Semi-hard cord and its fabric and elastic product, and surface treatment agent
By using blocked aliphatic isocyanates or aqueous dispersions of isocyanates as surface treatment agents to regulate the specific stiffness of semi-hard cords, the environmental and health issues of organic solvents are solved, and the appropriate hardness and flexibility of the cords are achieved. , meeting a variety of application needs.
Patent Information
- Application Number
- CN202210884029.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-07-26
AI Technical Summary
In the existing technology, surface treatment agents using organic solvents are harmful to the environment and health, and cannot effectively regulate the hardness of semi-rigid cords, resulting in inability to meet the stiffness and softness requirements of certain applications.
Using a water dispersion of blocked aliphatic isocyanate or a water dispersion of blocked aliphatic isocyanate as a surface treatment agent, the rope is impregnated by controlling its mass concentration to regulate the specific stiffness of the semi-hard rope to ensure The processed wire rope is in the range of 4-12mgf/dtex to meet the needs of different applications.
The use of inorganic solvent-based surface treatment agents is realized, which avoids the environmental and health hazards of organic solvents. By regulating the hardness of the cord, the stiffness and softness requirements of semi-rigid cords in different applications are met.
Smart Images

Figure CN115287902B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of rubber reinforcing cords, and in particular relates to a semi-hard cord and its fabric, elastic product and surface treatment agent. Background Art
[0002] The rubber-based transmission belt used to transmit power, also known as a V-belt, is reinforced with continuous long fibers. For example, in patent US9927002B2, the cord is twisted with continuous long fibers. The reinforced cord needs to be surface treated with an adhesive to provide the necessary adhesion to the rubber matrix.
[0003] Rubber products, such as tires, belts, hoses, and air springs, are made of rubber and reinforcing fibers, cords, or fabrics such as tire cords or canvas. The rubber matrix must have good adhesion to the reinforcing fibers to ensure that there will be no failures such as cavitation and delamination during use.
[0004] Usually, cords are divided into soft cords and hard cords. Soft cords are mainly used for cloth-wrapped tapes where the finished tape is wrapped with a layer of rubber-coated fabric, while hard cords are mainly used for trimming tapes that do not require cloth wrapping. However, some cloth-wrapped tapes, such as power transmission belts for washing machines, require the cords to have a certain degree of stiffness to maintain the stiffness of the rubber belt, while at the same time requiring the cords to have enough softness to maintain a certain degree of elongation. Cords that meet this use requirement are called semi-hardened cords.
[0005] At present, the surface treatment agent used for semi-hardened cords is aromatic polyisocyanate dissolved in diphenylmethane diisocyanate, or polyaromatic isocyanate dissolved in organic solvent toluene. However, the use of organic solvents such as toluene is unsafe and easy to burn or explode. It is also harmful to the environment and health. Therefore, it is necessary to develop an inorganic solvent-based hardening treatment agent. Summary of the invention
[0006] The present application provides a surface treatment agent and a hard rope and an elastomeric product treated with the surface treatment agent, so as to solve the technical problem that the raw material of the rope surface treatment agent in the prior art is an organic solvent.
[0007] In a first aspect, the present application provides a semi-hard cord, which is treated with a surface treatment agent, and has a specific stiffness of ≤12 mgf / dtex; the components of the surface treatment agent include an aqueous dispersion of a blocked aliphatic isocyanate, and / or an aqueous dispersion of a blocked aliphatic isocyanate.
[0008] Optionally, the raw material of the blocked aliphatic isocyanate includes a trimer of hexamethylene diisocyanate; the raw material of the aqueous dispersion of the blocked aliphatic isocyanate also includes any one of butanone oxime, caprolactam and dimethylpyrazole.
[0009] Optionally, the components of the surface treatment agent include: a blocked aliphatic isocyanate aqueous dispersion, water and a synergist, and the synergist is any one of glycidyl ether and styrene-butadiene-vinyl pyridine copolymer emulsion.
[0010] Optionally, in the surface treatment agent, the mass fraction of blocked aliphatic isocyanate is 0.5-7%, and / or the mass fraction of aliphatic isocyanate in the surface treatment agent is 0.15%-1.5%.
[0011] In a second aspect, the present application provides a fabric, wherein the fabric is composed of the semi-hard cords described in the first aspect, and the specific stiffness of the semi-hard cords in the fabric is ≤12 mgf / dtex.
[0012] In a third aspect, the present application provides an elastomeric product, the components of which include the semi-hard cord described in the first aspect or the fabric described in the second aspect.
[0013] In a fourth aspect, the present application provides an application of a surface treatment agent in treating a cord, the application comprising: treating the cord with the surface treatment agent, wherein the specific stiffness of the cord after the treatment is ≤12 mgf / dtex; the components of the surface treatment agent include an aqueous dispersion of a blocked aliphatic isocyanate, and / or an aqueous dispersion of a blocked aliphatic isocyanate, and the components of the aqueous dispersion of the blocked aliphatic isocyanate include a blocked aliphatic isocyanate and water;
[0014] The raw material of the blocked aliphatic isocyanate includes a trimer of hexamethylene diisocyanate;
[0015] The raw material of the aqueous dispersion of the blocked aliphatic isocyanate further comprises any one of butanone oxime, caprolactam and dimethylpyrazole;
[0016] and / or,
[0017] The components of the surface treatment agent include: blocked aliphatic isocyanate water dispersion, water and synergist, and the synergist is any one of glycidyl ether and styrene-butadiene-vinyl pyridine copolymer emulsion.
[0018] In a fifth aspect, the present application provides a method for regulating the specific stiffness of a semi-hard cord, the method comprising the following steps:
[0019] Obtaining a surface treatment agent, wherein the components of the surface treatment agent include an aqueous dispersion of a blocked aliphatic isocyanate and / or an aqueous dispersion of a blocked aliphatic isocyanate, wherein the components of the aqueous dispersion of a blocked aliphatic isocyanate include a blocked aliphatic isocyanate and water;
[0020] Performing a glue dipping treatment on the cord with an impregnation liquid containing the surface treatment agent described in the fourth aspect;
[0021] The mass concentration of isocyanate and / or isocyanate in the impregnating solution is controlled to be a predetermined concentration so as to adjust the specific stiffness of the semi-hard cord.
[0022] Optionally, the mass fraction of isocyanate in the impregnation solution is 0.15%-1.5%.
[0023] Optionally, the mass fraction of isocyanate in the impregnation solution is 0.5%-7%.
[0024] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0025] The surface treatment agent provided in the embodiments of the present application treats the cord by using a self-emulsifying aqueous dispersion containing aliphatic isocyanate or an aqueous dispersion of blocked aliphatic isocyanate. The stiffness of the cord is equivalent to that of the cord treated with aromatic isocyanate dissolved in an organic solvent. This solves the technical prejudice in the prior art that cords treated with aqueous dispersions of blocked aliphatic isocyanate or aqueous dispersions containing aliphatic isocyanate are too soft and cannot reach the hardness of cords treated with aromatic isocyanate. This achieves the goal that fibers treated with blocked aliphatic isocyanate can reach the hardness of fibers treated with an organic solvent solution of aromatic polyisocyanate. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 A schematic diagram of a process for regulating the specific stiffness of a semi-hard cord provided in an embodiment of the present application;
[0029] Figure 2 A schematic diagram of a process of an impregnation treatment method provided in an embodiment of the present application;
[0030] Figure 3 This is a schematic diagram of the cross-sectional structure of a rubber product provided in an embodiment of the present application. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0032] According to a typical embodiment of the present invention, a semi-hard cord is provided, wherein the semi-hard cord is treated with a surface treatment agent, and the specific stiffness of the semi-hard cord is ≤12 mgf / dtex; the components of the surface treatment agent include an aqueous dispersion of a blocked aliphatic isocyanate, and / or an aqueous dispersion of a blocked aliphatic isocyanate.
[0033] Specifically, the components of the aqueous dispersion of blocked aliphatic isocyanate include blocked aliphatic isocyanate and water.
[0034] By using the aqueous dispersion of blocked aliphatic isocyanate as a surface treatment agent for treating cords or fabrics, when the specific stiffness of the treated semi-hard cord does not exceed 12 mgf / dtex, the properties of the treated semi-hard cord include: stiffness of 4-12 mgf / dtex and elongation ≥4% at a load of 200N, which better meets the application requirements.
[0035] In some embodiments, the raw material of the blocked aliphatic isocyanate includes a trimer of hexamethylene diisocyanate; the raw material of the aqueous dispersion of the blocked aliphatic isocyanate also includes any one of butanone oxime, caprolactam and dimethylpyrazole.
[0036] Hexamethylene diisocyanate reacts with either butanone oxime or dimethylpyrazole to obtain an aqueous dispersion of aliphatic isocyanate, which has self-emulsifying properties and can be used as a surface treatment agent to treat rubber cords.
[0037] The mechanism for selecting butanone oxime is that the oxime group of butanone oxime can react with isocyanate. After the reaction, the isocyanate is protected at room temperature, but it can dissociate and release isocyanate at about 150 degrees Celsius. The released isocyanate can react with the target substance.
[0038] The mechanism for selecting dimethylpyrazole is that the oxime group of butanone oxime can react with isocyanate. After the reaction, the isocyanate is protected at room temperature, but it can dissociate and release isocyanate at about 130 degrees Celsius. The released isocyanate can react with the target substance.
[0039] Specifically, the mass fraction of the blocked aliphatic isocyanate in the aqueous dispersion of the blocked aliphatic isocyanate can be 44%-46%; the mass fraction of the blocked aliphatic isocyanate in the aqueous dispersion of the blocked aliphatic isocyanate can be 37%-39%. The raw materials in the aqueous dispersion of the blocked aliphatic isocyanate include a trimer of hexamethylene diisocyanate (HDI), part of the isocyanate groups on the trimer react with hydrophilic groups such as low molecular weight polyoxyethylene ether to produce self-emulsification ability in water, and other isocyanate groups react with butanone oxime, and are emulsified and diluted with water to a non-volatile content of 44%-46%, preferably 45%; the isocyanate groups in the aqueous dispersion of the blocked aliphatic isocyanate react with dimethylpyrazole, and are emulsified and diluted with water to a non-volatile content of 37%-39%.
[0040] It should be noted that the blocking group in the blocked aliphatic isocyanate is at least one of dimethylpyrazole, caprolactam or butanone oxime. The liquid of the aqueous dispersion of the blocked aliphatic isocyanate contains an epoxy compound and a styrene-butadiene-vinylpyridine copolymer.
[0041] In some embodiments, the components of the surface treatment agent include: a blocked aliphatic isocyanate aqueous dispersion, water, and a synergist, wherein the synergist is any one of glycidyl ether and styrene-butadiene-vinyl pyridine copolymer emulsion.
[0042] Specifically, glycidyl ether is a water-soluble epoxy compound, and the EX313 model of Nagase Chemical Co., Ltd. can be used; the mass percentage of non-volatile components in the styrene-butadiene-vinylpyridine copolymer emulsion is 40%, and the content of vinylpyridine in the copolymer is 15%, and the model produced by Trinseo, abbreviated as Pyratex240, can be used.
[0043] It should be noted that the preparation method containing blocked aliphatic isocyanate, glycidyl ether and water can be: first weigh water, then add glycidyl ether, stir and disperse to dissolve, and then add the water dispersion of blocked aliphatic isocyanate and stir evenly.
[0044] In addition, the preparation method of the emulsion containing blocked aliphatic isocyanate, water and styrene-butadiene-vinyl pyridine copolymer can be: first weigh water, then add the aqueous dispersion of blocked aliphatic isocyanate, stir and disperse, and then add the emulsion of styrene-butadiene-vinyl pyridine copolymer and stir evenly.
[0045] The mechanism for selecting glycidyl ether is that this type of epoxy compound has an aqueous solution and can form a uniform solution in water, which is conducive to penetrating into the fiber to form a better cohesion within the fiber bundle.
[0046] The mechanism for selecting styrene-butadiene-vinyl pyridine copolymer emulsion is that it is a commonly used polymer binder for fiber surface treatment and can enhance the adhesion between the fiber and the matrix material such as rubber.
[0047] In some embodiments, the mass fraction of blocked aliphatic isocyanate in the surface treatment agent is 0.5-7%, and / or the mass fraction of aliphatic isocyanate in the surface treatment agent is 0.15%-1.5%.
[0048] The mechanism for controlling the mass fraction of blocked aliphatic isocyanate in the aqueous dispersion of blocked isocyanate to be no more than 7% is that too high a concentration of blocked isocyanate will result in too high hardness of the cord after impregnation.
[0049] In a second aspect, the present application provides a fabric comprising the semi-hard cords described in the first aspect, wherein the specific stiffness of the semi-hard cords in the fabric is ≤12 mgf / dtex.
[0050] In a third aspect, the present application provides an elastomeric product, the components of which include the semi-hard cord described in the first aspect or the fabric described in the second aspect.
[0051] In a fourth aspect, the present application provides an application of a surface treatment agent in treating a cord, the application comprising: treating the cord with the surface treatment agent, wherein the specific stiffness of the cord after the treatment is ≤12 mgf / dtex; the components of the surface treatment agent include an aqueous dispersion of a blocked aliphatic isocyanate, and / or an aqueous dispersion of a blocked aliphatic isocyanate, and the components of the aqueous dispersion of the blocked aliphatic isocyanate include a blocked aliphatic isocyanate and water;
[0052] The raw material of the blocked aliphatic isocyanate includes a trimer of hexamethylene diisocyanate;
[0053] The raw material of the aqueous dispersion of the blocked aliphatic isocyanate further comprises any one of butanone oxime, caprolactam and dimethylpyrazole;
[0054] and / or,
[0055] The components of the surface treatment agent include: blocked aliphatic isocyanate water dispersion, water and synergist, and the synergist is any one of glycidyl ether and styrene-butadiene-vinyl pyridine copolymer emulsion.
[0056] In a fifth aspect, the present application provides a method for regulating the specific stiffness of a semi-hard cord, such as Figure 1 As shown, the method comprises the following steps:
[0057] Obtaining a surface treatment agent, wherein the components of the surface treatment agent include an aqueous dispersion of a blocked aliphatic isocyanate and / or an aqueous dispersion of a blocked aliphatic isocyanate, wherein the components of the aqueous dispersion of a blocked aliphatic isocyanate include a blocked aliphatic isocyanate and water;
[0058] Performing a glue dipping treatment on the cord with an impregnation liquid containing the surface treatment agent;
[0059] The mass concentration of isocyanate and / or isocyanate in the impregnating solution is controlled to be a predetermined concentration so as to adjust the specific stiffness of the semi-hard cord.
[0060] In some embodiments, the mass fraction of isocyanate in the impregnation solution is 0.15%-1.5%, and / or the mass fraction of isocyanate in the impregnation solution is 0.5%-7%.
[0061] In some embodiments, the mass fraction of blocked aliphatic isocyanate in the surface treatment agent is ≤7%.
[0062] In some embodiments, the mass fraction of aliphatic isocyanate in the surface treatment agent is 0.15%-1.5%.
[0063] The mechanism for controlling the mass fraction of blocked aliphatic isocyanate in the aqueous dispersion of blocked isocyanate to be no more than 7% is that too high a concentration of blocked isocyanate will result in too high hardness of the cord after impregnation.
[0064] The mechanism of the mass fraction of aliphatic isocyanate in the surface treatment agent being 0.15%-1.5% is that too high aliphatic isocyanate concentration will lead to too high hardness of the cord after impregnation, while too low aliphatic isocyanate concentration will lead to too low hardness of the cord, and the treatment effect is not achieved, and the cord is still in the soft state of untreated. Generally, the material of the untreated cord includes but is not limited to: polyester, aromatic polyamide or polyamide.
[0065] According to a typical embodiment of the present invention, a method for regulating the specific stiffness of a semi-hard cord is provided, the method comprising the following steps:
[0066] Obtaining a surface treatment agent, wherein the components of the surface treatment agent include an aqueous dispersion of a blocked aliphatic isocyanate and / or an aqueous dispersion of a blocked aliphatic isocyanate, wherein the components of the aqueous dispersion of a blocked aliphatic isocyanate include a blocked aliphatic isocyanate and water;
[0067] The cord is dipped in glue using an impregnation liquid containing a surface treatment agent;
[0068] The mass concentration of isocyanate and / or isocyanate in the impregnating solution is controlled to be a predetermined concentration so as to adjust the specific stiffness of the semi-hard cord.
[0069] Specifically, the line can be two strands of 1100dtex polyethylene terephthalate continuous fibers twisted in the Z direction with a twist of 190 twists / m. Then three strands of the twisted fibers are twisted in the reverse S direction with a twist of 110 twists / m, and the resulting cord product can be expressed as PET1100dtex / 2x3. The chemical composition of the cord can be at least one of polyester, aromatic polyamide or polyamide. The initial soft cord with a certain strength, elasticity and elongation is treated by the method of the present application, and the treated semi-hard cord has a specific stiffness of ≤12mgf / dtex and an elongation of greater than 4% under a load of 200N.
[0070] By controlling the mass concentration of isocyanate in the impregnation solution, the isocyanate reacts with the fiber. Due to the mechanism that the isocyanate is unblocked and released at high temperature to react with the fiber, the purpose of regulating the specific stiffness of the semi-hard rope can be achieved.
[0071] In some embodiments, the mass fraction of isocyanate in the impregnation solution is 0.15%-1.5%, and / or the mass fraction of isocyanate in the impregnation solution is 0.5%-7%.
[0072] By controlling the mass fraction of isocyanate in the impregnation liquid to 0.15%-1.5% and / or by controlling the mass fraction of isocyanate in the impregnation liquid to 0.5%-7%, it has a positive effect of being able to react moderately with the fiber, so that the cord is not too soft or too hard.
[0073] According to a typical embodiment of the present invention, a semi-hard cord is provided. The semi-hard cord is treated with the surface treatment agent described in the first aspect, and the specific stiffness of the semi-hard cord is ≤12 mgf / dtex.
[0074] According to a typical embodiment of the present invention, a fabric is provided. The fabric is treated with the surface treatment agent described in the first aspect, and the specific stiffness of the semi-hard cords in the fabric is ≤12 mgf / dtex.
[0075] According to a typical embodiment of the present invention, an elastomeric product is provided, wherein the components of the elastomeric product include the semi-hard cord described in the third aspect or the fabric described in the fourth aspect.
[0076] Specifically, elastomeric articles include, but are not limited to, tires or rubbers such as belts, conveyor belts, transmission belts, drive belts, hoses, ribbons, transport belts, and bellows.
[0077] The method of the present invention will be described in detail below with reference to embodiments, comparative examples and experimental data.
[0078] The experimental reagents include: IL-6, an aqueous dispersion of caprolactam-blocked diphenylmethane diisocyanate, 50% non-volatile content, produced by EMS AG, Switzerland; WANNATE® PM200, polymeric diphenylmethane diisocyanate, denoted as pMDI, produced by Wanhua Chemical Company; toluene and water, preferably soft water.
[0079] Example 1
[0080] An embodiment of the present application provides a semi-hard cord, which is treated with a surface treatment agent, and has a specific stiffness of ≤12 mgf / dtex; a component of the surface treatment agent includes an aqueous dispersion of a blocked aliphatic isocyanate.
[0081] The components of the aqueous dispersion of blocked aliphatic isocyanate include blocked aliphatic isocyanate and water, and the isocyanate content in the aqueous dispersion of blocked aliphatic isocyanate is 4.3% by weight. The raw materials of the aqueous dispersion of blocked aliphatic isocyanate include a trimer of hexamethylene diisocyanate (HDI), and part of the isocyanate groups on the trimer react with hydrophilic groups such as low molecular weight polyoxyethylene ether to generate self-emulsification ability in water, wherein the isocyanate groups react with butanone oxime and are emulsified and diluted with water to a non-volatile content of 44%-46%.
[0082] The aqueous dispersion of blocked aliphatic isocyanate and water are mixed in a mass ratio of 2:98 to obtain an impregnation solution; the wire rope is impregnated with the impregnation solution containing a surface treatment agent, such as Figure 2 As shown; the mass concentration of isocyanate and / or isocyanate in the impregnation solution is controlled to be a predetermined concentration to achieve the regulation of the stiffness of the semi-hard cord; the cross section of the obtained cord product is as shown Figure 3 shown.
[0083] Example 2
[0084] The difference between the embodiment of the present application and embodiment 1 is that the aqueous dispersion of blocked isocyanate and water are mixed in a mass ratio of 5:95 to obtain an impregnation solution.
[0085] Example 3
[0086] The difference between the embodiment of the present application and embodiment 1 is that the aqueous dispersion of blocked isocyanate and water are mixed in a mass ratio of 15:85 to obtain an impregnation solution.
[0087] Example 4
[0088] The difference between the embodiment of the present application and embodiment 1 is that the water dispersion of blocked isocyanate, glycidyl ether and soft water are mixed in a mass ratio of 5:2:93 to obtain an impregnation solution.
[0089] Example 5
[0090] The embodiment of the present application is different from embodiment 1 in that the water dispersion of blocked isocyanate, styrene-butadiene-vinyl pyridine copolymer emulsion and soft water are mixed in a mass ratio of 6:40:54 to obtain an impregnation solution.
[0091] Example 6
[0092] The embodiment of the present application is different from Embodiment 1 in that the aqueous dispersion of blocked isocyanate, styrene-butadiene-vinyl pyridine copolymer emulsion and soft water are mixed in a mass ratio of 15:40:45 to obtain an impregnation solution.
[0093] Example 7
[0094] The embodiment of the present application provides a semi-hard cord, which is treated with a surface treatment agent, and the specific stiffness of the semi-hard cord is ≤12 mgf / dtex; the component of the surface treatment agent includes an aqueous dispersion of a blocked aliphatic isocyanate. The components of the aqueous dispersion of the blocked isocyanate include a blocked isocyanate and soft water, and the isocyanate content in the aqueous dispersion of the blocked isocyanate is 4.3% by weight; the raw material of the aqueous dispersion of the blocked aliphatic isocyanate includes a trimer of hexamethylene diisocyanate (HDI), and some of the isocyanate groups on the trimer react with hydrophilic groups such as low molecular weight polyoxyethylene ether to produce self-emulsification ability in water, and the remaining isocyanate groups react with dimethylpyrazole, and are emulsified and diluted with water to a non-volatile content of 37%-39%.
[0095] Comparative Example 1
[0096] The comparative example of the present application provides an impregnation liquid, the chemical composition of which is 3% pMDI / toluene; pMDI toluene solution: 47.5 grams of toluene are weighed, and then 2.5 grams of pMDI is added to toluene and fully dissolved. It is expressed as 5% pMDI / toluene, and 5% pMDI / toluene is diluted with toluene to 3% pMDI / toluene.
[0097] Comparative Example 2
[0098] The comparative example of the present application provides an impregnation liquid, the chemical composition of which is an aqueous dispersion of caprolactam-blocked diphenylmethane diisocyanate (IL-6) and water, and the mass ratio thereof is 2:98.
[0099] Comparative Example 3
[0100] The comparative example of the present application provides an impregnation liquid, the chemical composition of which is an aqueous dispersion of diphenylmethane diisocyanate blocked with caprolactam (IL-6) and water, and the mass ratio thereof is 6:94.
[0101] Comparative Example 4
[0102] The comparative example of the present application provides an impregnation liquid, the chemical composition of which is an aqueous dispersion of caprolactam-blocked diphenylmethane diisocyanate (IL-6) and water, and the mass ratio thereof is 15:85.
[0103] Comparative Example 5
[0104] The comparative example of the present application provides an impregnation liquid, the chemical components of which are an aqueous dispersion of caprolactam-blocked diphenylmethane diisocyanate (IL-6), water and a styrene-butadiene-vinylpyridine copolymer emulsion (Pyratex 240), with a mass ratio of 6:40:54.
[0105] Comparative Example 6
[0106] The comparative example of the present application provides an impregnation liquid, the chemical components of which are an aqueous dispersion of caprolactam-blocked diphenylmethane diisocyanate (IL-6), water and a styrene-butadiene-vinylpyridine copolymer emulsion (Pyratex 240), with a mass ratio of 15:40:45.
[0107] Comparative Example 7
[0108] The comparative example of the present application provides an impregnation liquid, the chemical components of which are an aqueous dispersion of caprolactam-blocked diphenylmethane diisocyanate (IL-6), water and glycidyl ether, and the mass ratio thereof is 6:2:92.
[0109] The components of the surface treatment agent of the embodiment and the comparative example are shown in Table 1 and Table 2. The prepared surface treatment agent is configured into an impregnation liquid. The components of the impregnation liquid include blocked aliphatic isocyanate and water, and may further contain glycidyl ether and / or styrene-butadiene-vinyl pyridine polymer. The impregnation liquid is used for dipping. The method includes dipping PET1100 / 2x3 cord in the adhesive treatment liquid on a single cord dipping machine (manufactured by Lizler Square Electric), and then drying at 160 degrees Celsius for 1 minute, and then drying at 247 degrees Celsius for 1 minute before winding up.
[0110] The cords after dipping are tested to test the hardness, or stiffness, of the cords in accordance with GB / T 33099-2016. The results are expressed in grams-force (gf). The results are converted into milligrams-force (mgf) and then divided by the total fineness of the tested cord expressed in decitex (dtex) to obtain the specific stiffness mgf / dtex. Practical experience has shown that when the specific stiffness of the treated cord does not exceed 12 mgf / dtex, the stiffness and flexibility of the cord meet the process and application requirements better. Usually, when the cords with better specific stiffness are used in rubber products, the cuts of the rubber samples are neater. For semi-hard cords, both hardness and flexibility should be paid attention to, so as to comprehensively control their specific stiffness to meet the hardness and flexibility requirements; conventionally, the specific stiffness of semi-hard cords is not higher than 12 mgf / dtex, and more preferably 4-10 mgf / dtex.
[0111] In addition, the wire rope is also subjected to tensile testing according to GB / T 32108-2015, and the elongation at break and the elongation at a fixed load of 200 Newtons (N) are obtained according to this standard test. The elongation at break reflects the extent to which the wire rope can be stretched when it is stretched to break, and the elongation at a fixed load of 200N reflects the extent to which the wire rope can be elongated under this load. These two performance indicators reflect the elasticity of the wire rope. The higher these two values are, the better the elasticity of the wire rope is.
[0112] The test results are shown in Table 1 and Table 2.
[0113] Table 1 shows the test results of the comparative example.
[0114] project Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Isocyanate content in the impregnation solution (mass fraction) 5% 1% 3% 7.5% 3% 7.5% 3% Isocyanate content in the impregnation solution (mass fraction) 1.55% 0.09% 0.26% 0.66% 0.26% 0.66% 0.26% Stiffness (gf) (GB / T 33099-2016) 32.9 20.2 32.3 56.8 28.3 50.2 35.8 Specific stiffness (mgf / dtex) 5.0 3.0 4.9 8.6 4.3 7.6 5.4 200N fixed load elongation 3.74% 3.91% 4.56% 4.25% 4.67% 4.51% 4.71% Elongation at break 8.82% 9.21% 9.01% 8.93% 9.21% 9.07% 9.69%
[0115] Table 2 is the test results of the embodiment.
[0116] project Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Isocyanate content in the impregnation solution (mass fraction) 0.9% 2.25% 6.75% 2.25% 2.7% 6.75% 5.7% Isocyanate content in the impregnation solution (mass fraction) 0.19% 0.47% 1.42% 0.47% 0.56% 1.42% 1.29% Stiffness (gf) (GB / T 33099-2016 28.3 35.7 68.7 39.3 36.1 58.7 59.3 Specific stiffness (mgf / dtex) 4.3 5.4 10.4 5.9 5.5 8.9 9.0 200N fixed load elongation 4.61% 4.58% 4.65% 5.21% 4.47% 4.74% 4.69% Elongation at break 11.30% 11.10% 9.85% 11.35% 11.31% 11.02% 10.98%
[0117] As can be seen from the table, the fiber treated with internally emulsified aqueous blocked aliphatic isocyanate can achieve the hardness of the fiber treated with an organic solvent solution of aromatic polyisocyanate (Comparative Example 1 and all Examples). In addition, the comparison between the internally emulsified blocked aliphatic isocyanate and the aqueous dispersion of blocked aromatic isocyanate shows that aliphatic compounds are generally softer than aromatics, but it can be seen from the results that to achieve the same semi-hard cord stiffness after treatment, the amount of the internally emulsified aliphatic isocyanate used is lower than the amount of the aqueous dispersion of blocked aromatic isocyanate (Comparative Example 2 and Example 1, Comparative Example 3 and Example 2, Comparative Example 4 and Example 3, Comparative Example 7 and Example 4, Comparative Example 5 and Example 5, Comparative Example 6 and Example 6).
[0118] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0119] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for regulating the specific stiffness of a semi-rigid cord, It is characterized in that The method comprises the following steps: Obtaining a surface treatment agent, wherein the component of the surface treatment agent is a water dispersion of a blocked aliphatic isocyanate; The cord is subjected to a dipping treatment using an impregnation solution obtained by mixing a surface treatment agent with water, wherein the components of the aqueous dispersion of the blocked aliphatic isocyanate include blocked aliphatic isocyanate and water; The raw material of the blocked aliphatic isocyanate includes a trimer of hexamethylene diisocyanate; The raw materials of the aqueous dispersion of the blocked aliphatic isocyanate also include butanone oxime; The mass concentrations of isocyanate and isocyanate in the impregnation liquid are controlled to be predetermined concentrations to achieve regulation of the specific stiffness of the semi-hard cord; the mass fraction of isocyanate in the impregnation liquid is 1.29%; the mass fraction of isocyanate in the impregnation liquid is 5.7%; the specific stiffness of the semi-hard cord is ≤12 mgf / dtex.
2. A semi-rigid rope, It is characterized in that Prepared by the method according to claim 1.
3. A fabric, It is characterized in that The fabric is composed of the semi-hard cords according to claim 2, and the specific stiffness of the semi-hard cords in the fabric is ≤12 mgf / dtex.
4. An elastomeric product, It is characterized in that The components of the elastomeric article include the semi-rigid cord of claim 2 or the fabric of claim 3.
Citation Information
Patent Citations
Friction transmission belt
US9927002B2
Environment-friendly fiber framework material dip solution and dipping process
CN106084362A
Environment-friendly fiber framework material impregnation liquid, preparation method thereof and application of liquid
CN109082893A
Adhesive composition for organic fiber, method for treating organic fiber, organic fiber, and tire
CN110317560A
Aramid fiber hard cord impregnation pretreatment liquid and aramid fiber hard cord impregnation method
CN112878046A