Quantum dot thin films and their preparation methods and quantum dot light-emitting diodes and their preparation methods

By treating quantum dot films with proton reagents to passivate surface defect states, the problems of low luminous efficiency and short lifetime in quantum dot light-emitting diodes have been solved, enabling efficient commercial applications.

CN115249774BActive Publication Date: 2026-11-17TCL TECHNOLOGY GROUP CORPORATION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110447958.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-25
Publication Date
2026-11-17
Estimated Expiration
2041-04-25

AI Technical Summary

Technical Problem

In existing quantum dot light-emitting diode devices, surface defect states of quantum dots cause exciton quenching, resulting in low luminous efficiency and short lifetime, which cannot meet the needs of commercial applications.

Method used

Quantum dot films are treated with proton reagents to passivate dangling bonds on the quantum dot surface, reduce defect states, and improve luminescence efficiency and lifespan.

Benefits of technology

By passivating the surface defect states of quantum dots, the luminous efficiency and lifespan of quantum dot light-emitting diodes are significantly improved, meeting the needs of commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115249774B_ABST
    Figure CN115249774B_ABST
Patent Text Reader

Abstract

This application relates to the field of quantum dot film deposition technology, and more particularly to a quantum dot thin film and its preparation method, and a quantum dot light-emitting diode and its preparation method. The preparation method of the quantum dot thin film includes the following steps: providing an initial quantum dot thin film; treating the initial quantum dot thin film with a proton reagent to obtain the quantum dot thin film. This preparation method can passivate surface defects of the quantum dots, reduce the quenching of excitons by defect states, and ultimately improve the luminous efficiency and lifespan of the quantum dot thin film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of quantum dot film formation technology, and particularly relates to a quantum dot thin film and its preparation method and a quantum dot light-emitting diode and its preparation method. Background Technology

[0002] Quantum dots (QDs), as nanomaterials with unique luminescent properties, exhibit tunable emission wavelengths with varying quantum dot size. They also possess advantages such as wide color gamut, high luminous efficiency, high optical and thermal stability, and solution-processability, leading to their widespread application in light-emitting diode (LED) device research in recent years. Significant improvements have been made in the photoelectric performance of quantum dot light-emitting diode (QLED) devices in recent years, with device structures shifting towards organic-inorganic hybrid structures. During QLED device structure optimization, brightness and lifetime have been greatly improved. Simultaneously, to meet the demands of commercial applications, research into device stability has received increasing attention.

[0003] Quantum dot materials obtained by conventional synthesis methods are generally linked to surface ligands via coordination bonds. These ligands ensure stable dispersion of quantum dots in solvents, preventing aggregation and sedimentation, and effectively passivate vacancies and dangling bonds on the quantum dot surface. However, when quantum dots are used as the emitting layer in quantum dot light-emitting diode (LED) devices, the surface ligands, acting as insulating organic materials, increase the interfacial barrier between the emitting layer and adjacent functional layers, hindering carrier injection and leading to increased operating voltage and lower photoelectric conversion efficiency. Therefore, controlling the content of surface ligands is crucial for ensuring the performance of quantum dot LED devices while maintaining good dispersion in solvents. However, with reduced surface ligands, due to their high specific surface area, unprotected atoms on the quantum dot surface exist in defect states. These defect states trap electrons and holes in delocalized states, causing exciton quenching and rapid performance degradation.

[0004] Whether in the formulation of inks for the quantum dot emitting layer or the fabrication of quantum dot light-emitting diode (LED) devices, the external environment is a key factor affecting the efficiency and stability of electroluminescent devices. During the synthesis, purification, ink formulation, and solution processing of quantum dot materials into the emitting layer of quantum dot LEDs, a certain number of defects inevitably arise on the quantum dot surface. Simultaneously, the high specific surface area of ​​quantum dots means that unprotected atoms exist in defect states. These defects have the ability to trap electrons and holes in the delocalized state of the quantum dot, introducing rapid non-radiative recombination channels for exciton recombination. Moreover, the recombination rate of these non-radiative channels caused by defects is much higher than that of radiative channels, resulting in a sharp decrease in the luminescence efficiency of the quantum dot. That is, when photoelectric conversion is performed through external light or electrical excitation, the presence of defect states quenches excitons and increases non-radiative recombination, reducing fluorescence efficiency and photoelectric performance. The resulting quantum dot LED devices exhibit a significant roll-off effect in brightness and external quantum efficiency, making their photoelectric performance unsuitable for commercial applications. Summary of the Invention

[0005] The purpose of this application is to provide a quantum dot thin film and a method for preparing the same, and a quantum dot light-emitting diode and a method for preparing the same, in order to solve the technical problem of how to reduce surface defects in quantum dot thin films.

[0006] To achieve the above-mentioned objectives, the technical solution adopted in this application is as follows:

[0007] In a first aspect, this application provides a method for preparing quantum dot thin films, comprising the following steps:

[0008] Provide initial quantum dot films;

[0009] The initial quantum dot film was treated with a proton reagent to obtain a quantum dot film.

[0010] The quantum dot film preparation method provided in this application involves treating the initial quantum dot film with a protonating reagent. During this treatment, the protonating reagent makes surface contact with the initial quantum dot film. Specifically, after protonation, the protonating reagent connects with dangling bonds on the quantum dot surface, thereby passivating surface defects of the quantum dot, reducing the quenching of excitons due to defect states, and ultimately improving the luminescence efficiency and lifespan of the quantum dot film.

[0011] Secondly, this application provides a quantum dot thin film, which is prepared by the quantum dot thin film preparation method of this application.

[0012] The quantum dot film provided in this application is prepared by a method unique to this application. Because this method treats the initial quantum dot film with a proton reagent, the quantum dot film can reduce the surface defect states of the quantum dots and has excellent luminescence efficiency and lifespan.

[0013] Thirdly, this application provides a quantum dot light-emitting diode, including an anode, a cathode, and a quantum dot light-emitting layer located between the anode and the cathode, wherein the quantum dot light-emitting layer is a quantum dot thin film prepared by the preparation method of this application.

[0014] The quantum dot light-emitting layer in the quantum dot light-emitting diode provided in this application is a quantum dot thin film obtained by a unique preparation method of this application. Because this quantum dot thin film can reduce the surface defect states of quantum dots and reduce the quenching of excitons, the device has excellent luminous efficiency and lifespan.

[0015] Fourthly, this application provides a method for fabricating a quantum dot light-emitting diode, comprising the following steps:

[0016] Provide substrate;

[0017] An initial quantum dot film is prepared on the substrate, and then the initial quantum dot film is treated with a proton reagent to obtain a quantum dot light-emitting layer.

[0018] The quantum dot thin film preparation method provided in this application involves treating an initial quantum dot thin film on a substrate with a protonating reagent to obtain the quantum dot light-emitting layer. During this treatment, the protonating reagent makes surface contact with the initial quantum dot thin film, causing the protonating reagent to be protonated and connected to dangling bonds on the quantum dot surface. This passivates surface defects of the quantum dot and reduces the quenching of excitons due to defect states. Therefore, this quantum dot light-emitting diode preparation method can ultimately improve the luminous efficiency and lifespan of the device. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 This is a schematic diagram of the process for preparing quantum dot thin films provided by the present invention;

[0021] Figure 2 This is a schematic diagram of the quantum dot light-emitting diode device structure provided by the present invention;

[0022] Figure 3This is a schematic diagram of the process for preparing quantum dot thin films provided by the present invention;

[0023] Figure 4 This is a current efficiency curve of the light-emitting diode device of Embodiment 1 and Comparative Example 1 provided by the present invention;

[0024] Figure 5 These are device lifetime test curves for Embodiment 1 and Comparative Example 1 provided by the present invention. Detailed Implementation

[0025] To make the technical problems, technical solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0026] The first aspect of this application provides a method for preparing quantum dot thin films, such as... Figure 1 As shown, the preparation method includes the following steps:

[0027] S01: Provides the initial quantum dot film;

[0028] S02: The initial quantum dot film is treated with a proton reagent to obtain a quantum dot film.

[0029] The quantum dot film preparation method provided in this application involves treating the initial quantum dot film with a protonating reagent. During this process, the protonating reagent makes surface contact with the initial quantum dot film. Specifically, after protonation, the protonating reagent connects with dangling bonds on the quantum dot surface, thereby passivating surface defects of the quantum dot, reducing the quenching of excitons due to defect states, and ultimately improving the luminescence efficiency and lifespan of the quantum dot film.

[0030] In step 01 of this application, the initial quantum dot film can be either a wet film or a dry film. A wet film can be a moist initial quantum dot film formed by depositing a quantum dot solution onto a substrate; a dry film can be a dry, solid initial quantum dot film formed by depositing a quantum dot solution onto a substrate and then performing a solvent removal process. Because some proton reagents may be antisolvents of the solvent in the quantum dot solution, the treatment of a moist initial quantum dot film with proton reagents may slightly affect the stability of the quantum dots within the initial quantum dot film. Therefore, this application prefers a dry, solid initial quantum dot film, specifically, an initial quantum dot film obtained by depositing a quantum dot solution onto a substrate and then performing a solvent removal process.

[0031] In the quantum dot solution used to prepare the initial quantum dot film, the solvent can be at least one of saturated or unsaturated alkanes or aromatic hydrocarbons, such as one or more of dichloromethane, chloroform, toluene, n-hexane, cyclohexane, n-heptane, n-octane, cycloheptane, and dioxane. Quantum dot materials obtained by conventional synthesis methods are generally linked to surface ligands via coordination bonds. In the initial quantum dot film of this application, the quantum dot surface is also bound to surface ligands, which can be long-chain ligands, such as one or more of oleylamine (OLAM), oleic acid (OA), tri-n-octylphosphine (TOP), tri-n-octylphosphine oxide (TOPO), and tributylphosphine (TBP). In this initial quantum dot film, a certain number of unprotected cation dangling bonds, i.e., defect states on the quantum dot surface, will form on the quantum dot surface. This application involves mixing a protonating reagent with the initial quantum dot film. The protonating reagent protonates and dehydrogenates at defect sites on the quantum dot surface, forming coordinate bonds with cations and passivating dangling bonds. Simultaneously, some in-situ bonded surface ligands are replaced by the protonated reagent. Ultimately, the protonating reagent treatment reduces exciton quenching caused by defect states, thereby improving the luminescence efficiency and lifespan of the quantum dot film.

[0032] It should be noted that if the proton reagent is directly added to the quantum dot solution for mixing and modification before film formation, some of the proton reagent may be antisolvents of the solvent in the quantum dot solution. This would affect the stability of the quantum dots in the solution system, reduce the dispersibility of the quantum dots in the solvent, and even cause them to precipitate from the dispersion solvent. Moreover, the surface tension and viscosity of the solvent after mixing will change. Therefore, the form of proton reagent mixing and modification with the quantum dot solution cannot improve the final quality of the quantum dot film. However, if the quantum dot solution is first formed into an initial quantum dot film, even if it is a wet film containing some solvent, such as when the proton reagent and the solvent are antisolvents, the quantum dot solution has already formed a very thin film layer. In the thin film state, it can passivate the surface defects of the quantum dots and reduce the quenching effect of the defect state on the excitons. However, the effect of the dry solid initial quantum dot film is better. Therefore, this application modifies the initial quantum dot film by treating it with a protonating reagent, allowing the protonating reagent to make surface contact with the initial quantum dot film, rather than by doping the quantum dot solution with the protonating reagent. More preferably, the initial dry solid quantum dot film is treated with a protonating reagent. This quantum dot film preparation method can passivate surface defect state traps in quantum dots, reducing the quenching of excitons by defect states. Quantum dot films prepared using this process, when used as the light-emitting layer in quantum dot light-emitting diodes, can improve the device's luminous performance and lifespan.

[0033] The initial quantum dot thin film provided in this application includes quantum dots comprising at least one single or composite structure quantum dot from groups II-VI, III-V, IV-VI, VI-VI, VIII-VI, I-III-VI, II-IV-VI, and II-IV-V of the periodic table. The composite structure quantum dots include core-shell structure quantum dots, wherein the core constituting the core-shell structure quantum dots comprises at least one of CdSe, CdS, CdTe, CdSeTe, CdZnS, PbSe, ZnTe, CdSeS, PbS, PbTe, HgS, HgSe, HgTe, GaN, GaP, GaAs, InP, InAs, InZnP, InGaP, and InGaN; and the shell constituting the core-shell structure quantum dots comprises at least one of ZnSe, ZnS, and ZnSeS.

[0034] The protonating agent refers to a molecule containing -OH or -NH bonds that can act as hydrogen bond donors; it is also called a protonating solvent. The protonating agent includes at least one of hydroxyl-containing and amino-containing protonating agents. The hydroxyl-containing protonating agent includes at least one of water, methanol, ethanol, propanol (e.g., isopropanol), butanol (e.g., n-butanol), pentanol (e.g., n-pentanol), formic acid, acetic acid, propionic acid, and butyric acid; the amino-containing protonating agent includes at least one of methylamine, ethylamine, and propylamine. When the above protonating agents are mixed with the initial quantum dot film, they can dehydrogenate and protonate at defect sites on the quantum dot surface, then bind to coordinated unsaturated cations on the quantum dot surface. Simultaneously, a small portion of the long-chain ligands on the quantum dot surface are also replaced by the protonated agent.

[0035] In step S02 above, there are two ways to mix the protonating reagent with the initial quantum dot film. One method is to deposit the liquid protonating reagent onto the surface of the initial quantum dot film for proton exchange, covering the initial quantum dot film, and then annealing to obtain the final modified quantum dot film. The other method is to contact the gaseous protonating reagent with the initial quantum dot film for proton exchange, and then annealing to obtain the final modified quantum dot film. The gaseous protonating reagent can be obtained by atomizing the liquid protonating reagent through heating, ultrasound, spraying, or other methods.

[0036] Specifically, in one embodiment, the proton reagent is a liquid proton reagent, and the mixing process includes: depositing the liquid proton reagent onto the surface of the initial quantum dot film, followed by annealing. The step of depositing the liquid proton reagent onto the surface of the initial quantum dot film and then annealing includes: adding the liquid proton reagent at a rate of 3-20 μl / cm³ each time. 2 Spin-coating is performed 2-5 times, i.e., using the initial quantum dot film as a reference, each 1 cm layer is coated. 2Spin-coat 2-20 μl of liquid proton reagent per unit area, repeating 2-5 times.

[0037] Specifically, a spin coater can be used to repeatedly drop liquid proton solvent onto the initial quantum dot film while it is rotating; wherein the rotation speed is 1000-3000 rpm, and the volume of proton solvent added each time is 3-20 μl / cm³. 2 The protonation reaction is carried out in 2-5 drops. Since the protonating reagent is in direct contact with the initial quantum dot film and is prone to evaporation, to avoid differences in contact time between the covered protonating reagent and the initial quantum dot film, a rapid drop-feeding method is used to protonate the quantum dot surface while rotating the spin coater. Because the contact time between the protonating solvent added in one drop and the quantum dot film surface is short when the spin coater is rotating, multiple repeated drops are used to ensure sufficient protonation and more effectively passivate surface defects of the quantum dots. Specifically, the protonating reagent is added at a rate of 3-20 g / cm³ each time. 2 The amount of spin coating is 2-5 times. When this preparation method is used to prepare the quantum dot light-emitting layer in quantum dot light-emitting diodes, the number of drop-coating times is in the range of 2-5 times, and it will not damage the underlying organic hole transport material.

[0038] Furthermore, a liquid proton reagent is deposited on the surface of the initial quantum dot film, and then annealed at a temperature of 60-100°C for 5-20 minutes.

[0039] In another embodiment, the protonating agent is a gaseous protonating agent, and the mixing treatment step includes: placing the initial quantum dot film in the gaseous protonating agent for a settling treatment, followed by annealing. The settling time is 30 s to 5 min; if the settling time is less than 30 s, the protonation reaction at the defects on the quantum dot surface is insufficient, resulting in low defect passivation; if the settling time is greater than 5 min, excessively long protonating agent treatment may generate new defect states, which become new luminescence quenching centers. When this preparation method is used to prepare a quantum dot emitting layer in a quantum dot light-emitting diode, for the structure of a positive device, the above-mentioned settling time range will not affect the underlying organic hole transport material, nor will it cause it to degrade.

[0040] Furthermore, the initial quantum dot film is placed in the gaseous proton reagent for static treatment, and then annealed at a temperature of 60-100℃ for 5-20 minutes.

[0041] A second aspect of this application provides a quantum dot thin film, which is prepared by the quantum dot thin film preparation method described above.

[0042] The quantum dot film provided in this application is prepared by a method unique to this application. Because this method treats the initial quantum dot film with a proton reagent, the quantum dot film can reduce the surface defect states of the quantum dots and has excellent luminescence efficiency and lifespan.

[0043] A third aspect of this application provides a quantum dot light-emitting diode, including an anode, a cathode, and a quantum dot light-emitting layer located between the anode and the cathode, wherein the quantum dot light-emitting layer is a quantum dot thin film prepared by the preparation method of this application.

[0044] The quantum dot light-emitting layer in the quantum dot light-emitting diode provided in this application is a quantum dot thin film obtained by a unique preparation method of this application. Because the quantum dot thin film can passivate the defect states on the quantum dot surface, the number of defect states on the quantum dot surface is significantly reduced after passivation, the ability to capture electrons and holes in the delocalized state is reduced, and the non-radiative recombination channels of exciton quenching are reduced. Therefore, the device has good luminous efficiency and lifespan.

[0045] Specifically, the external quantum efficiency (EQE) of quantum dot light-emitting diode devices is improved by nearly 30%.

[0046] In one embodiment, a hole transport layer may be disposed between the anode and the quantum dot light-emitting layer, and further, a hole injection layer may be disposed between the hole transport layer and the anode; alternatively, an electron transport layer may be disposed between the cathode and the quantum dot light-emitting layer, and further, an electron injection layer may be disposed between the electron transport layer and the cathode. The quantum dot light-emitting diode can be either a forward-facing device or an inverted device.

[0047] Furthermore, such as Figure 2 As shown, the quantum dot light-emitting diode device of this application includes an anode, a hole injection layer, a hole transport layer, a quantum dot light-emitting layer, an electron transport layer, and a cathode. The quantum dot light-emitting layer is a quantum dot thin film prepared by the method of this application.

[0048] In a preferred embodiment, red quantum dot material CdZnSe / ZnSe / ZnS is used as the light-emitting layer of the device. The electroluminescence wavelength of the quantum dot material is 622 nm, and the full width at half maximum (FWHM) is 22 nm. The surface ligand is oleic acid. The light-emitting layer film is treated with methanol solvent atomized into vapor by ultrasonication for 1 min. The quantum dot light-emitting diode device prepared in this way can achieve a maximum current efficiency of 30 cd / A, and there is no significant roll-off with increasing brightness. The measured lifetime T... 95@1000nit = 3170h (the time required for brightness to decay from 1000nit to 95%), and there was no significant brightness increase in the initial stage of the lifetime test, indicating that the surface defects of the quantum dots have been passivated; compared to the device without proton reagent treatment, the maximum current efficiency is 20cd / A, and the efficiency decreases significantly at high brightness, T 95 @1000nit=1000h, there is a brightness increase process of about 5h in the initial stage of lifetime testing, indicating that the surface defects of quantum dot materials are continuously passivated, causing the brightness to increase. The main reason for this difference is that the unpassivated defect states on the surface of quantum dots have a continuous quenching effect on the electrogenerated excitons, causing the luminous efficiency to roll off as the current increases.

[0049] In another preferred embodiment, water was spin-coated onto the green quantum dot luminescent layer using a spin coater at 2000 rpm, with 50 μL added each time, repeated three times. The quantum dots used had a CdZnSeS / ZnS structure, an electroluminescence wavelength of 535 nm, a full width at half maximum (FWHM) of 25 nm, and oleylamine as the surface ligand. The device fabricated in this manner achieved a maximum current efficiency of 80 cd / A, with no significant roll-off as brightness increased. The measured lifetime T... 95 @1000nit = 6400h; the maximum current efficiency of the untreated device can reach 55cd / A, and there is no significant roll-off with increasing brightness. The measured lifetime T 95 @1000nit = 2600h.

[0050] In one embodiment, the anode is selected from one or more of indium tin oxide, fluorine-doped tin oxide, indium zinc oxide, graphene, and carbon nanotubes; the hole injection layer material is one or more of PEDOT:PSS, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide, and copper oxide; the hole transport layer material is one or more of PVK, Poly-TPD, CBP, TCTA, and TFB; the quantum dot light-emitting layer includes a red quantum dot light-emitting layer, a green quantum dot light-emitting layer, and a blue quantum dot light-emitting layer; the quantum dot material includes nano-II-VI semiconductors. The quantum dot light-emitting layer is prepared by the above-described quantum dot film preparation method of this application. The material of the electron transport layer is one or more of n-type ZnO, TiO2, SnO, Ta2O3, AlZnO, ZnSnO, InSnO, and Alq3. The cathode is selected from one or more of Al, Ca, Ba, and Ag.

[0051] The fourth aspect of this application provides a method for fabricating a quantum dot light-emitting diode, such as... Figure 3 As shown, the preparation method includes the following steps:

[0052] E01: Provide substrate;

[0053] E02: An initial quantum dot film is prepared on the substrate, and then the initial quantum dot film is treated with a proton reagent to obtain a quantum dot light-emitting layer.

[0054] The quantum dot thin film preparation method provided in this application involves treating an initial quantum dot thin film on a substrate with a protonating reagent to obtain the quantum dot light-emitting layer. During this treatment, the protonating reagent makes surface contact with the initial quantum dot thin film, causing the protonating reagent to be protonated and connected to dangling bonds on the quantum dot surface. This passivates surface defects of the quantum dot and reduces the quenching of excitons due to defect states. Therefore, this quantum dot light-emitting diode preparation method can ultimately improve the luminous efficiency and lifespan of the device.

[0055] Specifically, an initial quantum dot film is formed on a provided substrate, and then the initial quantum dot film is treated with a proton reagent to obtain a quantum dot light-emitting layer. The initial quantum dot film can be a wet film or a dry film; this application preferably uses a dry, solid initial quantum dot film, that is, this application preferably deposits a quantum dot solution on the substrate and then removes the solvent to obtain the initial quantum dot film.

[0056] Further, the protonating agent is a liquid protonating agent, and the step of treating the initial quantum dot film with the protonating agent includes: depositing the liquid protonating agent on the surface of the initial quantum dot film, followed by annealing; or, the protonating agent is a gaseous protonating agent, and the step of treating the initial quantum dot film with the protonating agent includes: placing the initial quantum dot film in a gaseous protonating agent for a static treatment, followed by annealing. The step of depositing the liquid protonating agent on the surface of the initial quantum dot film and then annealing includes: applying the liquid protonating agent at a rate of 3-20 μl / cm² each time. 2 Spin-coating is performed 2-5 times; subsequent annealing is carried out at 60-100℃ for 5-20 minutes. Alternatively, the initial quantum dot film can be placed in a gaseous proton reagent for 30 seconds to 5 minutes, followed by annealing at 60-100℃ for 5-20 minutes. The specific details of these two methods have been described above.

[0057] Furthermore, the proton reagent includes at least one of hydroxyl-containing proton reagents and amino-containing proton reagents. The hydroxyl-containing proton reagent includes at least one of water, methanol, ethanol, propanol, butanol, pentanol, formic acid, acetic acid, propionic acid, and butyric acid; the amino-containing proton reagent includes at least one of methylamine, ethylamine, and propylamine.

[0058] In the above-mentioned method for fabricating quantum dot light-emitting diodes, the substrate used can be either an anode substrate or a cathode substrate.

[0059] In one embodiment, the substrate is an anode substrate. After fabricating a quantum dot light-emitting layer on the anode substrate, a cathode is further fabricated on the quantum dot light-emitting layer. Before fabricating the quantum dot light-emitting layer, a hole functional layer (such as a hole transport layer, or a sequentially stacked hole injection layer and hole transport layer) can be fabricated on the anode substrate, and then the quantum dot light-emitting layer can be fabricated on the hole functional layer. After fabricating the quantum dot light-emitting layer, an electron functional layer (such as an electron transport layer, or a sequentially stacked electron transport layer and electron injection layer) can be fabricated on the quantum dot light-emitting layer, and then the cathode can be fabricated on the electron functional layer.

[0060] In one embodiment, the substrate is a cathode substrate. After a quantum dot light-emitting layer is fabricated on the cathode substrate, an anode is further fabricated on the quantum dot light-emitting layer. Before fabricating the quantum dot light-emitting layer, an electronic functional layer (such as an electron transport layer, or a sequentially stacked electron injection layer and electron transport layer) can be fabricated on the cathode substrate, and then the quantum dot light-emitting layer can be fabricated on the electronic functional layer. After fabricating the quantum dot light-emitting layer, a hole functional layer (such as a hole transport layer, or a sequentially stacked hole transport layer and hole injection layer) can be fabricated on the quantum dot light-emitting layer, and then the cathode can be fabricated on the hole functional layer.

[0061] The following description is based on specific embodiments.

[0062] Example 1

[0063] A quantum dot light-emitting diode, such as Figure 2 As shown, it includes an anode, a hole injection layer, a hole transport layer, a quantum dot light-emitting layer, an electron transport layer, and a cathode.

[0064] The fabrication method of this device includes:

[0065] PEDOT:PSS material was spin-coated onto the ITO anode layer and then annealed at 100°C for 15 min to obtain a hole injection layer. TFB material was then spin-coated onto the hole injection layer and annealed at 100°C for 15 min to form a hole transport layer. A CdZnSe / ZnSe / ZnS red quantum dot layer was formed on the hole transport layer, which serves as the carrier. The device was then placed in a methanol atmosphere with ultrasonic atomization and left to stand for 1 min. After removal, it was annealed at 80°C for 10 min to obtain a quantum dot emitting layer. A ZnO electron transport layer was fabricated on the quantum dot emitting layer. Finally, an Al cathode electrode layer was deposited by vapor deposition, and the device was encapsulated to form an electroluminescent device.

[0066] The photoelectric performance and lifetime of this quantum dot light-emitting diode device were tested, and the test results are shown in Table 1 and 2. Figure 3-4 As shown.

[0067] Example 2

[0068] A quantum dot light-emitting diode, such as Figure 2 As shown, it includes an anode, a hole injection layer, a hole transport layer, a quantum dot light-emitting layer, an electron transport layer, and a cathode.

[0069] The fabrication method of this device includes:

[0070] PEDOT:PSS material was spin-coated onto the ITO anode layer and then annealed at 100°C for 15 min to obtain a hole injection layer. TFB material was then spin-coated onto the hole injection layer and annealed at 100°C for 15 min to form a hole transport layer. A CdZnSeS / ZnS green quantum dot layer was formed on the hole transport layer, which serves as the carrier layer. A distilled water film was then spin-coated onto this green quantum dot layer using a spin coater at 2000 rpm, with 50 μL of distilled water applied each time, repeated three times. The layer was then annealed on a hot plate at 80°C for 10 min to obtain a quantum dot luminescent layer. A ZnO electron transport layer was fabricated on the quantum dot luminescent layer. Finally, an Ag cathode electrode layer was deposited by vapor deposition, and the device was encapsulated to form an electroluminescent device.

[0071] The photoelectric performance and lifetime of the quantum dot light-emitting diode device were tested, and the test results are shown in Table 1.

[0072] Comparative Example 1

[0073] A quantum dot light-emitting diode, such as Figure 2 As shown, it includes an anode, a hole injection layer, a hole transport layer, a quantum dot light-emitting layer, an electron transport layer, and a cathode.

[0074] The materials and fabrication methods for each layer of this device are the same as in Example 1, except that the quantum dot emitting layer is formed directly on the hole transport layer as a CdZnSe / ZnSe / ZnS red quantum dot layer.

[0075] The photoelectric performance and lifetime of this quantum dot light-emitting diode device were tested, and the test results are shown in Table 1 and 2. Figure 3-4 As shown.

[0076] Comparative Example 2

[0077] A quantum dot light-emitting diode, such as Figure 2 As shown, it includes an anode, a hole injection layer, a hole transport layer, a quantum dot light-emitting layer, an electron transport layer, and a cathode.

[0078] The materials and fabrication methods for each layer of this device are the same as in Example 2, except that the quantum dot emitting layer is formed directly on the hole transport layer as a CdZnSeS / ZnS green quantum dot layer.

[0079] The photoelectric performance and lifetime of the quantum dot light-emitting diode device were tested, and the test results are shown in Table 1.

[0080] Test Results

[0081] The above embodiments and comparative examples were tested. The device lifetime testing used a customized 128-channel lifetime testing system from Guangzhou New Vision Company. The system architecture consisted of a constant voltage / constant current source driving the QLED to test changes in voltage or current; a photodiode detector and testing system to test changes in the QLED's brightness (photocurrent); and a luminance meter to test and calibrate the QLED's brightness (photocurrent). The results are as follows: Figure 4-5 And as shown in Table 1.

[0082] Table 1

[0083] EL(nm) FWHM(nm) EQE (%) CE(cd / A) <![CDATA[T 95 @1000nit(h)]]> Example 1 626 22 19.9 27 3170 Example 2 535 25 18 80 6400 Comparative Example 1 626 22 10 13.5 1260 Comparative Example 2 535 25 11 55 2600

[0084] As can be seen from the data in Table 1, compared with the control group that was not treated with proton reagents, the embodiments of this application passivate the surface defect states of quantum dots by treating the quantum dot light-emitting layer in the quantum dot light-emitting diode with proton reagents during the preparation process, thereby improving the luminous efficiency and lifespan of the device.

[0085] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method for preparing a quantum dot thin film, characterized in that, Includes the following steps: Provide initial quantum dot films; The initial quantum dot film was treated with a proton reagent to obtain a quantum dot film; In this process, the protonating reagent is protonated and dehydrogenated at the defect sites on the quantum dot surface of the initial quantum dot film and forms a coordinate bond with the unsaturated cations on the quantum dot surface. At the same time, some of the initial ligands on the quantum dot surface of the initial quantum dot film are replaced by the protonated protonating reagent. The processing steps include: depositing a liquid protonating agent on the surface of the initial quantum dot film, followed by a first annealing treatment; or, placing the initial quantum dot film in a gaseous protonating agent for a static treatment, followed by a second annealing treatment. The proton reagent includes at least one of a hydroxyl-containing proton reagent and an amino-containing proton reagent. The hydroxyl-containing proton reagent includes at least one of water, methanol, ethanol, propanol, butanol, pentanol, formic acid, acetic acid, propionic acid, and butyric acid. The amino-containing proton reagent includes at least one of methylamine, ethylamine, and propylamine.

2. The preparation method according to claim 1, characterized in that, The method for preparing the initial quantum dot film includes: depositing a quantum dot solution on a substrate, and then performing a solvent removal process to obtain the initial quantum dot film.

3. The preparation method according to claim 1, characterized in that, The step of depositing a liquid protonating agent on the surface of the initial quantum dot film, followed by a first annealing treatment, includes: adding the liquid protonating agent at a rate of 3-20 μl / cm³ each time. 2 Spin coat 2-5 times; and / or, The temperature of the first annealing treatment is 60-100℃, and the time is 5-20 minutes.

4. The preparation method according to claim 1, characterized in that, The settling time is 30 seconds to 5 minutes; and / or, The second annealing treatment is performed at a temperature of 60-100℃ for 5-20 minutes.

5. A quantum dot thin film, characterized in that, The quantum dot film is prepared by the preparation method according to any one of claims 1-4.

6. A quantum dot light-emitting diode, comprising an anode, a cathode, and a quantum dot light-emitting layer located between the anode and the cathode, characterized in that, The quantum dot light-emitting layer is the quantum dot thin film as described in claim 5.

7. A method for fabricating a quantum dot light-emitting diode, characterized in that, Includes the following steps: A substrate is provided; an initial quantum dot film is prepared on the substrate, and then the initial quantum dot film is treated with a proton reagent to obtain a quantum dot light-emitting layer; In this process, the protonating reagent is protonated and dehydrogenated at the defect sites on the quantum dot surface of the initial quantum dot film and forms a coordinate bond with the unsaturated cations on the quantum dot surface. At the same time, some of the initial ligands on the quantum dot surface of the initial quantum dot film are replaced by the protonated protonating reagent. The processing steps include: depositing a liquid protonating agent on the surface of the initial quantum dot film, followed by a first annealing treatment; or, placing the initial quantum dot film in a gaseous protonating agent for a static treatment, followed by a second annealing treatment. The proton reagent includes at least one of a hydroxyl-containing proton reagent and an amino-containing proton reagent. The hydroxyl-containing proton reagent includes at least one of water, methanol, ethanol, propanol, butanol, pentanol, formic acid, acetic acid, propionic acid, and butyric acid. The amino-containing proton reagent includes at least one of methylamine, ethylamine, and propylamine.

8. The preparation method according to claim 7, characterized in that, The method for preparing the initial quantum dot film includes: depositing a quantum dot solution on the substrate, and then performing a solvent removal process to obtain the initial quantum dot film.

9. The preparation method according to claim 7, characterized in that, The step of depositing a liquid proton reagent on the surface of the initial quantum dot film includes: adding the liquid proton reagent at a rate of 3-20 μl / cm³ each time. 2 Apply the amount of product by spin coating 2-5 times; or, The settling time is 30 seconds to 5 minutes.

Citation Information

Patent Citations

  • Quantum dot electroluminescent device and preparation method thereof

    CN110224074A

  • Preparation method of quantum dot film and preparation method of quantum dot light-emitting diode

    CN111129355A