A method for preparing a tail-type micro-cantilever atomic force scanning probe

By preparing a trailing micro-cantilever atomic force scanning probe in an atomic force microscope, and using SOI wafer and photolithography technology, the problem of spectrum shift caused by samples with different mechanical parameters has been solved, and the stability and stability of the probe spectrum have been achieved. Rapid mechanical parameter measurement supports non-destructive detection of superficial defects.

CN115267261BActive Publication Date: 2024-10-11UNIV OF SCI & TECH OF CHINA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210960971.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-11
Publication Date
2024-10-11
Estimated Expiration
2042-08-11

AI Technical Summary

Technical Problem

In contact resonance microscopy imaging with atomic force microscopy, samples with different mechanical parameters cause the probe contact resonance spectrum to shift, making it difficult to achieve rapid mechanical parameter measurement and non-destructive detection of superficial defects.

Method used

The preparation method of the trailing micro-cantilever atomic force scanning probe is adopted, and the SOI wafer is used as the starting sample, and the composite beam structure including the main beam and the inner beam is prepared using photolithography and dry etching technology to realize the probe tip and The suspended release of the composite beam ensures that the spectrum does not change with changes in the mechanical properties of the material.

Benefits of technology

It achieves the stability of the probe spectrum, supports rapid mechanical parameter measurement and non-destructive detection of superficial defects, can analyze the mechanical properties of materials based on the resonance peak amplitude, and improves the accuracy and efficiency of imaging results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115267261B_ABST
    Figure CN115267261B_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a trailing micro-cantilever atomic force scanning probe. The main body of the probe is an SOI wafer. The probe tip structure is first obtained on the front side by photolithography and dry etching, and then the structure of the composite beam is obtained by photolithography and dry etching. Finally, the micro-cantilever in the effective area is released from the back side by dry etching. Experimental results show that the cantilever beam of the probe prepared by the preparation method is a composite beam including a main beam and an inner beam. The size, thickness and pattern of the composite beam can be customized. The minimum spacing between the main beam and the inner beam can be 1μm, and the minimum thickness can be 1μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of atomic force microscopes, and more specifically to a method for preparing a trailing micro-cantilever atomic force scanning probe. Background Art

[0002] Atomic force microscopy can measure the mechanical parameters of samples using the working mode of ultrasonic atomic force microscopy. In this working mode, the tip of the probe is inserted into the sample. Under the action of external excitation, the microcantilever tip or the sample vibrates. By analyzing the spectrum during the vibration process, relevant information about the sample can be obtained. However, for samples with different mechanical parameters, the resonance peak frequency is different.

[0003] like Figure 1 (a) shows a two-phase material, in which material B is embedded and grown in the matrix material A to form an island structure. This type of material is often seen in two-phase and multi-phase polymer materials, and there are obvious differences in mechanical properties between different materials. This difference in mechanical properties will lead to a shift in the contact resonance spectrum when the probe acts on different phase materials in contact resonance atomic force microscopy imaging. Figure 1 As shown in (b), when the embedded material B has a larger elastic modulus than the matrix material A, the probe contact resonance spectrum will shift significantly toward the high frequency direction. At the same time, if it has a smaller damping loss, the probe contact resonance spectrum quality factor Q value will also increase significantly, resulting in a large difference in the shape of the contact resonance spectrum on the two materials. At this time, when different excitation frequencies are used in the contact resonance atomic force microscopy imaging process, it can be easily based on Figure 1 (b) The spectrum determines the amplitude of different phase materials at the imaging frequency, so the amplitude contrast of the two materials in the imaging results can also be determined. When imaging is performed according to the five excitation frequencies from left to right as shown in the figure, it can be determined that the amplitude imaging result will be as follows: Figure 1 As shown in (c), it can be found that with the change of the excitation frequency, not only the absolute value of the imaging contrast (i.e., the image contrast) will change, but also the relative contrast between the two materials will change at a certain frequency point (i.e., Figure 1 (b) The contrast inversion phenomenon occurs around the intersection of the two spectra. Summary of the invention

[0004] In view of this, an object of the present invention is to provide a method for preparing a tail-type micro-cantilever atomic force scanning probe. The tail-type micro-cantilever atomic force scanning probe obtained by the preparation method provided by the present invention can have a resonance peak frequency in the spectrum that does not change with the change of the mechanical properties of the material, thereby realizing rapid mechanical parameter measurement and non-destructive detection of shallow surface defects.

[0005] The present invention provides a method for preparing a tailing micro-cantilever atomic force scanning probe, comprising the following steps:

[0006] a) selecting an SOI wafer as a starting sample, wherein the SOI wafer comprises a top device silicon layer, an intermediate oxide layer and a substrate silicon layer;

[0007] b) growing a silicon oxide layer on the top device silicon layer;

[0008] c) forming a circular photoresist mask with a diameter of 0.5 μm to 1 μm on the silicon oxide layer using a photoresist;

[0009] d) removing the silicon oxide layer on the top device silicon layer that is not covered by the circular photoresist mask, and removing the photoresist;

[0010] e) After rinsing the sample, etching the top device silicon layer to form a conical needle tip structure with a height of 11.5 μm to 13 μm;

[0011] f) using photoresist to form a photoresist mask on the surface of the top device silicon layer to hollow out the composite beam structure;

[0012] g) etching the top device silicon layer until the middle oxide layer is exposed to obtain a composite beam structure, and removing the photoresist;

[0013] h) depositing a silicon oxide layer on the surface of the top device silicon layer and the surface of the substrate silicon layer respectively;

[0014] i) using photoresist to protect the composite beam structure and the conical needle tip structure on the surface of the top device silicon layer, and using photoresist to cover the structure to be retained on the surface of the substrate silicon layer;

[0015] j) removing the silicon oxide layer on the substrate surface not covered by the photoresist;

[0016] k) etching the substrate silicon layer until 20 μm to 40 μm remain, and removing the photoresist;

[0017] l) using the silicon oxide layer of the substrate silicon layer as a mask, etching the remaining substrate silicon layer until the middle oxide layer is exposed;

[0018] m) using gaseous HF to release the silicon oxide layer on the surface of the top device silicon layer, the remaining silicon oxide layer on the surface of the substrate silicon layer and the intermediate oxide layer, thereby obtaining a trailing micro-cantilever atomic force scanning probe.

[0019] Preferably, in step a), the thickness of the top device silicon layer is 10 μm to 20 μm; the thickness of the intermediate oxide layer is 0.5 μm to 3 μm; and the thickness of the substrate silicon layer is 300 μm to 500 μm.

[0020] Preferably, the method of growing the silicon oxide layer in step b) is plasma enhanced chemical vapor deposition, and the thickness of the silicon oxide layer is 50 nm to 300 nm.

[0021] Preferably, the process of forming a circular photoresist mask with a diameter of 0.5 μm to 1 μm on the silicon oxide layer using photoresist in step c) is specifically as follows:

[0022] Spin-coat a photoresist with a thickness of 1 μm to 3 μm on the top device silicon layer and bake it on a hot plate at 100°C to 120°C for 60s to 120s; use a UV photolithography machine for exposure, with an exposure dose of 300mJ / cm 2 ~600mJ / cm 2 After the exposure is completed, the sample is developed in a developer at room temperature for 40s to 60s, and then the sample is placed on a hot plate at 100℃ to 120℃ to harden the film for 2min to 5min to form a circular photoresist mask with a diameter of 0.5μm to 1μm.

[0023] Preferably, in step d), the device for removing the silicon oxide layer on the top device silicon layer not covered by the circular photoresist mask is a reactive ion etcher; and the method for removing the photoresist is to place the NMP solution in a water bath at 70° C. to 90° C. for 10 min to 30 min.

[0024] Preferably, the rinsing treatment in step e) uses a BOE buffered oxide etchant with a volume ratio of 48wt% to 50wt% HF aqueous solution: 35wt% to 45wt% NH4F aqueous solution = 1: (6 to 8) to rinse the sample for 5s to 30s;

[0025] The method of etching the top device silicon layer to form a conical needle tip structure with a height of 11.5μm to 13μm is a Cryo silicon process, and the etching conditions are: 92sccm SF6, 15-25sccm O2, 12mTorr, 600W ICP, 8W RF, -100℃.

[0026] Preferably, the process of using photoresist to form a photoresist mask for hollowing out the composite beam structure on the surface of the top device silicon layer in step f) is specifically as follows:

[0027] A photoresist with a thickness of 0.8μm to 1.5μm is spin-coated on the surface of the top device silicon layer and baked on a hot plate at 100℃ to 120℃ for 60s to 120s. A high-resolution exposure overlay is performed using a Heidelberg laser direct writing device in a gas-focused high depth of field mode with an exposure dose of 90mW to 120mW. The developer is used for development for 40s to 60s, and the film is hardened on a hot plate at 100℃ to 120℃ for 2min to 5min to form a photoresist mask that hollows out the composite beam structure.

[0028] Preferably, the method of etching the top device silicon layer in step g) is the Bosch silicon process; the method of removing the photoresist is to use NMP solution in a water bath at 70° C. to 90° C. for 10 min to 30 min.

[0029] Preferably, the silicon oxide layer is deposited in step h) by low pressure chemical vapor deposition, and the thickness of the silicon oxide layer is 300 nm to 1000 nm.

[0030] Preferably, the process of using photoresist to protect the composite beam structure and the conical needle tip structure on the surface of the top device silicon layer in step i) is specifically as follows:

[0031] Spin-coat a photoresist with a thickness of 10 μm to 20 μm on the surface of the top device silicon layer to protect the front composite beam structure and the conical needle tip structure, and bake on a hot plate at 85° C. to 95° C. for 10 min to 30 min;

[0032] The process of using photoresist to cover the structure to be retained on the surface of the substrate silicon layer is specifically as follows:

[0033] Spin-coat a photoresist with a thickness of 8 μm to 10 μm on the surface of the substrate silicon layer and bake it on a hot plate at 85°C to 95°C for 5 min to 10 min. Use a UV lithography machine to perform back-overlay exposure with an exposure dose of 700 mJ / cm 2 ~1000mJ / cm 2 , use developer to develop for 4min to 6min, and harden the film on a hot plate at 90℃ to 110℃ for 5min to 15min.

[0034] The invention provides a method for preparing a trailing micro-cantilever atomic force scanning probe, comprising the following steps: a) selecting an SOI wafer as a starting sample, wherein the SOI wafer comprises a top device silicon layer, an intermediate oxide layer and a substrate silicon layer; b) growing a silicon oxide layer on the top device silicon layer; c) using photoresist to form a circular photoresist mask with a diameter of 0.5 μm to 1 μm on the silicon oxide layer; d) removing the silicon oxide layer on the top device silicon layer that is not covered by the circular photoresist mask, and removing the photoresist; e) after rinsing the sample, etching the top device silicon layer to form a conical needle tip structure with a height of 11.5 μm to 13 μm; f) using photoresist to form a photoresist mask with a composite beam structure hollowed out on the surface of the top device silicon layer; g) etching the top device silicon layer. The method comprises the following steps: h) depositing silicon oxide layers on the surface of the top device silicon layer and the surface of the substrate silicon layer respectively; i) using photoresist to protect the composite beam structure and the conical needle tip structure on the surface of the top device silicon layer, and using photoresist to cover the structure to be retained on the surface of the substrate silicon layer; j) removing the silicon oxide layer on the substrate surface not covered by the photoresist; k) etching the substrate silicon layer until 20 μm to 40 μm remain, and removing the photoresist; l) using the silicon oxide layer of the substrate silicon layer as a mask, etching the remaining substrate silicon layer until the middle oxide layer is exposed; m) using gaseous HF to release the silicon oxide layer on the surface of the top device silicon layer, the remaining silicon oxide layer on the surface of the substrate silicon layer and the middle oxide layer, to obtain a trailing micro-cantilever atomic force scanning probe. Compared with the prior art, the main body of the probe prepared by the preparation method provided by the present invention is an SOI wafer, and the probe tip structure is first obtained on the front side by photolithography and dry etching, and then the structure of the composite beam is obtained by photolithography and dry etching, and finally the micro-cantilever beam in the effective area is released from the back side by dry etching; experimental results show that the cantilever beam of the probe prepared by the preparation method is a composite beam including a main beam and an inner beam, and the size, thickness and pattern of the composite beam can be customized, the minimum spacing between the main beam and the inner beam can be achieved to be 1μm, and the minimum thickness can be achieved to be 1μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic diagram of the technical problems of the prior art micro-cantilever atomic force scanning probe in detecting samples with different mechanical parameters;

[0036] Figure 2 A processing flow chart of a method for preparing a trailing micro-cantilever atomic force scanning probe provided by an embodiment of the present invention;

[0037] Figure 3 A physical picture of a trailing micro-cantilever atomic force scanning probe manufactured and processed according to an embodiment of the present invention;

[0038] Figure 4The frequency-amplitude relationship curve obtained by scanning molybdenum disulfide and graphene at a set frequency using the trailing microcantilever atomic force scanning probe processed and prepared by the embodiment of the present invention;

[0039] Figure 5 The amplitude diagram is obtained by scanning molybdenum disulfide and graphene at a set frequency using the trailing micro-cantilever atomic force scanning probe processed and prepared by an embodiment of the present invention. DETAILED DESCRIPTION

[0040] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The present invention provides a method for preparing a tailing micro-cantilever atomic force scanning probe, comprising the following steps:

[0042] a) selecting an SOI wafer as a starting sample, wherein the SOI wafer comprises a top device silicon layer, an intermediate oxide layer and a substrate silicon layer;

[0043] b) growing a silicon oxide layer on the top device silicon layer;

[0044] c) forming a circular photoresist mask with a diameter of 0.5 μm to 1 μm on the silicon oxide layer using a photoresist;

[0045] d) removing the silicon oxide layer on the top device silicon layer that is not covered by the circular photoresist mask, and removing the photoresist;

[0046] e) After rinsing the sample, etching the top device silicon layer to form a conical needle tip structure with a height of 11.5 μm to 13 μm;

[0047] f) using photoresist to form a photoresist mask on the surface of the top device silicon layer to hollow out the composite beam structure;

[0048] g) etching the top device silicon layer until the middle oxide layer is exposed to obtain a composite beam structure, and removing the photoresist;

[0049] h) depositing a silicon oxide layer on the surface of the top device silicon layer and the surface of the substrate silicon layer respectively;

[0050] i) using photoresist to protect the composite beam structure and the conical needle tip structure on the surface of the top device silicon layer, and using photoresist to cover the structure to be retained on the surface of the substrate silicon layer;

[0051] j) removing the silicon oxide layer on the substrate surface not covered by the photoresist;

[0052] k) etching the substrate silicon layer until 20 μm to 40 μm remain, and removing the photoresist;

[0053] l) using the silicon oxide layer of the substrate silicon layer as a mask, etching the remaining substrate silicon layer until the middle oxide layer is exposed;

[0054] m) using gaseous HF to release the silicon oxide layer on the surface of the top device silicon layer, the remaining silicon oxide layer on the surface of the substrate silicon layer and the intermediate oxide layer, thereby obtaining a trailing micro-cantilever atomic force scanning probe.

[0055] In the present invention, the SOI wafer in step a) is preferably a double-sided polished SOI wafer; the present invention has no special limitation on its source, and commercially available products known to those skilled in the art can be used.

[0056] In the present invention, the thickness of the top device silicon layer in step a) is preferably 10 μm to 20 μm; the thickness of the intermediate oxide layer is preferably 0.5 μm to 3 μm; and the thickness of the substrate silicon layer is preferably 300 μm to 500 μm.

[0057] In the present invention, the method of growing the silicon oxide layer in step b) is preferably plasma enhanced chemical vapor deposition (PECVD); in step b), a thinner silicon oxide layer needs to be used as a mask to facilitate precise control of the needle tip etching height, and the thickness of the silicon oxide layer is preferably 50nm to 300nm.

[0058] In the present invention, the process of forming a circular photoresist mask with a diameter of 0.5 μm to 1 μm on the silicon oxide layer using photoresist in step c) is preferably specifically as follows:

[0059] Spin-coat a photoresist with a thickness of 1 μm to 3 μm on the top device silicon layer and bake it on a hot plate at 100°C to 120°C for 60s to 120s; use a UV photolithography machine for exposure, with an exposure dose of 300mJ / cm 2 ~600mJ / cm 2 After the exposure is completed, the sample is developed in a developer at room temperature for 40s to 60s, and then the sample is placed on a hot plate at 100°C to 120°C to harden the film for 2min to 5min, forming a circular photoresist mask with a diameter of 0.5μm to 1μm. The present invention has no special restrictions on the types and sources of the photoresist and developer.

[0060] In the present invention, the device for removing the silicon oxide layer on the top device silicon layer not covered by the circular photoresist mask in step d) is preferably a reactive ion etcher; the method for removing the photoresist is preferably a NMP solution 70°C to 90°C water bath for 10min to 30min.

[0061] In the present invention, the rinsing treatment in step e) preferably uses a BOE buffered oxide etching solution with a volume ratio of 48wt% to 50wt% HF aqueous solution: 35wt% to 45wt% NH4F aqueous solution = 1: (6 to 8) to rinse the sample for 5s to 30s; the BOE rinsing treatment of the sample in step e) is mainly to remove the residual silicon oxide after etching the needle tip silicon oxide mask, which can effectively avoid the formation of a micro-mask effect when etching the needle tip by the Cryo process.

[0062] In the present invention, the method of etching the top device silicon layer in step e) to form a conical needle tip structure with a height of 11.5μm to 13μm is preferably a Cryo silicon process, and the etching conditions are: 92sccm SF6, 15-25sccm O2, 12mTorr, 600WICP, 8W RF, -100℃; the tilt angle can be adjusted by the etching gas ratio. In order to avoid the cumbersome process of conventional needle tip preparation, the present invention proposes a new needle tip preparation method: using a low-temperature etching method to directly obtain a conical needle tip structure with an adjustable tilt angle.

[0063] In the present invention, the process of using photoresist to form a photoresist mask for hollowing out the composite beam structure on the surface of the top device silicon layer in step f) is preferably specifically as follows:

[0064] Spin-coat a photoresist with a thickness of 0.8 μm to 1.5 μm on the surface of the top device silicon layer, and bake it on a hot plate at 100°C to 120°C for 60s to 120s, and use the Heidelberg laser direct writing equipment to perform high-resolution exposure and overlay, with an exposure dose of 90mW to 120mW, and use a developer to develop for 40s to 60s, and harden the film on a hot plate at 100°C to 120°C for 2min to 5min to form a photoresist mask with a hollowed-out composite beam structure. Step f) requires the use of the Heidelberg laser direct writing equipment to perform high-resolution exposure and overlay, because the needle tip height is relatively high, and the conventional ultraviolet exposure mode cannot achieve high-resolution exposure and overlay. Therefore, in view of the high needle tip height, the requirement of 1μm to 2μm high resolution is required when overlaying and etching the composite beam, and the laser direct writing high-depth-of-field gas-focusing exposure mode is adopted.

[0065] In the present invention, the method of etching the top device silicon layer in step g) is preferably the Bosch silicon process; the method of removing the photoresist is preferably NMP solution 70° C. to 90° C. water bath for 10 min to 30 min.

[0066] In the present invention, the method of depositing the silicon oxide layer in step h) is preferably low-pressure chemical vapor deposition (LPCVD). In step h), the silicon oxide of a certain thickness grown by LPCVD on the front side of the composite beam can offset part of the stress of the intermediate silicon oxide sacrificial layer, ensuring that the composite beam will not break simply due to the stress of the intermediate oxide layer when released, and at the same time, the probe tip can be sharpened to a certain extent; the thickness of the silicon oxide layer is 300nm to 1000nm.

[0067] In the present invention, the process of using photoresist to protect the composite beam structure and the conical needle tip structure on the surface of the top device silicon layer in step i) is preferably specifically as follows:

[0068] Spin-coat a photoresist with a thickness of 10 μm to 20 μm on the surface of the top device silicon layer to protect the front composite beam structure and the conical needle tip structure, and bake on a hot plate at 85° C. to 95° C. for 10 min to 30 min;

[0069] The process of using photoresist to cover the structure to be retained on the surface of the substrate silicon layer is preferably as follows:

[0070] Spin-coat a photoresist with a thickness of 8 μm to 10 μm on the surface of the substrate silicon layer and bake it on a hot plate at 85°C to 95°C for 5 min to 10 min. Use a UV lithography machine to perform back-overlay exposure with an exposure dose of 700 mJ / cm 2 ~1000mJ / cm 2 , use developer to develop for 4min to 6min, and harden the film on a hot plate at 90℃ to 110℃ for 5min to 15min.

[0071] In the present invention, the device for removing the silicon oxide layer on the substrate surface not covered by the photoresist in step j) is preferably a reactive ion etching device.

[0072] In the present invention, the method of etching the substrate silicon layer until 20μm to 40μm remain in step k) is preferably the Bosch silicon process; the substrate silicon is etched by the silicon Bosch process until 20μm to 40μm remain, and the front protective glue is removed, mainly because the glue is difficult to remove after dry etching. If the glue is removed directly after the silicon is etched, the beam is relatively thin and easily broken; if there are 20μm to 40μm of silicon remaining, the beam has better support; the method of removing the photoresist is preferably NMP solution 70℃ to 90℃ water bath for 10min to 30min.

[0073] In the present invention, the method of etching the remaining substrate silicon layer until the middle oxide layer is exposed in step 1) is preferably a Bosch silicon process.

[0074] In the present invention, gaseous HF is used in step m) to release all silicon oxide layers, thereby avoiding damage to the beam caused by solution tension when using HF solution to remove silicon oxide.

[0075] The invention provides a method for preparing a trailing micro-cantilever atomic force scanning probe, comprising the following steps: a) selecting an SOI wafer as a starting sample, wherein the SOI wafer comprises a top device silicon layer, an intermediate oxide layer and a substrate silicon layer; b) growing a silicon oxide layer on the top device silicon layer; c) using photoresist to form a circular photoresist mask with a diameter of 0.5 μm to 1 μm on the silicon oxide layer; d) removing the silicon oxide layer on the top device silicon layer that is not covered by the circular photoresist mask, and removing the photoresist; e) after rinsing the sample, etching the top device silicon layer to form a conical needle tip structure with a height of 11.5 μm to 13 μm; f) using photoresist to form a photoresist mask with a composite beam structure hollowed out on the surface of the top device silicon layer; g) etching the top device silicon layer. The method comprises the following steps: h) depositing silicon oxide layers on the surface of the top device silicon layer and the surface of the substrate silicon layer respectively; i) using photoresist to protect the composite beam structure and the conical needle tip structure on the surface of the top device silicon layer, and using photoresist to cover the structure to be retained on the surface of the substrate silicon layer; j) removing the silicon oxide layer on the substrate surface not covered by the photoresist; k) etching the substrate silicon layer until 20 μm to 40 μm remain, and removing the photoresist; l) using the silicon oxide layer of the substrate silicon layer as a mask, etching the remaining substrate silicon layer until the middle oxide layer is exposed; m) using gaseous HF to release the silicon oxide layer on the surface of the top device silicon layer, the remaining silicon oxide layer on the surface of the substrate silicon layer and the middle oxide layer, to obtain a trailing micro-cantilever atomic force scanning probe. Compared with the prior art, the main body of the probe prepared by the preparation method provided by the present invention is an SOI wafer, and the probe tip structure is first obtained on the front side by photolithography and dry etching, and then the structure of the composite beam is obtained by photolithography and dry etching, and finally the micro-cantilever beam in the effective area is released from the back side by dry etching; experimental results show that the cantilever beam of the probe prepared by the preparation method is a composite beam including a main beam and an inner beam, and the size, thickness and pattern of the composite beam can be customized, the minimum spacing between the main beam and the inner beam can be achieved to be 1μm, and the minimum thickness can be achieved to be 1μm.

[0076] In order to further illustrate the present invention, the following examples are provided for detailed description.

[0077] Example

[0078] See also Figure 2 As shown, Figure 2 The processing flow chart of the method for preparing the trailing micro-cantilever atomic force scanning probe provided by the embodiment of the present invention; the specific process is as follows:

[0079] (1) Double-sided polished SOI wafers were selected as the starting sample. The thickness of the top device silicon layer 1 was 15 μm, the thickness of the middle oxide layer 2 was 1 μm, and the thickness of the substrate silicon layer 3 was 300 μm ( Figure 2 a).

[0080] (2) Using plasma enhanced chemical vapor deposition (PECVD) to grow a 300 nm silicon oxide layer 4 on the top device silicon layer 1 ( Figure 2 b).

[0081] (3) Spin-coat 2 μm thick NR9-3000PY photoresist 5 on the top device silicon layer 1 and bake on a 120°C hot plate for 90 seconds; use a SUSS MA6 UV lithography machine for exposure, with an exposure dose of 400 mJ / cm 2 Then, the sample was developed with developer AZ300MIF for 50 seconds and fixed with ultrapure water for 30 seconds. Finally, the sample was placed on a hot plate at 120°C for 2 minutes to form a circular photoresist mask with a diameter of 1 μm ( Figure 2 c).

[0082] (4) Using Oxford NGP80 reactive ion etcher to remove the silicon oxide layer 4 on 1 that is not covered by the photoresist, and using NMP solution in a water bath at 80°C for 15 minutes to remove the photoresist ( Figure 2 d).

[0083] (5) The sample was rinsed for 10 seconds using a BOE buffered oxide etching solution with a volume ratio of 49 wt % HF aqueous solution: 40 wt % NH 4 F aqueous solution = 1:7.

[0084] (6) The top device silicon layer 1 was etched using the Oxford Estrelas Cryo silicon process to form a conical needle tip with a height of 12.5 μm. The tilt angle can be adjusted by the etching gas ratio. The etching conditions are: 92 sccm SF6, 21 sccm O2, 12 mTorr, 600 W ICP, 8 W RF, -100 °C ( Figure 2 e).

[0085] (7) A 1 μm thick S1813 photoresist 6 was spin-coated on the surface of the top device silicon layer 1 and baked on a hot plate at 115° C. for 90 seconds. A high-resolution exposure overlay was performed using a Heidelberg laser direct writing device in a gas-focused high-depth-of-field mode with an exposure power of 105 mW. The photoresist was developed using an AZ300MIF developer for 50 seconds and then fixed with deionized water. The photoresist was hardened at 115° C. for 2 minutes ( Figure 2 f).

[0086] (8) Using the Oxford Estrelas Bosch silicon process, the top device silicon layer 1 is etched until the middle oxide layer 2 is exposed to obtain a composite beam structure, and the photoresist is removed in an NMP 80°C water bath for 15 minutes ( Figure 2 g).

[0087] (9) Using low pressure chemical vapor deposition (LPCVD) to deposit 500 nm silicon oxide layers 7 and 8 on both sides of the sample ( Figure 2 h).

[0088] (10) Spin-coat AZ4620 photoresist 9 with a thickness of 15 μm on the surface of the top device silicon layer 1 to protect the front composite beam and needle tip structure, and bake it on a 90°C hot plate for 10 minutes; Spin-coat AZ4620 photoresist 10 with a thickness of 8 μm on the surface of the substrate silicon layer 8, and bake it on a 90°C hot plate for 10 minutes, and perform back overlay exposure using a SUSS MA6 UV lithography machine, with an exposure dose of 900 mJ / cm 2 , developed with AZ300MIF developer for 5 minutes and then fixed with deionized water, hardened at 100°C for 5 minutes ( Figure 2 i).

[0089] (11) Using Oxford NGP80 reactive ion etching equipment, remove the 500 nm silicon oxide layer 8 ( Figure 2 j).

[0090] (12) The substrate silicon was etched using the Oxford Estrelas Bosch silicon process until 20 μm remained, and the photoresist was removed using NMP 80°C water bath for 15 minutes ( Figure 2 k).

[0091] (13) Using the 0.5 μm silicon oxide on the back as a mask, the remaining 20 μm is etched using the Bosch silicon process until the middle oxide layer is exposed ( Figure 2 l).

[0092] (14) Using gaseous HF to release silicon oxide layers 2, 7 and 8, a microcantilever probe with a sharpened tip is obtained ( Figure 2 m).

[0093] After SEM testing, the actual image of the trailing micro-cantilever atomic force scanning probe processed and prepared in the embodiment of the present invention is shown in Figure 3 shown.

[0094] Figures 4-5 The frequency-amplitude relationship curve and amplitude diagram obtained by scanning molybdenum disulfide and graphene at a set frequency using the trailing micro-cantilever atomic force scanning probe processed and prepared by the embodiment of the present invention; Figure 4It can be seen that material A and material B have a common resonance frequency, but different resonance peak amplitudes. The mechanical properties of the two materials are reflected in the resonance peak amplitude. The elastic modulus of the sample can be quantitatively measured by analyzing the resonance peak amplitude. Compared with the method of tracking the resonance peak frequency, the application of the tailing microcantilever atomic force scanning probe can achieve rapid mechanical parameter measurement. At the same time, due to the different contact stiffness of the shallow surface defect surface and the defect-free surface to the needle tip, the probe can also be used for non-destructive detection of shallow surface defects.

[0095] The method for preparing the trailing micro-cantilever atomic force scanning probe provided by the present invention has the following advantages:

[0096] (1) Probes can be mass-produced through micro-nano processing methods, and the size, thickness and pattern of the composite beam can be customized; (2) The present invention proposes a new method for preparing a probe tip, which is to use a silicon low-temperature etching method to directly obtain a conical tip structure with an adjustable inclination angle; (3) Due to the high tip height, a high resolution of 1-2 μm is required when overlay etching the composite beam, which requires the use of a Heidelberg laser direct writing high depth of field gas focusing exposure mode; (4) In order to ensure that the composite beam does not break due to the stress of the intermediate oxide layer when it is released, a certain thickness of oxide layer needs to be deposited on the front of the composite beam using LPCVD to offset part of the stress; (5) In addition to offsetting part of the stress, the use of LPCVD to deposit a certain thickness of oxide layer on the front of the composite beam can also achieve sharpening of the probe tip.

[0097] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a tailing micro-cantilever atomic force scanning probe, comprising the following steps: a) selecting an SOI wafer as a starting sample, wherein the SOI wafer comprises a top device silicon layer, an intermediate oxide layer and a substrate silicon layer; b) growing a silicon oxide layer on the top device silicon layer; c) forming a circular photoresist mask with a diameter of 0.5 μm to 1 μm on the silicon oxide layer using a photoresist; d) removing the silicon oxide layer on the top device silicon layer that is not covered by the circular photoresist mask, and removing the photoresist; e) After rinsing the sample, etching the top device silicon layer to form a conical needle tip structure with a height of 11.5 μm to 13 μm; f) using photoresist to form a photoresist mask on the surface of the top device silicon layer to hollow out the composite beam structure; g) etching the top device silicon layer until the middle oxide layer is exposed to obtain a composite beam structure, and removing the photoresist; h) depositing a silicon oxide layer on the surface of the top device silicon layer and the surface of the substrate silicon layer respectively; i) using photoresist to protect the composite beam structure and the conical needle tip structure on the surface of the top device silicon layer, and using photoresist to cover the structure to be retained on the surface of the substrate silicon layer; j) removing the silicon oxide layer on the substrate surface not covered by the photoresist; k) etching the substrate silicon layer until 20 μm to 40 μm remain, and removing the photoresist; l) using the silicon oxide layer of the substrate silicon layer as a mask, etching the remaining substrate silicon layer until the middle oxide layer is exposed; m) using gaseous HF to release the silicon oxide layer on the surface of the top device silicon layer, the remaining silicon oxide layer on the surface of the substrate silicon layer and the intermediate oxide layer, thereby obtaining a trailing micro-cantilever atomic force scanning probe.

2. The preparation method according to claim 1, characterized in that: In step a), the thickness of the top device silicon layer is 10 μm to 20 μm; the thickness of the intermediate oxide layer is 0.5 μm to 3 μm; and the thickness of the substrate silicon layer is 300 μm to 500 μm.

3. The preparation method according to claim 1, characterized in that: The method of growing the silicon oxide layer in step b) is plasma enhanced chemical vapor deposition, and the thickness of the silicon oxide layer is 50nm to 300nm.

4. The preparation method according to claim 1, characterized in that: The process of forming a circular photoresist mask with a diameter of 0.5 μm to 1 μm on the silicon oxide layer using photoresist in step c) is specifically as follows: Spin-coat a photoresist with a thickness of 1 μm to 3 μm on the top device silicon layer and bake it on a hot plate at 100°C to 120°C for 60s to 120s; use a UV photolithography machine for exposure, with an exposure dose of 300mJ / cm 2 ~600mJ / cm 2 After the exposure is completed, the sample is developed in a developer at room temperature for 40s to 60s, and then the sample is placed on a hot plate at 100℃ to 120℃ to harden the film for 2min to 5min to form a circular photoresist mask with a diameter of 0.5μm to 1μm.

5. The preparation method according to claim 1, characterized in that: The device for removing the silicon oxide layer on the top device silicon layer not covered by the circular photoresist mask in step d) is a reactive ion etcher; the method for removing the photoresist is to place the NMP solution in a water bath at 70° C. to 90° C. for 10 min to 30 min.

6. The preparation method according to claim 1, characterized in that: The rinsing treatment in step e) uses a BOE buffered oxide etchant with a volume ratio of 48 wt% to 50 wt% HF aqueous solution: 35 wt% to 45 wt% NH4F aqueous solution = 1: (6 to 8) to rinse the sample for 5s to 30s; The method of etching the top device silicon layer to form a conical needle tip structure with a height of 11.5μm to 13μm is a Cryo silicon process, and the etching conditions are: 92sccm SF6, 15-25sccm O2, 12mTorr, 600W ICP, 8W RF, -100℃.

7. The preparation method according to claim 1, characterized in that: The process of using photoresist to form a photoresist mask for hollowing out the composite beam structure on the surface of the top device silicon layer in step f) is specifically as follows: A photoresist with a thickness of 0.8μm to 1.5μm is spin-coated on the surface of the top device silicon layer and baked on a hot plate at 100℃ to 120℃ for 60s to 120s. A high-resolution exposure overlay is performed using a Heidelberg laser direct writing device in a gas-focused high depth of field mode with an exposure dose of 90mW to 120mW. The developer is used for development for 40s to 60s, and the film is hardened on a hot plate at 100℃ to 120℃ for 2min to 5min to form a photoresist mask that hollows out the composite beam structure.

8. The preparation method according to claim 1, characterized in that: The method of etching the top device silicon layer in step g) is the Bosch silicon process; the method of removing the photoresist is to use NMP solution in a water bath at 70° C. to 90° C. for 10 min to 30 min.

9. The preparation method according to claim 1, characterized in that: The silicon oxide layer is deposited in step h) by low pressure chemical vapor deposition, and the thickness of the silicon oxide layer is 300 nm to 1000 nm.

10. The preparation method according to claim 1, characterized in that: The process of using photoresist to protect the composite beam structure and the conical needle tip structure on the surface of the top device silicon layer in step i) is specifically as follows: Spin-coat a photoresist with a thickness of 10 μm to 20 μm on the surface of the top device silicon layer to protect the front composite beam structure and the conical needle tip structure, and bake on a hot plate at 85° C. to 95° C. for 10 min to 30 min; The process of using photoresist to cover the structure to be retained on the surface of the substrate silicon layer is specifically as follows: Spin-coat a photoresist with a thickness of 8 μm to 10 μm on the surface of the substrate silicon layer and bake it on a hot plate at 85°C to 95°C for 5 min to 10 min. Use a UV lithography machine to perform back-overlay exposure with an exposure dose of 700 mJ / cm 2 ~1000mJ / cm 2 , use developer to develop for 4min to 6min, and harden the film on a hot plate at 90℃ to 110℃ for 5min to 15min.

Citation Information

Patent Citations

  • Miniaturized cantilever probe for scanning probe microscopy and fabrication thereof

    CN104755942A

  • Self-filling three-arm type thermal scanning probe for micro-nano manufacturing

    CN111812357A

  • Method for manufacturing probe of scanning-type probe microscope (Spm) probe

    JP1999211735A

  • Method of manufacturing probe tip and probe for use in scanning probe microscope

    KR100766407B1