Maleimide resin and method for producing the same, maleimide solution, curable resin composition and cured product thereof
By optimizing the composition and processing methods of maleimide resin, the problem of insufficient dielectric properties in the high-frequency region is solved, the application in high-speed communication technology is realized, and the hygroscopicity and heat resistance are improved.
Patent Information
- Application Number
- CN202180016765.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-05
AI Technical Summary
Existing maleimide resins have insufficient dielectric properties in the high-frequency region and cannot meet the needs of high-speed communications. Moreover, their electrical properties greatly deteriorate after absorbing moisture in the air, and their application range is limited.
By optimizing the composition of maleimide resin, ensure the content and location of N,N'-(phenylenebis(2,2-propylene)diphenylene)bismaleimide. Xiangbi, combined with specific hardening accelerators and solvent systems, improves its solvent solubility and high-frequency electrical properties.
We have realized a maleimide resin with excellent electrical properties in the high-frequency region, which is suitable for high-speed communication technology and has good hygroscopicity and heat resistance.
Smart Images

Figure CN115210293B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a maleimide resin and a method for producing the same, a maleimide solution, a curable resin composition and a cured product thereof. The present invention can be preferably used in semiconductor sealing materials, printed wiring boards, build-up laminates and other electrical and electronic parts, carbon fiber reinforced plastics, glass fiber reinforced plastics and other lightweight and high-strength materials. Background Art
[0002] In recent years, the required characteristics of laminated boards equipped with electrical and electronic components have become wider and more advanced due to the expansion of their application areas. For example, existing semiconductor chips are mainly mounted on metal lead frames, while in recent years, semiconductor chips with high processing power such as CPUs are mostly mounted on laminated boards made of polymer materials. With the development of high-speed components such as CPUs and the increase in clock frequency, the problems of signal transmission delay and propagation loss have also increased, and low dielectric constant and low dielectric loss tangent are required for wiring boards. In particular, due to the prevalence of 5G in recent years, not only Sub6, but also the electrical characteristics of quasi-millimeter waves and millimeter waves above 10GHz, especially above 28GHz, have begun to receive attention, requiring materials that can be used stably in these ranges. At the same time, as the heat generation of the chip increases with the speed of the components, it is also necessary to improve heat resistance.
[0003] In addition, due to the popularity of mobile electronic devices such as mobile phones, precision electronic devices have been used and carried in outdoor environments and extremely close to the human body, so they need to be resistant to external environments (especially resistant to humid and hot environments). Furthermore, in the automotive field, electrification is developing rapidly, and precision electronic devices are sometimes also configured near the engine, and heat resistance and moisture resistance are required at a higher level. In addition, since precision electronic devices are used in automobiles and mobile devices, safety such as flame retardancy is also more important. However, due to the increase in environmental awareness in recent years, the use of halogen flame retardants is avoided. Therefore, the necessity of imparting flame retardancy without using halogens has increased.
[0004] Conventionally, wiring boards using a resin obtained by combining a bisphenol A-type cyanate ester compound with a bismaleimide compound, i.e., BT resin, as described in Patent Document 1, have been widely used as high-performance wiring boards due to their excellent heat resistance, chemical resistance, electrical properties, etc. However, in situations where higher performance is required as described above, improvements are required.
[0005] In addition, in recent years, from the perspective of energy saving, the lightweighting of aircraft, automobiles, trains, ships, etc. is being promoted. In particular, in the field of transportation, lightweight and high-strength carbon fiber composite materials are being studied to replace the metal materials previously used. For example, in the Boeing 787, lightweighting is achieved by increasing the ratio of composite materials, thereby greatly improving fuel efficiency. In the aviation field, in order to further achieve lightweighting, there is also a trend of introducing carbon fiber composite materials into the components around the engine, and naturally a high level of heat resistance is required. In the automotive field, some propeller shafts made of composite materials are equipped, and there is also a trend of using composite materials to make car bodies for high-end cars. In the past, in the field of carbon fiber composite materials, composite materials were used, and the materials used were bisphenol A type diglycidyl ether or tetraglycidyl diaminodiphenylmethane of epoxy resin, as well as diaminodiphenylmethane, diaminodiphenyl sulfone, etc. as hardeners, but in order to further promote lightweighting and high heat resistance, it is necessary to expand the application of composite materials. As one of the means, maleimide resins are being studied for the materials used for this purpose.
[0006] In this case, the maleimide compounds or bismaleimide resins available on the market have greatly improved heat resistance compared to the epoxy resins used previously, and there is a strong demand for their use as described above, but their dielectric properties, especially the dielectric properties in the high-frequency region, are not sufficient to meet the needs of high-speed communication. Furthermore, there is a problem that the electrical properties are greatly deteriorated due to the absorption of moisture in the air, and their application range is limited.
[0007] In this regard, maleimide resins such as those disclosed in Patent Documents 2 and 3 have been developed, but they are still far from being sufficient.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Publication No. 54-30440
[0011] Patent Document 2: Japanese Patent Application Laid-Open No. 3-100016
[0012] Patent Document 3: Japanese Patent Application Publication No. 2009-1783
[0013] Patent Document 4: Japanese Patent Publication No. 4-75222
[0014] Patent document 5: Japanese Patent Publication No. 6-37465. Summary of the invention
[0015] [Problems to be solved by the invention]
[0016] The present invention provides a maleimide resin having excellent solvent solubility and excellent electrical properties even in a high-frequency region, which is particularly helpful for the development of high-speed communication technologies represented by 5G.
[0017] [Technical means to solve the problem]
[0018] The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the present invention.
[0019] That is, the present invention relates to the following [1] to [7]. [1]
[0021] A maleimide resin represented by the following formula (1), and
[0022] In the maleimide resin, the content of N,N'-(phenylenebis(2,2-propylene)diphenylene)bismaleimide is 98 area % or less in terms of GPC area percentage,
[0023] The content of the maleimide compound represented by the following formula (2) in the N,N′-(phenylenebis(2,2-propylene)diphenylene)bismaleimide is 30 area % or more and less than 60 area % in terms of HPLC area percentage.
[0024]
[0025] (In formula (1), n is the number of repetitions, and its average value is 1<n<5)
[0026] [2]
[0028] The maleimide resin of the above item [1], wherein in the above N,N'-(phenylenebis(2,2-propylene)diphenylene)bismaleimide, the area ratio (O / P) of the ortho position to the para position obtained by HPLC area percentage is 100% or more and less than 200%. [3]
[0030] The maleimide resin as described in the above item [1] or [2], wherein the content of the maleimide compound represented by the following formula (3) in the above N,N'-(phenylenebis(2,2-propylene)diphenylene)bismaleimide is less than 50 area % in terms of HPLC area percentage.
[0031] [4]
[0033] A maleimide solution comprising the maleimide resin according to any one of the above items [1] to [3] and an organic solvent, wherein the organic solvent is at least one selected from ketones, hydrocarbons, and esters. [5]
[0035] A curable resin composition comprising the maleimide resin according to any one of the above items [1] to [3], or the maleimide solution according to the above item [4], and further comprising a curing accelerator. [6]
[0037] A cured product obtained by curing the maleimide resin according to any one of the above items [1] to [3] or the curable resin composition according to the above item [5]. [7]
[0039] A method for producing a maleimide resin as described in any one of the preceding items [1] to [3], comprising: adding 1 to 12 wt % of a protonic acid relative to the total amount of aniline to aniline and diisopropylbenzene or di(α-hydroxyisopropyl)benzene, and reacting at 140 to 190° C. to obtain an aromatic amine resin; and subjecting the aromatic amine resin to maleimide treatment.
[0040] [Effects of the Invention]
[0041] The maleimide resin of the present invention has excellent solvent solubility and its cured product also has excellent electrical properties in a high frequency region, and can be used in various applications such as electronic materials and structural materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] [ Figure 1 ] is a graph showing the change in elastic modulus of the hardened materials of Example 15 and Comparative Examples 8 to 9 according to temperature. DETAILED DESCRIPTION
[0043] Hereinafter, one embodiment of the present invention will be described in detail.
[0044] The maleimide resin of the present embodiment is represented by the following formula (1).
[0045]
[0046] (In formula (1), n is the number of repetitions, and its average value is 1<n<5)
[0047] In formula (1), the value of n can be calculated from the number average molecular weight determined by gel permeation chromatography (GPC, detector: RI) of maleimide resin or the area ratio of each separated peak. n is usually 1<n<5, more preferably 1<n<3.
[0048] When the average value n is 1, the solubility in the solvent is low, causing the crystal to precipitate. On the other hand, when the average value n is 5 or more, the fluidity during molding is poor, causing the problem that the properties as a cured product cannot be exhibited.
[0049] In the formula (1) of the maleic imide resin of the present embodiment, the content of N,N'-(phenylene di(2,2-propylene) diphenylene) bismaleic imide as the n=1 body obtained by GPC analysis (RI) is 98 area % or less, preferably 20 to 90 area %, more preferably 30 to 80 area %, further preferably 40 to 75 area %, and most preferably in the range of 40 to 70 area %. When the content of the n=1 body is 98 area % or less, the heat resistance is good. In addition, the crystallinity is reduced and the solvent solubility is good. On the other hand, when the lower limit of the n=1 body is 20 area % or more, the viscosity of the resin solution is reduced and the impregnation is good. In addition, since the solvent can be removed at low temperature when taken out as a solid, self-polymerization is not easy to occur and it is easy to handle.
[0050] The area % can be measured by GPC (gel permeation chromatography). In the present embodiment, the area % is measured under the following conditions.
[0051] GPC analysis
[0052] GPC: DGU-20A3R, LC-20AD, SIL-20AHT, RID-20A, SPD-20A, CTO-20A, CBM-20A (all manufactured by Shimadzu Corporation)
[0053] Column: Shodex KF-603, KF-602×2, KF-601×2
[0054] Linking eluent: tetrahydrofuran
[0055] Flow rate: 0.5ml / min
[0056] Column temperature: 40℃
[0057] Detection: RI (differential refractive index detector).
[0058] The softening point of the maleimide resin of the present embodiment is preferably 50°C to 150°C, more preferably 80°C to 120°C, further preferably 90°C to 120°C, and particularly preferably 95°C to 120°C. In addition, the melt viscosity at 150°C is 0.05 to 100 Pa·s, preferably 0.1 to 40 Pa·s. However, there is a case where this value is exceeded due to high molecular weight during polymerization when the solvent is removed. The preferred range is an indicator when the change in area % in GPC with n=1 during solidification from a solution state is less than 3 area %.
[0059] The acid value of the maleimide resin of this embodiment is preferably 30 mg KOH / g, more preferably 1 to 15 mg KOH / g. If the acid value is high, more molecules are not maleimide-modified and the structure having carboxylic acid is excessive, which affects electrical properties and water resistance.
[0060] The maleimide resin of the present embodiment contains maleimide compounds represented by the following formulas (2) to (4) as positional isomers of N,N′-(phenylenebis(2,2-propylene)diphenylene)bismaleimide in which n=1 in the above formula (1).
[0061]
[0062] The content of each of the maleimide compounds represented by the above formulae (2) to (4) in N,N′-(phenylenebis(2,2-propylene)diphenylene)bismaleimide is preferably as follows in terms of HPLC area percentage.
[0063] About the maleimide compound represented by the above-mentioned formula (2), it is 30 area % or more and less than 60 area %, preferably 35 area % or more and less than 55 area %, and further preferably 40 area % or more and less than 55 area %. By making the present compound with asymmetric structure more than 30 area %, solvent solubility is improved, and dielectric properties are improved. On the other hand, since it is necessary to remove the maleimide compound represented by the above-mentioned formula (3) by crystallization, for example, additional steps are required to make the content ratio more than 60 area %, so it is not good in terms of the aspects of rising manufacturing costs and increasing industrial waste.
[0064] The content of the maleimide compound represented by the above formula (3) is preferably less than 50 area %, more preferably 2 area % or more and less than 35 area %, and preferably 5 area % or more and less than 30 area %. When the content is less than 50 area %, the solvent solubility is improved and the electrical properties are also good.
[0065] The content of the maleimide compound represented by the above formula (4) is preferably 15% by area or more and less than 60% by area, and more preferably 25% by area or more and less than 50% by area. By making the content 15% by area or more, the dielectric properties are good, and by making the content less than 60% by area, the hardenability and adhesion are good, and the defects when manufacturing the substrate etc. can be suppressed.
[0066] Furthermore, since the maleic imide compound represented by the above formula (3) has the greatest influence on the problem of crystallinity and the problem of deterioration of electrical characteristics, the total ratio of the maleic imide compound represented by formula (2) and the maleic imide compound represented by formula (4) in N,N'-(phenylene di(2,2-propylene) diphenylene) bismaleic imide is preferably 50 area % or more, more preferably 60 area % or more, and particularly preferably 70 area % or more.
[0067] In N,N′-(phenylenebis(2,2-propylene)diphenylene)bismaleimide, the area ratio (O / P) of the ortho position to the para position is preferably 50% or more and less than 300%, and more preferably 100% or more and less than 200%.
[0068] When the area ratio (O / P) is 50% or more, the solvent solubility and electrical properties are good. When the area ratio (O / P) is less than 300%, problems such as increased manufacturing costs and increased industrial waste do not occur.
[0069] In addition, the area ratio (O / P) of the ortho direction to the para direction was calculated by the following formula.
[0070] The area ratio of the ortho position to the para position (O / P) = (area % of the maleic imide compound represented by the above formula (4)) × 2 + (area % of the maleic imide compound represented by the above formula (2)) / (area % of the maleic imide compound represented by the above formula (3)) × 2 + (area % of the maleic imide compound represented by the above formula (2)).
[0071] The above content rate can be measured by HPLC (high performance liquid chromatography), and in this embodiment, the measurement is performed under the following conditions.
[0072] HPLC analysis
[0073] Infusion Unit LC-20AD manufactured by Shimadzu Corporation
[0074] Photodiode array detector SPD-M20A manufactured by Shimadzu Corporation
[0075] Column oven CTO-20A manufactured by Shimadzu Corporation
[0076] Column: Intersil ODS-2.5μm, 4.6×250mm, 40℃
[0077] Mobile phase A: acetonitrile (AN)
[0078] Mobile phase B: Water (W)
[0079] Time program:
[0080] 0-28min.AN / W=30% / 70%→100% / 0%
[0081] 28-40min.AN / W=100% / 0%
[0082] Flow rate: 1.0mL / min
[0083] Detection: UV 200-274nm, PDA
[0084] Measurement wavelength: 225nm.
[0085] The measurement wavelength of HPLC is preferably in the range of 210 to 230 nm. The reason is that although the measurement can be performed at other wavelengths, sometimes the actual content is far different due to the difference in the absorption wavelength. In addition, the ratio can also be calculated by NMR. When using NMR, it can be used 13 The ratio was calculated from the peak intensity ratio of the isopropylidene group appearing at 1 to 2 ppm by C-NMR.
[0086] The maleimide resin of one embodiment of the present invention has high solubility in solvents and other resins, and can be treated as a maleimide solution (hereinafter also referred to as varnish) or a curable resin composition. In addition, the cured product of the maleimide resin of one embodiment of the present invention has excellent electrical properties, heat resistance, weather resistance, hygroscopicity, and flame retardancy.
[0087] As the solvent that can be used, for example, ketones such as acetone, methyl ethyl ketone, and cyclohexanone; hydrocarbons such as benzene, toluene, xylene, tetramethylbenzene, and cyclohexane; glycol ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, triethylene glycol dimethyl ether, and triethylene glycol diethyl ether; esters such as ethyl acetate, butyl acetate, methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, carbitol acetate, propylene glycol monomethyl ether acetate, dialkyl glutarate, dialkyl succinate, and dialkyl adipate; cyclic esters such as γ-butyrolactone; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent petroleum naphtha, etc. Among these, ketones, hydrocarbons, and esters are preferred, and hydrocarbons are further preferred, and aromatic hydrocarbons are particularly preferred. These can be used alone or in combination of two or more. The solvent is used in a range of 10 to 80% by weight, preferably 20 to 70% by weight, in the obtained varnish, in terms of solid content concentration excluding the solvent.
[0088] Furthermore, although a maleimide solution can be prepared by dissolving a maleimide resin in a solvent, it is preferred that the solvent used in the synthesis be directly used as the maleimide solution because industrial waste and energy consumption can be reduced.
[0089] Next, a method for producing the maleimide resin of the present embodiment will be described, but the present invention is not limited to this production method.
[0090] [Method for producing aromatic amine resin]
[0091] The maleimide resin of the present embodiment can use an aromatic amine resin represented by the following formula (5) as a precursor.
[0092]
[0093] (In formula (5), n is the number of repetitions, and its average value is 1<n<5)
[0094] The method for producing the aromatic amine resin represented by the above formula (5) is not particularly limited. For example, Patent Document 4 discloses the following: Aniline is reacted with m-diisopropylbenzene or m-di(α-hydroxyisopropyl)benzene at 180 to 250° C. in the presence of an acidic catalyst, thereby obtaining the n=1 isomer in the above formula (5) as a main component. The n=1 isomer includes three isomers, namely, 1-(o-aminoisopropylphenyl)-3-(p-aminoisopropylphenyl)benzene represented by the following formula (6), 1,3-bis(p-aminoisopropylphenyl)benzene represented by the following formula (7), and 1,3-bis(o-aminoisopropylphenyl)benzene represented by the following formula (8).
[0095]
[0096] In Patent Document 4, the n=2 to 5 isomers contained as secondary components are further purified by crystallization to obtain 1,3-bis(p-aminoisopropylphenyl)benzene with a purity of 98%. In Patent Document 5, 1,3-bis(p-aminoisopropylphenyl)benzene is imidized to synthesize N,N'-(1,3-phenylenebis(2,2-propylene)di-p-phenylene)bismaleimide, thereby obtaining a crystalline product. However, in order to dissolve it in a solvent, it is necessary to heat it. If it is left at room temperature after heating, crystals will precipitate in a few hours. Therefore, there is also the possibility of crystallization when adjusting the resin composition. The higher the concentration of N,N'-(1,3-phenylenebis(2,2-propylene)di-p-phenylene)bismaleimide, the higher the possibility of crystallization. In order to manufacture printed wiring boards and composite materials, glass cloth or carbon fiber is impregnated with varnish to adhere the resin. However, if crystals precipitate, the impregnation operation cannot be performed. On the other hand, if the temperature is increased to maintain the dissolved state, the reaction of the composition will be accelerated and the usable time of the varnish will be shortened.
[0097] In the production method according to one embodiment of the present invention, by synthesizing the maleimide resin using an amine resin having a molecular weight distribution and containing an asymmetric amine, the solvent solubility and the dielectric properties of the cured product thereof can be improved.
[0098] In the aromatic amine resin represented by the above formula (5), the aromatic amine compound represented by the above formula (6) is preferably 30 area % or more and less than 60 area % in terms of HPLC area percentage, more preferably 30 area % or more and less than 55 area % and particularly preferably 35 area % or more and less than 50 area % in terms of HPLC area percentage.
[0099] When synthesizing the aromatic amine resin represented by the above formula (5), the acidic catalyst used can be listed as: hydrochloric acid, phosphoric acid, sulfuric acid, formic acid, zinc chloride, ferric chloride, aluminum chloride, p-toluenesulfonic acid, methanesulfonic acid and the like. In the present embodiment, protonic acids such as hydrochloric acid, p-toluenesulfonic acid, and methanesulfonic acid are preferred. These can be used alone or in combination of two or more. The amount of the catalyst used is generally 1 to 30% by weight, preferably 1 to 17% by weight, more preferably 1 to 12% by weight, and particularly preferably 1 to 7% by weight relative to the aniline used. If the amount of the catalyst used is too much, the target asymmetric structure compound is less, and a compound with a symmetric structure is preferentially formed. If the amount of the catalyst used is too little, not only the reaction is slowed down, but also the reaction cannot be completed, so it is not good.
[0100] Regarding the reaction, as needed, it can be carried out using organic solvents such as toluene and xylene, or it can be carried out without a solvent. For example, after an acidic catalyst is added to a mixed solution of aniline and a solvent, when the catalyst contains water, it is preferably removed from the system by azeotropy. Thereafter, after adding diisopropylbenzene or di(α-hydroxyisopropyl)benzene, the solvent is removed from the system, and the temperature is raised at the same time, and the reaction is carried out at 140 to 190°C, preferably 160 to 190°C for 5 to 50 hours, preferably 5 to 30 hours. When the reaction temperature is too high, the asymmetric structure will recombine after generation, and a symmetric structure will be preferentially formed, so the target solvent solubility and electrical properties cannot be exerted. Since byproduct water is produced when di(α-hydroxyisopropyl)benzene is used, water and the solvent are azeotropically removed from the system at the same time when the temperature is raised. After the reaction is completed, the acidic catalyst is neutralized by an alkaline aqueous solution, and a water-insoluble organic solvent is added to the oil layer, and the wastewater is repeatedly washed with water until the wastewater becomes neutral. Thereafter, the solvent and excess aniline derivative are removed under heating and reduced pressure. When activated clay or ion exchange resin is used, the reaction solution is filtered after the reaction is completed to remove the catalyst.
[0101] In addition, since diphenylamine may be produced as a byproduct depending on the reaction temperature and the type of catalyst, it is preferred to remove diphenylamine as needed. The diphenylamine derivative may be removed to less than 1 wt %, preferably less than 0.5 wt %, and more preferably less than 0.2 wt % under high temperature and high vacuum or by means of steam distillation.
[0102] The maleimide resin of the present embodiment is obtained, for example, by subjecting the aromatic amine resin represented by the above formula (5) to addition reaction or dehydration condensation reaction with maleic acid or maleic anhydride (hereinafter also referred to as "maleic anhydride") in the presence of a solvent and a catalyst.
[0103] [Method for producing maleimide resin]
[0104] As for the solvent used in the reaction, a water-insoluble solvent is used because water generated in the reaction needs to be removed from the system. Examples of the water-insoluble solvent include aromatic solvents such as toluene and xylene; aliphatic solvents such as cyclohexane and n-hexane; ethers such as diethyl ether and diisopropyl ether; ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as methyl isobutyl ketone and cyclopentanone, but the solvents are not limited to these, and two or more solvents may be used in combination.
[0105] In addition to the above-mentioned non-water-soluble solvents, aprotic polar solvents may also be used in combination. Examples include dimethyl sulfone, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, etc., and two or more thereof may be used in combination. When aprotic polar solvents are used, it is preferred to use a solvent with a higher boiling point than the non-water-soluble solvent used in combination.
[0106] In addition, the catalyst used in the reaction is an acidic catalyst, which is not particularly limited, and examples thereof include p-toluenesulfonic acid, hydroxy-p-toluenesulfonic acid, methanesulfonic acid, sulfuric acid, phosphoric acid, etc. The amount of the acidic catalyst used is generally 0.1 to 10% by weight, preferably 1 to 5% by weight, relative to the aromatic amine resin. When the acid catalyst is more, the para orientation becomes stronger, and there is a concern that the crystallinity and dielectric properties are adversely affected.
[0107] For example, the aromatic amine resin represented by the above formula (5) is dissolved in toluene and N-methyl-2-pyrrolidone, maleic anhydride is added thereto to generate amic acid, and then p-toluenesulfonic acid is added while the reaction is carried out while removing water generated under reflux conditions from the system.
[0108] Alternatively, maleic anhydride is dissolved in toluene, and an N-methyl-2-pyrrolidone solution of the aromatic amine resin represented by the above formula (5) is added under stirring to generate amic acid, and then p-toluenesulfonic acid is added to remove water generated under reflux conditions from the system while the reaction is carried out.
[0109] Alternatively, maleic anhydride is dissolved in toluene, p-toluenesulfonic acid is added, and a solution of an aromatic amine resin represented by the above formula (5) in N-methyl-2-pyrrolidone is added dropwise under stirring and reflux, and at the same time, water produced by azeotropy during the process is removed from the system, and toluene is returned to the system, and the reaction is carried out simultaneously (the above is the first stage reaction).
[0110] In any method, maleic anhydride is usually used in an amount of 1 to 3 equivalents, preferably 1.2 to 2.0 equivalents, based on the amine groups of the aromatic amine resin represented by the above formula (5).
[0111] In order to reduce the unclosed-loop amic acid, after the maleimide reaction listed above, water is added to the reaction solution to separate it into a resin solution layer and a water layer. Excess maleic acid or maleic anhydride, aprotic polar solvent, and catalyst are dissolved on the water layer side, so they are separated and removed, and the same operation is repeated to thoroughly remove the excess maleic acid or maleic anhydride, aprotic polar solvent, and catalyst. It is also possible to add a catalyst to the maleimide resin solution of the organic layer from which the excess maleic acid or maleic anhydride, aprotic polar solvent, and catalyst have been removed again, and the dehydration ring-closure reaction of the residual amic acid under heating reflux conditions is performed again (the above is the second stage reaction). By carrying out this method, a maleimide resin solution with a lower acid value can be obtained, but in this embodiment, it is also OK even if only the first stage reaction is performed.
[0112] The time of the dehydration ring-closure reaction is usually 1 to 5 hours, preferably 1 to 3 hours, and the above-mentioned aprotic polar solvent can also be added as needed. After the reaction is completed, it is cooled and repeatedly washed with water until the washing water becomes neutral. Thereafter, after removing water by azeotropic dehydration under heating and reduced pressure, the solvent can be distilled off, or other solvents can be added to adjust the resin solution to the desired concentration. The solvent can also be completely distilled off to make a solid resin and take it out.
[0113] Next, the curable resin composition of the present embodiment will be described.
[0114] The curable resin composition of the present embodiment may contain a compound capable of undergoing a cross-linking reaction with the maleimide resin of the present embodiment. The compound is not particularly limited as long as it is a compound having a functional group (or structure) capable of undergoing a cross-linking reaction with the maleimide resin, such as an amino group, a cyanate group, a phenolic hydroxyl group, an alcoholic hydroxyl group, an allyl group, a methallyl group, an acryloyl group, a methacryloyl group, a vinyl group, or a conjugated diene group.
[0115] Since the amine compound and the maleimide compound undergo a crosslinking reaction, the aromatic amine resin represented by the above formula (5) can be used. Since the maleimide resin can also self-polymerize, it can also be used alone. In addition, an amine compound other than the aromatic amine resin represented by the above formula (5) or a maleimide compound other than the maleimide resin represented by the above formula (1) can also be used in combination.
[0116] The content of the maleimide resin represented by the above formula (1) in the curable resin composition of the present embodiment is preferably 10 wt % or more, more preferably 15 wt % or more, and further preferably 20 wt %. In the case of the above range, the physical properties of the cured product tend to be high in mechanical strength, peel strength, and heat resistance.
[0117] As the amine compound that can be blended into the curable resin composition of the present embodiment, a previously known amine compound can be used. Specific examples of the amine compound include diethylenetriamine, triethylenetetramine, tetraethylenepentamine, meta-xylylenediamine, trimethylhexamethylenediamine, 2-methylpentanediamine, diethylaminopropylamine, isophoronediamine, 1,3-bisaminomethylcyclohexane, bis(4-aminocyclohexyl)methane, bis(4-amino-3-methylcyclohexyl)methane, norbornenediamine, 1,2-diaminocyclohexane, diaminodiphenylmethane, meta-phenylenediamine, diaminodiphenylsulfone, dicyandiamide, polyoxypropylenediamine, polyoxypropylenetriamine, N-aminoethylpiperazine, aniline-formalin resin, etc., but are not limited to these. These can be used alone or in combination of two or more.
[0118] Furthermore, the aromatic amine resin described in the claims of Patent Document 3 is particularly preferred because of its low hygroscopicity, flame retardancy, and excellent dielectric properties.
[0119] As the maleimide compound that can be blended into the hardenable resin composition of the present embodiment, a conventionally known maleimide compound can be used. Specific examples of maleimide compounds include 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, metaphenylene bismaleimide, 2,2'-bis[4-(4-maleimide phenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenyl sulfone bismaleimide, 1,3-bis(3-maleimide phenoxy)benzene, 1,3-bis(4-maleimide phenoxy)benzene, etc., but are not limited thereto. These may be used alone or in combination of two or more. The blending amount of the maleimide compound is preferably within a range of 5 times or less, and more preferably within a range of 2 times or less, the maleimide resin of the present embodiment in terms of weight ratio.
[0120] Furthermore, the maleimide resin described in the claims of Patent Document 3 is particularly preferred because of its low hygroscopicity, flame retardancy, and excellent dielectric properties.
[0121] As the cyanate compound that can be incorporated into the curable resin composition of the present embodiment, a previously known cyanate compound can be used. As specific examples of the cyanate compound, cyanate compounds obtained by reacting condensation products of phenols and various aldehydes, polymers of phenols and various diene compounds, condensation products of phenols and ketones, and condensation products of bisphenols and various aldehydes with cyanogen halides can be cited, but the present invention is not limited to these. These can be used alone or in combination of two or more.
[0122] Examples of the phenols include phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, and dihydroxynaphthalene.
[0123] Examples of the various aldehydes include formaldehyde, acetaldehyde, alkyl aldehydes, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, and cinnamaldehyde.
[0124] Examples of the various diene compounds include dicyclopentadiene, terpenes, vinylcyclohexene, norbornene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, and isoprene.
[0125] Examples of the ketones include acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, and phenyl ketone.
[0126] Furthermore, cyanate compounds whose synthesis method is described in Japanese Patent Application Laid-Open No. 2005-264154 are particularly preferred as cyanate compounds because of their low hygroscopicity, flame retardancy, and excellent dielectric properties.
[0127] The curable resin composition of the present embodiment may be further blended with an epoxy resin. As the epoxy resin that can be blended, any epoxy resin known in the prior art may be used. Specific examples of epoxy resins include: glycidyl ether epoxy resins obtained by glycidylating condensation products of phenols and various aldehydes, polymers of phenols and various diene compounds, condensation products of phenols and ketones, condensation products of bisphenols and various aldehydes, and alcohols; alicyclic epoxy resins represented by 4-vinyl-1-cyclohexene diepoxide, 3,4-epoxycyclohexylmethyl-3,4'-epoxycyclohexanecarboxylate, etc.; glycidylamine epoxy resins represented by tetraglycidyldiaminodiphenylmethane (TGDDM), triglycidyl para-aminophenol, etc.; glycidyl ester epoxy resins, etc., but are not limited to these. These may be used alone or in combination of two or more.
[0128] In addition, a phenol aralkyl resin obtained by condensing phenols with a dihalogenated methyl aralkyl derivative or an aralkyl alcohol derivative is used as a raw material, and then subjected to a dehydrochlorination reaction with epichlorohydrin to obtain an epoxy resin. The epoxy resin obtained in this way has low hygroscopicity, flame retardancy, and excellent dielectric properties, so it is particularly preferred as an epoxy resin.
[0129] When epoxy resin is added, the amount is not particularly limited, but is preferably 0.1 to 10 times, more preferably 0.2 to 4 times, of the maleimide resin in terms of weight ratio. If the epoxy resin is added in an amount less than 0.1 times of the maleimide resin, there is a concern that the cured product may become brittle, and if it exceeds 10 times, there is a concern that the dielectric properties may be reduced.
[0130] The curable resin composition of the present embodiment may further contain a compound having a phenol resin.
[0131] As the phenolic resin that can be blended, any phenolic resin known in the art can be used. Specific examples of the phenolic resin include: bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.), polycondensates of phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehydes, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.); polycondensates of phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornene, vinylnorbornene, tetrahydroindene, etc.); , divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.); polycondensates of phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, diphenyl ketone, etc.); polycondensates of phenols and aromatic dimethanols (benzenedimethanol, α,α,α',α'-benzenedimethanol, biphenyl dimethanol, α,α,α',α'-biphenyl dimethanol, etc.); polycondensates of phenols and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethyl biphenyl, etc.); polycondensates of bisphenols and various aldehydes; and modified products thereof, but not limited to these. These may be used alone or in combination of two or more.
[0132] Furthermore, phenol aralkyl resins obtained by condensing phenols with the above-mentioned dihalogenated methyl aralkyl derivatives or aralkyl alcohol derivatives are particularly preferred as the phenol resin because of their low hygroscopicity, flame retardancy, and excellent dielectric properties.
[0133] Furthermore, when the phenol resin has an allyl group or a methallyl group, the reactivity with maleimide groups is better than that with hydroxyl groups, so the curing speed is faster, and the number of crosslinking points increases, so the strength and heat resistance are improved, which is preferred.
[0134] Furthermore, an allyl ether formed by allylation of the hydroxyl groups of the phenol resin and a methallylation of the methallylation of the phenol resin may be blended. Since the hydroxyl groups are etherified, the water absorption property is reduced.
[0135] The curable resin composition of the present embodiment may further contain a compound having an acid anhydride group.
[0136] As the compound having an acid anhydride group that can be blended, any one known in the prior art can be used. Specific examples of the compound having an acid anhydride group include 1,2,3,4-butanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, pyromellitic acid dianhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, and 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride.
[0137] The compound having an acid anhydride group can be used alone or in combination of two or more. The acid anhydride group reacts with an amine to form an amic acid, which, when further heated at 200°C to 300°C, undergoes a dehydration reaction to form an imide structure, thereby becoming a material with extremely excellent heat resistance.
[0138] The curable resin composition of the present embodiment may be mixed with a catalyst (curing accelerator) for curing as needed. Examples thereof include imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, and 1-cyanoethyl-2-ethyl-4-methylimidazole; amines such as triethylamine, triethylenediamine, 2-(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)undec-7-ene, tris(dimethylaminomethyl)phenol, and benzyldimethylamine; and triphenylphosphine, tributylphosphine. , trioctylphosphine and other phosphines; organic metal salts such as tin octanoate, zinc octanoate, dibutyltin dimaleate, zinc naphthenate, cobalt naphthenate, tin oleate, etc.; metal chlorides such as zinc chloride, aluminum chloride, tin chloride, etc.; organic peroxides such as di-tert-butyl peroxide and diisopropylphenyl peroxide; azo compounds such as azobisisobutyronitrile and azobisdimethylvaleronitrile; inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, etc.; Lewis acids such as boron trifluoride; salts such as sodium carbonate and lithium chloride, etc. In this embodiment, it is particularly preferred to blend the above-mentioned amines, phosphines, and organic peroxides. The blending amount of the curing catalyst is preferably 10 parts by weight or less, and more preferably 5 parts by weight or less, relative to a total of 100 parts by weight of the curable resin composition.
[0139] In this embodiment, in particular, in terms of dielectric properties, it is preferred to blend a hardenable polymer such as polybutadiene and its modified products, styrene butadiene copolymer, and further preferably blend a substituted or unsubstituted polyphenylene ether, polystyrene, or fluororesin, and it is particularly preferred to blend a molecule having a 1,2-vinyl group, an acryloyl group, a methacryloyl group, an allyl group, a methallyl group, vinylbenzene, indene, or the like as a functional group. In terms of dielectric properties, film properties, etc., it is particularly preferred to blend a styrene butadiene copolymer having a 1,2-vinyl group, or a combination thereof with a polyphenylene ether having an acryloyl group or a methacryloyl group.
[0140] Furthermore, the curable resin composition of the present embodiment may be blended with known additives as needed. Specific examples of usable additives include: epoxy resin curing agents, modified acrylonitrile copolymers, polyethylene, polyimide, maleimide compounds, maleimide resins, cyanate compounds, cyanate resins, silicone gels, silicone oils, and inorganic fillers such as silica, alumina, calcium carbonate, quartz powder, aluminum powder, graphite, talc, clay, iron oxide, titanium oxide, aluminum nitride, asbestos, mica, and glass powder, surface treatment agents for fillers such as silane coupling agents, mold release agents, and colorants such as carbon black, phthalocyanine blue, and phthalocyanine green. The amount of the additives blended is preferably 1000 parts by weight or less, and more preferably 700 parts by weight or less, relative to 100 parts by weight of the curable resin composition.
[0141] The preparation method of the hardenable resin composition of the present embodiment is not particularly limited, and the components may be simply mixed uniformly, or the components may be prepolymerized. For example, the maleimide resin and the cyanate compound are heated in the presence or absence of a catalyst, in the presence or absence of a solvent, thereby prepolymerizing. Similarly, the maleimide resin of the present embodiment may be added, and epoxy resin, amine compound, maleimide-based compound, cyanate compound, phenol resin, acid anhydride compound, and other additives may be added as needed to perform prepolymerization. With regard to the mixing or prepolymerization of the components, for example, an extruder, a kneader, a roller, etc. may be used in the absence of a solvent, and a reaction kettle with a stirring device may be used in the presence of a solvent.
[0142] By heating and melting the curable resin composition of the present embodiment to reduce viscosity, and impregnating it with reinforcing fibers such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, and alumina fiber, a prepreg can be obtained. In addition, by impregnating the above-mentioned varnish with the fiber as described above and heating and drying, a prepreg can also be obtained. As the fiber used, especially in high-frequency applications, it is preferred to use glass fibers that use not only E glass, but also low-dielectric glass such as NE glass, quartz glass, etc. The blending amount of the fiber material is preferably 10% to 70% by volume relative to the total amount of resin 100% by volume, and is particularly preferably 20% to 65% by volume. In addition, it can also be combined with fillers, etc. for processing. In this case, the total amount of fiber and filler is preferably 80% by volume or less relative to the total amount of resin 100% by volume. If it exceeds 80% by volume, not only the sheet becomes brittle, but also cannot show fluidity during subsequent hardening, making it difficult to process as a substrate.
[0143] The above-mentioned prepreg is cut into the desired shape, and after being laminated with copper foil or the like as needed, pressure is applied to the laminate by a press molding method, an autoclave molding method, a sheet winding molding method, or the like, and the curable resin composition is heated and cured at the same time, thereby obtaining a laminated board (printed wiring board) for electrical and electronic use, or a carbon fiber reinforced material.
[0144] [Example]
[0145] The present invention is specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples. In addition, "parts" and "%" herein represent "parts by weight" and "% by weight", respectively. The softening point and melt viscosity are measured by the following method.
[0146] Softening point: Measured by a method in accordance with JIS K-7234.
[0147] Acid value: Measured by a method in accordance with JIS K-0070:1992.
[0148] GPC (Gel Permeation Chromatography) Analysis
[0149] GPC: DGU-20A3R, LC-20AD, SIL-20AHT, RID-20A, SPD-20A, CTO-20A, CBM-20A (all manufactured by Shimadzu Corporation)
[0150] Column: Shodex KF-603, KF-602×2, KF-601×2
[0151] Linking eluent: tetrahydrofuran
[0152] Flow rate: 0.5ml / min
[0153] Column temperature: 40℃
[0154] Detection: RI (differential refractive index detector).
[0155] Maleimide equivalent
[0156] Calculated by area % of GPC.
[0157] HPLC (High Performance Liquid Chromatography) Analysis
[0158] Infusion Unit LC-20AD manufactured by Shimadzu Corporation
[0159] Photodiode array detector SPD-M20A manufactured by Shimadzu Corporation
[0160] Column oven CTO-20A manufactured by Shimadzu Corporation
[0161] Column: Intersil ODS-2.5μm, 4.6×250mm, 40℃
[0162] Mobile phase A: acetonitrile (AN)
[0163] Mobile phase B: Water (W)
[0164] Time program:
[0165] 0-28min.AN / W=30% / 70%→100% / 0%
[0166] 28-40min.AN / W=100% / 0%
[0167] Flow rate: 1.0mL / min
[0168] Detection: UV 200-274nm, PDA
[0169] Measurement wavelength: 225nm.
[0170] [Synthesis example 1]
[0171] 373 parts of aniline, 150 parts of toluene, 194 parts of meta-di(α-hydroxyisopropyl)benzene, and 75 parts of activated clay (E manufactured by Japan Activated Clay) were added to a flask equipped with a thermometer, a cooling tube, a Dean-Stark azeotropic distillation separator, and a stirrer, and water and toluene were distilled off. At the same time, the temperature in the system was raised to 170°C over 6 hours, and the reaction was carried out at this temperature for 20 hours. Thereafter, the mixture was cooled to room temperature, 600 parts of toluene were added, and the activated clay was removed by filtration. Subsequently, the excess aniline and toluene were distilled off from the oil layer by a rotary evaporator under heating and reduced pressure, thereby obtaining 320 parts of the aromatic amine resin (SA-1) represented by the above formula (5). The amine equivalent of the aromatic amine resin (SA-1) was 180.5 g / eq, and the softening point was 45°C. According to GPC analysis (RI), the n=1 body was 78.8 area %, and the average n was 1.22. The ratio of isomers in the n=1 form obtained by HPLC analysis is shown in Table 1. The area ratio (o / p) of the ortho position to the para position was 28%.
[0172] The area ratio of the ortho position to the para position obtained by HPLC analysis (O / P) = (area % of the aromatic amine compound represented by the above formula (7)) × 2 + (area % of the aromatic amine compound represented by the above formula (6)) / (area % of the aromatic amine compound represented by the above formula (8)) × 2 + (area % of the aromatic amine compound represented by the above formula (6)).
[0173] [Synthesis example 2]
[0174] 804 parts of aniline, 432 parts of toluene, and 450 parts of 35% hydrochloric acid were added to a flask equipped with a thermometer, a cooling tube, a Dean-Stark azeotropic distillation separator, and a stirrer. The temperature was raised while distilling off water and toluene to make the system 170°C. 158 parts of 1,3-diisopropenylbenzene was added dropwise over 1.5 hours at this temperature, and the reaction was carried out at this temperature for 30 hours. Thereafter, 87 parts of a 30% aqueous sodium hydroxide solution was slowly added dropwise while cooling so that the system would not reflux violently. 432 parts of toluene was added at a temperature below 80°C, and the reaction mixture was allowed to stand at 70°C to 80°C. The separated lower water layer was removed, and the reaction solution was repeatedly washed with water until the washing liquid became neutral. Next, excess aniline and toluene were distilled off from the oil layer by a rotary evaporator under heating and reduced pressure, and then 864 parts of toluene were added to heat and dissolve. Thereafter, 864 parts of cyclohexane were added, crystallized, filtered, and dried to obtain 303 parts of the aromatic amine resin (SA-2) represented by the above formula (5). According to GPC analysis (RI), the n=1 isomer was more than 98%, and the average n was 1. The ratio of isomers in the n=1 isomer obtained by HPLC analysis is shown in Table 1. In addition, the area ratio (o / p) of the ortho position to the para position was 0%.
[0175] [Synthesis example 3]
[0176] 373 parts of aniline, 250 parts of toluene, and 10 parts of 35% hydrochloric acid were added to a flask equipped with a thermometer, a cooling tube, a Dean-Stark azeotropic distillation separator, and a stirrer. The temperature was raised while distilling off water and toluene to make the system 170°C. At this temperature, 194 parts of 1,3-diisopropenylbenzene were added dropwise over 1.5 hours, and the reaction was carried out at this temperature for 45 hours. Thereafter, 17.4 parts of a 30% aqueous sodium hydroxide solution were slowly added dropwise while cooling so that the system would not reflux violently. 300 parts of toluene were added at 80°C or less, and the mixture was allowed to stand at 70°C to 80°C. The separated lower water layer was removed, and the reaction liquid was repeatedly washed with water until the washing liquid became neutral. Subsequently, the excess aniline and toluene were distilled off from the oil layer using a rotary evaporator under heating and reduced pressure, thereby obtaining 306 parts of the aromatic amine resin (A-1) represented by the above formula (5). The amine equivalent of the aromatic amine resin (A-1) was 187.9 g / eq and the softening point was 59°C. According to GPC analysis (RI), the n=1 isomer was 62.5 area % and the average n was 1.45. The ratio of isomers in the n=1 isomer obtained by HPLC analysis is shown in Table 1. In addition, the area ratio of the ortho position to the para position (o / p) was 176%.
[0177] [Synthesis Examples 4 to 12]
[0178] Amine resins A-2 to A-10 were synthesized by changing the catalyst, catalyst amount, aniline amount, reaction temperature and reaction time in Synthesis Example 3. The results are shown in Table 1.
[0179] [Synthesis Example 13]
[0180] 192 parts of aniline, 123 parts of toluene, and 194 parts of 1,3-diisopropenylbenzene were added to a flask equipped with a thermometer, a cooling tube, a Dean-Stark azeotropic distillation separator, and a stirrer, and 21 parts of 35% hydrochloric acid were added while stirring. Thereafter, the temperature was raised and water and toluene were distilled off at 160°C in the system, and the reaction was carried out for 24 hours. Thereafter, 30 parts of a 30% aqueous sodium hydroxide solution were slowly added dropwise in a manner that would not cause violent reflux in the system, 20 parts of toluene were added at a temperature below 80°C, and the mixture was allowed to stand at 70°C to 80°C. The separated lower water layer was removed, and the reaction liquid was repeatedly washed with water until the washing liquid became neutral. Subsequently, the excess aniline and toluene were distilled off from the oil layer using a rotary evaporator under heating and reduced pressure, thereby obtaining 158 parts of the aromatic amine resin (A-11) represented by the above formula (5). The amine equivalent of the aromatic amine resin (A-13) was 186 g / eq and the softening point was 58.8° C. The n=1 isomer was 64.9 area % by GPC analysis (RI). The isomer ratios in the n=1 isomer determined by HPLC analysis are shown in Table 1.
[0181] [Table 1]
[0182]
[0183] HCl: 35% hydrochloric acid aqueous solution (manufactured by Junsei Chemical).
[0184] [Comparative Example 1]
[0185] 147 parts of maleic anhydride, 300 parts of toluene, and 4 parts of methanesulfonic acid were added to a flask equipped with a thermometer, a cooling tube, a Dean Stark azeotropic distillation separator, and a stirrer, and the mixture was heated to reflux. Then, the reflux state was maintained, and the following resin solution was dripped over 3 hours, i.e., 197 parts of aromatic amine resin (SA-1) were dissolved in 95 parts of N-methyl-2-pyrrolidone and 100 parts of toluene to make the resin solution. During this period, the condensed water and toluene that were azeotropically distilled under reflux conditions were cooled and separated in the Dean Stark azeotropic distillation separator, and the toluene as the organic layer was returned to the system, and the water was discharged outside the system. After the resin solution was added, the reflux state was maintained, the dehydration operation was performed, and the reaction was performed for 6 hours at the same time. After the reaction, the mixture was washed with water four times to remove methanesulfonic acid and excess maleic anhydride, and water was removed from the system by azeotroping toluene and water under reduced pressure at a temperature below 70°C. Subsequently, 2 parts of methanesulfonic acid were added and the mixture was reacted under heating reflux for 2 hours. After the reaction, the mixture was washed with water four times until the washing water became neutral, and then water was removed from the system by azeotroping toluene and water under reduced pressure at a temperature below 70°C. Toluene was completely distilled off under reduced pressure to obtain maleimide resin (SM-1) represented by the above formula (1). The softening point of the obtained maleimide resin (SM-1) was 100°C and the acid value was 9 mg KOH / g. According to GPC analysis (RI), the n=1 isomer was 73% and the average n was 1.37. The ratio of isomers in the n=1 isomer obtained by HPLC analysis is shown in Table 2. In addition, the area ratio (o / p) of the ortho-direction to the para-direction was 30%.
[0186] [Comparative Example 2]
[0187] 147 parts of maleic anhydride, 300 parts of toluene, and 3.3 parts of methanesulfonic acid were added to a flask equipped with a thermometer, a cooling tube, a Dean-Stark azeotropic distillation separator, and a stirrer, and heated to reflux. Then, the reflux state was maintained, and the following resin solution was added dropwise over 3 hours, i.e., a resin solution prepared by dissolving 172 parts of 1,3-bis(p-aminoisopropylphenyl)benzene (SA-2) in 66 parts of N-methyl-2-pyrrolidone and 100 parts of toluene. During this period, the condensed water and toluene that were azeotropically distilled under reflux conditions were cooled and separated in the Dean-Stark azeotropic distillation separator, and the toluene as the organic layer was returned to the system, and the water was discharged to the outside of the system. After the addition of the resin solution was completed, the reflux state was maintained, the dehydration operation was performed, and the reaction was performed for 2 hours. After the reaction, the mixture was washed with water four times to remove methanesulfonic acid and excess maleic anhydride, and water was removed from the system by azeotroping toluene and water under reduced pressure at a temperature below 70°C. Subsequently, 1.7 parts of methanesulfonic acid were added and the mixture was reacted under heating reflux for 2 hours. After the reaction, the mixture was washed with water three times until the washing water became neutral, and then water was removed from the system by azeotroping toluene and water under reduced pressure at a temperature below 70°C. Subsequently, toluene was completely distilled off under reduced pressure to obtain 237 parts of maleimide resin (SM-2). The softening point of the obtained maleimide resin (SM-2) was 91°C and the acid value was 3 mg KOH / g. According to GPC analysis (R1), the n=1 isomer was 95% and the average n was 1.02. The ratio of isomers in the n=1 isomer is shown in Table 2. In addition, the area ratio (o / p) of the ortho position to the para position was 0%.
[0188] [Example 1]
[0189] 147 parts of maleic anhydride, 300 parts of toluene, and 4 parts of methanesulfonic acid were added to a flask equipped with a thermometer, a cooling tube, a Dean Stark azeotropic distillation separator, and a stirrer, and the mixture was heated to reflux. Then, the reflux state was maintained, and the following resin solution was added dropwise for 3 hours, i.e., 197 parts of aromatic amine resin (A-1) was dissolved in 95 parts of N-methyl-2-pyrrolidone and 100 parts of toluene to form a resin solution. During this period, the condensed water and toluene that were azeotropically distilled under reflux conditions were cooled and separated in the Dean Stark azeotropic distillation separator, and the toluene as the organic layer was returned to the system, and the water was discharged outside the system. After the resin solution was added dropwise, the reflux state was maintained, the dehydration operation was performed, and the reaction was performed for 6 hours at the same time. After the reaction is completed, the mixture is washed with water four times repeatedly to remove methanesulfonic acid and excess maleic anhydride, and water is removed from the system by azeotroping toluene and water under heating and reduced pressure below 70°C. Subsequently, 2 parts of methanesulfonic acid are added and the mixture is reacted under heating and reflux for 2 hours. After the reaction is completed, the mixture is washed with water four times repeatedly until the washing water becomes neutral, and then water is removed from the system by azeotroping toluene and water under heating and reduced pressure below 70°C. Subsequently, as for toluene, the solvent is distilled off under heating and reduced pressure until the resin concentration reaches about 70-80%, and then toluene is added to adjust the resin concentration to 60%. Thus, a maleic imide solution (V1) containing maleic imide resin (M-1) is obtained. According to GPC analysis (RI), the n=1 isomer is 57%, and the average n is 1.80. The ratio of isomers in the n=1 isomer obtained by HPLC analysis is shown in Table 2. 50 parts of the obtained resin solution were taken and the solvent was completely distilled off under heating and reduced pressure to obtain the maleimide resin (M-1) represented by the above formula (1). The obtained maleimide resin (M-1) had a softening point of 115°C and an acid value of 7.5 mg KOH / g. In addition, the area ratio of the ortho position to the para position (o / p) was 163%.
[0190] [Example 2]
[0191] To a flask equipped with a thermometer, a cooling tube, a Dean Stark azeotropic distillation separator, and a stirrer, 147 parts of maleic anhydride, 300 parts of toluene, and 4 parts of methanesulfonic acid were added, and the mixture was heated to reflux. Then, the reflux state was maintained, and the following resin solution was dripped over 3 hours, i.e., 197 parts of aromatic amine resin (A-2) were dissolved in 95 parts of N-methyl-2-pyrrolidone and 100 parts of toluene to make the resin solution. During this period, the condensed water and toluene that were azeotropically obtained under reflux conditions were cooled and separated in the Dean Stark azeotropic distillation separator, and the toluene as the organic layer was returned to the system, and the water was discharged outside the system. After the resin solution was added, the reflux state was maintained, the dehydration operation was performed, and the reaction was performed for 6 hours at the same time. After the reaction, the mixture was washed with water four times to remove methanesulfonic acid and excess maleic anhydride, and water was removed from the system by azeotroping toluene and water under reduced pressure at a temperature below 70°C. Subsequently, 2 parts of methanesulfonic acid were added and the mixture was reacted under heating reflux for 2 hours. After the reaction, the mixture was washed with water four times until the washing water became neutral, and then water was removed from the system by azeotroping toluene and water under reduced pressure at a temperature below 70°C. Subsequently, toluene was completely distilled off under reduced pressure at a temperature below 70°C, thereby obtaining the maleic imide resin (M-2) represented by the above formula (1). The softening point of the obtained maleic imide resin (M-2) was 111°C, and the acid value was 8 mg KOH / g. According to GPC analysis (RI), the n=1 isomer was 56%, and the average n was 1.78. The ratio of isomers in the n=1 isomer obtained by HPLC analysis is shown in Table 2. In addition, the area ratio of the ortho position to the para position (o / p) was 120%.
[0192] [Examples 3 to 5]
[0193] The amine resins obtained in Synthesis Examples 6, 8, and 9 were synthesized in the same manner as in Example 1. Table 2 shows the results.
[0194] [Example 14]
[0195] To a flask equipped with a thermometer, a cooling tube, a Dean Stark azeotropic distillation separator, and a stirrer, 147 parts of maleic anhydride, 300 parts of toluene, and 8 parts of methanesulfonic acid were added, and the mixture was heated to reflux. Then, the reflux state was maintained, and the following resin solution was dripped over 3 hours, i.e., 190 parts of aromatic amine resin (A-11) were dissolved in 95 parts of N-methyl-2-pyrrolidone and 100 parts of toluene to make the resin solution. During this period, the condensed water and toluene that were azeotropically distilled under reflux conditions were cooled and separated in the Dean Stark azeotropic distillation separator, and the toluene as the organic layer was returned to the system, and the water was discharged outside the system. After the resin solution was added, the reflux state was maintained, the dehydration operation was performed, and the reaction was performed for 6 hours at the same time.
[0196] After the reaction, the mixture was washed with water four times to remove methanesulfonic acid and excess maleic anhydride, and water was removed from the system by azeotroping toluene and water under heating and reduced pressure below 70°C. Subsequently, 2 parts of methanesulfonic acid were added and the mixture was reacted under heating and reflux for 2 hours. After the reaction, the mixture was washed with water four times until the washing water became neutral, and then water was removed from the system by azeotroping toluene and water under heating and reduced pressure below 70°C. Subsequently, as for toluene, the solvent was distilled off under heating and reduced pressure until the resin concentration reached about 70-80%, and then toluene was added to prepare the resin concentration to 60%. Thus, a maleic imide solution (V-11) containing maleic imide resin (M-11) was obtained. According to GPC analysis (RI), the n=1 isomer was 48.1%, and the average n was 1.85. The ratio of isomers in the n=1 isomer obtained by HPLC analysis is shown in Table 2. In addition, the area ratio of the ortho position to the para position (o / p) was 127%.
[0197] 50 portions of the obtained resin solution were taken and the solvent was completely distilled off under heating and reduced pressure, thereby obtaining the maleimide resin (M-11) represented by the above formula (1). The obtained maleimide resin (M-11) had a softening point of 126°C and an acid value of 9.5 mg KOH / g.
[0198] [Table 2]
[0199]
[0200]
[0201] [Comparative Examples 3, 4 and Examples 6 to 10]
[0202] The maleimide resins obtained in Comparative Examples 1 and 2 and Examples 1 to 5 were dissolved in toluene so that the resin portion was 60%, and maleimide resin solutions VSM-1, 2, and VM-1 to 5 were obtained. The obtained maleimide resin solutions were stored at -10°C for three months, and the presence or absence of crystal precipitation was observed. The case where crystal precipitation was observed was marked as ×, and the case where crystal precipitation was not observed was marked as ○, and the results are shown in Table 3.
[0203] [Table 3]
[0204]
[0205] From Table 3, it was confirmed that the maleimide resin of the present embodiment was excellent in solution stability.
[0206] [Examples 11, 12, Comparative Examples 5, 6]
[0207] 0.75 parts by weight of a catalyst (DCP, diisopropylphenyl peroxide, manufactured by Nouryon Chemicals) was added to 50 parts by weight of each of the maleimide resins M-1 and M-3 obtained in Examples 1 and 3, and SM-1 and SM-2 obtained in Comparative Examples 1 and 2, and cured at 250°C for 2 hours. A plate of 2.5 mm × 50 mm × 0.25 mm was cut out from the obtained cured product, and the dielectric constant and dielectric loss tangent were measured at frequencies of 1 GHz and 10 GHz using a cavity resonator (ADMS01OC1 manufactured by AET). The results of the measurements are shown in Table 4.
[0208] [Table 4]
[0209] Comparative Example 5 Comparative Example 6 Embodiment 11 Example 12 Maleimide SM-1 SM-2 M-1 M-3 Dielectric constant (1GHz) 2.71 2.72 2.69 - Dielectric loss tangent (1GHz) 0.0017 0.002 0.0016 - Dielectric constant (10GHz) 2.66 2.68 2.62 2.59 Dielectric loss tangent (10GHz) 0.0019 0.0026 0.0016 0.0016
[0210] ※“-” in the table means not measured.
[0211] According to Table 4, it was confirmed that the maleimide resin of the present embodiment had excellent dielectric properties not only at 1 GHz but also at 10 GHz.
[0212] [Example 13, Comparative Example 7]
[0213] 1.5 parts by weight of a catalyst (2E4MZ: 2-ethyl-4-methylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.)) was added to 50 parts by weight of each of the maleimide resin M-4 obtained in Example 4 and the SM-1 obtained in Comparative Example 1, and the mixture was cured at 250°C for 2 hours. A plate of 50 mm×50 mm×0.25 mm was cut out from the obtained cured product, and the dielectric loss tangent at each frequency of 25°C and 150°C was measured using a balanced circular plate resonator method (resonator: a balanced circular plate resonator manufactured by FATEC was used). The results of the measurement are shown in Table 5.
[0214] [Table 5]
[0215]
[0216] From Table 5, it was confirmed that the maleimide resin of the present embodiment has excellent dielectric properties even in the high frequency region. In addition, it was confirmed that the maleimide resin of the present embodiment has small differences due to temperature and has high environmental resistance.
[0217] [Example 15, Comparative Examples 8 and 9]
[0218] Using the maleimide resin (M-11) obtained from Example 14, the maleimide resin (SM-1) obtained from Comparative Example 1, and the maleimide resin (SM-2) obtained from Comparative Example 2, various epoxy resins, hardeners, and hardening accelerators were blended in the proportions (parts by weight) described in Table 6, kneaded and flattened by a mixing roll, and then a resin molded body was prepared by transfer molding, and hardened at 200°C for 2 hours. The physical properties of the hardened products thus obtained were measured for the following items, and the measured results are shown in Table 6. In addition, for each hardened product, the change in elastic modulus due to temperature was measured by a dynamic viscoelasticity device (DMA). The results are shown in Figure 1 .
[0219] TMA Tg: glass transition temperature measured by a thermomechanical characterization device.
[0220] DMA elastic modulus: measured by a dynamic viscoelasticity tester (DMA).
[0221] Td5 (5% thermal weight loss temperature): The thermal decomposition temperature of the powder obtained by pulverizing the hardened material is measured by TG-DTA using a sample that passes through a 100-mesh sieve and does not pass through a 200-mesh sieve. This is the temperature at which the weight is reduced by 5% with a sample size of 10 mg, a heating rate of 10°C / min, and an air volume of 200 ml / hr.
[0222] ·Flexural modulus: measured in accordance with JIS K-6911.
[0223] Dielectric constant and dielectric loss tangent: measured at room temperature using a cavity resonator (manufactured by AET).
[0224] [Table 6]
[0225]
[0226] E1: NC-3000-L (manufactured by Nippon Kayaku, epoxy equivalent is 271g / eq)
[0227] P1: Kayado GPH-65 (manufactured by Nippon Kayaku, hydroxyl equivalent 200g / eq)
[0228] C1:2E4MZ: 2-ethyl-4-methylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0229] According to the results of Table 6, it is confirmed that the cured product of Example 15 has a high elastic modulus in the range from room temperature to low temperature, which contributes to the rigidity of the substrate, and also maintains a high elastic modulus in the temperature range during reflow soldering. In addition, since it can be confirmed that the heat resistance (Tg) is also high, and the stability when hot (thermal decomposition resistance Td5) is also excellent, it can be said that the weather resistance generated by heat is excellent. Furthermore, in terms of dielectric properties, it is confirmed that the influence of dielectric property degradation caused by the addition of epoxy resin can be suppressed, and both the dielectric constant and the dielectric loss tangent are excellent.
[0230] [Example 16, Comparative Example 10]
[0231] 0.75 parts by weight of a catalyst (DCP, diisopropylphenyl peroxide, manufactured by Nouryon Chemicals) was added to 50 parts by weight of each of the maleimide resin (M-11) obtained in Example 14 and the maleimide resin (SM-1) obtained in Comparative Example 1, and transfer molding was performed at 175°C, followed by curing at 250°C for 2 hours. A 2.5 mm × 50 mm × 0.25 mm plate was cut out from the obtained cured product, dried and immersed in water at room temperature for 24 hours, and then the dielectric constant and dielectric loss tangent were measured at a frequency of 10 GHz using a cavity resonator (manufactured by AET). The results of the measurement are shown in Table 7.
[0232] [Table 7]
[0233]
[0234] From the results of Table 7, it was confirmed that the cured product of Example 16 had less decrease in dielectric properties after the water absorption test and low hygroscopicity, and therefore had excellent weather resistance.
[0235] This application is based on Japanese Patent Application No. 2020-41840 filed on March 11, 2020, the contents of which are incorporated herein by reference.
Claims
1. A maleimide resin represented by the following formula (1), and In the maleimide resin, the content of N,N'-(phenylenebis(2,2-propylene)diphenylene)bismaleimide is 98% by area or less in terms of GPC area percentage, In the N,N'-(phenylenebis(2,2-propylene)diphenylene)bismaleimide, the content of the maleimide compound represented by the following formula (2) is 30 area % or more and less than 60 area % in terms of HPLC area percentage. In the N,N'-(phenylenebis(2,2-propylene)diphenylene)bismaleimide, the area ratio O / P of the ortho position to the para position obtained by HPLC area percentage is 100% or more and less than 200%, In the N,N'-(phenylenebis(2,2-propylene)diphenylene)bismaleimide, the content of the maleimide compound represented by the following formula (3) is less than 50% by area percentage in terms of HPLC area percentage. In formula (1), n is the number of repetitions, and its average value is 1<n<5.
2. A maleimide solution comprising the maleimide resin according to claim 1 and an organic solvent, wherein the organic solvent is selected from at least one of ketones, hydrocarbons, and esters.
3. A curable resin composition comprising the maleimide resin according to claim 1 or the maleimide solution according to claim 2, and further comprising a curing accelerator.
4. A cured product obtained by curing the maleimide resin according to claim 1 or the curable resin composition according to claim 3.
5. A method for producing the maleimide resin according to claim 1, comprising: A step of adding 1 to 12 wt % of a protonic acid relative to the total amount of aniline to aniline and diisopropylbenzene or di(α-hydroxyisopropyl)benzene, and reacting at 140 to 190° C. to obtain an aromatic amine resin; and The aromatic amine resin is subjected to a step of maleimidizing.
Citation Information
Patent Citations
JP1979030440B2
Preparation of polymaleimide compound
JP1991100016A
JP1992075222B2
Method for producing bismaleimide compounds
JP1994037465B2
New cyanate ester compound, flame-retardant resin composition and cured product thereof
JP2005264154A