prepared in Embodiment 5 above on the readout circuit surface. Both the substrate and the readout circuit are made of materials commonly used in the art. The array is then housed in a casing, specifically by connecting the electrodes on the readout circuit to pins on the package casing using leads. These pins are then connected to other devices via wires on a printed circuit board, thereby achieving the connection between the internal chip and the external circuitry.

[0092] The focal plane array designed in this invention can achieve detection of both visible and infrared wavelengths.

[0093] like Figure 5 As shown, this figure is the equivalent circuit diagram of the aforementioned array device.

[0094] This invention adopts a dual-end configuration, which enables the detection of both visible and infrared wavelengths by providing different bias voltages in different bands.

[0095] The invention was designed to obtain Figure 2 The array device shown operates in the visible light region (390 nm–760 nm) and the short-wave infrared region (1.5 μm–2.5 μm), at room temperature, with a pixel responsivity of 0.5 A / W and a pixel detectivity of 1 × 10⁻⁶. 11 Jones, with a power conversion efficiency of 12%. The pixel responsivity, pixel detectivity, and power conversion efficiency were calculated according to the formulas specified in the People's Republic of China National Standard GB / T17444-1998 "Technical Specification for Testing Characteristic Parameters of Infrared Focal Plane Arrays".

[0096] In summary, the fabrication method designed in this invention is relatively simple, low-cost, and has a high yield. Furthermore, the resulting detector not only possesses the advantages of visible light and infrared detection but also exhibits high photoelectric conversion efficiency and good device efficiency. Specifically, the pixel responsivity is not less than 0.5 A / W, and the pixel detectivity is 0.1–10 × 10⁻⁶. 11 Jones, with a power conversion efficiency of no less than 12%.

[0097] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0098] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments described herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A non-inverted bonded dual-band quantum dot pixel, characterized in that, The pixel includes a bottom electrode, a top electrode, and a hole transport layer, an infrared photosensitive film layer, and a visible light photosensitive film layer located between the top electrode and the bottom electrode. The infrared photosensitive film layer includes an intrinsic layer of chalcogenide mercury colloidal quantum dots and a doped layer of chalcogenide silver colloidal quantum dots. The visible light photosensitive film layer includes an electron transport layer and a cadmium telluride colloidal quantum dot layer. The hole transport layer is located between the top electrode and the infrared photosensitive film layer; The visible light photosensitive film layer is located between the infrared photosensitive film layer and the bottom electrode; The chalcogenide silver colloidal quantum dot doping layer is located between the hole transport layer and the chalcogenide mercury colloidal quantum dot intrinsic layer; The electron transport layer is located between the intrinsic layer of the chalcogenide mercury colloidal quantum dot and the cadmium telluride colloidal quantum dot layer; Furthermore, the chalcogenide silver colloidal quantum dot doped layer, the chalcogenide mercury colloidal quantum dot intrinsic layer, the electron transport layer, and the cadmium telluride colloidal quantum dot layer constitute a PNP heterojunction.

2. The non-inverted bonded dual-band quantum dot pixel according to claim 1, characterized in that, The electron transport layer is made of any one of cadmium selenide, cadmium sulfide, or zinc oxide.

3. The non-inverted bonded dual-band quantum dot pixel according to claim 1, characterized in that, The hole transport layer is made of DMSO and NiO. x Or any of PEDOT:PSS.

4. The non-inverted bonded dual-band quantum dot pixel according to any one of claims 1 to 3, characterized in that, The thickness of the chalcogenide silver colloidal quantum dot doping layer is less than that of the intrinsic chalcogenide mercury colloidal quantum dot layer, and the thickness of the electron transport layer is less than that of the cadmium telluride colloidal quantum dot layer.

5. The non-inverted bonded dual-band quantum dot pixel according to claim 4, characterized in that, The bottom electrode is made of an infrared transparent conductive material composited on a silicon substrate, and the top electrode is made of a metallic conductive material.

6. The non-inverted bonded dual-band quantum dot pixel according to claim 5, characterized in that, The pixel, from bottom to top, is composed of an ITO layer, a cadmium telluride colloidal quantum dot layer, a zinc oxide layer, a mercury telluride colloidal quantum dot intrinsic layer, a silver telluride colloidal quantum dot doped layer, a PEDOT:PSS layer, and a gold electrode, all stacked on a silicon substrate. The cadmium telluride colloidal quantum dot layer has a thickness of 400-600 nm, the zinc oxide layer has a thickness of 30-50 nm, the mercury telluride colloidal quantum dot intrinsic layer has a thickness of 400-600 nm, the silver telluride colloidal quantum dot doped layer has a thickness of 30-50 nm, the PEDOT:PSS layer has a thickness of 30-50 nm, and the gold electrode has a thickness of 30-50 nm.

7. A method for fabricating a non-inverted bonded dual-band quantum dot pixel, characterized in that, It includes the following steps: 1) Select the bottom electrode; 2) Preparation of cadmium telluride colloidal quantum dot layer: Coat the upper surface of the bottom electrode with cadmium telluride colloidal quantum dot ink, then place it on a hot plate for a period of time, then immerse it in a saturated CdCl2 solution for treatment, take it out and rinse off the excess CdCl2 solution with isopropanol, and continue to place it on a hot plate for sintering. Repeat the whole process multiple times to obtain cadmium telluride colloidal quantum dot layer. 3) Preparation of electron transport layer: Take electron transport layer solution and coat it on the upper surface of cadmium telluride colloidal quantum dot layer in step 1), and then place it on a hot plate for annealing to obtain electron transport layer; 4) Preparation of the intrinsic layer of sulfide-based mercury colloidal quantum dots: The upper surface of the electron transport layer prepared in step 3) is coated with sulfide-based mercury colloidal quantum dot ink, and then 1,2-ethanedithiol is added dropwise for a period of time. The excess 1,2-ethanedithiol is washed away with isopropanol, and then a methanol solution of HgCl2 is added dropwise for treatment. The excess HgCl2 is washed away with isopropanol, and the excess isopropanol is removed by spin coating. The whole process is repeated multiple times to obtain the sulfide-based mercury colloidal quantum dot layer. 5) Preparation of chalcogenide silver colloidal quantum dot doped layer: The chalcogenide mercury colloidal quantum dot intrinsic layer prepared in step 4) is coated with chalcogenide silver colloidal quantum dot ink, then treated in methanol solution of HgCl2, and after removal, the residual HgCl2 is washed away with isopropanol, and the excess isopropanol is removed by spin coating machine; thus, chalcogenide silver colloidal quantum dot doped layer is obtained. 6) Preparation of hole transport layer: The hole transport layer solution is coated on the upper surface of the chalcogenide silver colloidal quantum dot doped layer prepared in step 5), and then placed on a hot plate for annealing to obtain the hole transport layer. 7) Encapsulating the top electrode: A metal conductive material is vapor-deposited on the upper surface of the hole transport layer prepared in step 6) to form the top electrode.

8. The method for preparing a non-inverted bonded dual-band quantum dot pixel according to claim 7, characterized in that, The coating method includes one or more of the following: drop coating, spray coating, spin coating, scraping, or ink printing.

9. A non-inverted bonded dual-band quantum dot focal plane array, characterized in that, It includes a readout circuit and a plurality of non-inverted bonded dual-band quantum dot pixels of any one of claims 1 to 6 or claim 7 arranged in a row and column array on the readout circuit.

10. The application of the non-inverted bonded dual-band quantum dot focal plane array as described in claim 9 in visible light 390nm~760nm and / or short-wave infrared 1.5um~2.5um.

Citation Information

Patent Citations

  • Imaging device, preparation method thereof, imaging array and preparation method thereof

    CN114551486A