A production method for improving the cross-sectional shape of hot-rolled strip steel
By optimizing the temperature, reduction rate and roll gap deviation adjustment in the production of low carbon steel hot-rolled strips, the problems of poor cross-section shape control and poor crown wedge adjustment ability are solved, and the incidence of ridges in cold-rolled products is significantly reduced. , achieving simplification of the production process and cost reduction.
Patent Information
- Application Number
- CN202211047732.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-30
AI Technical Summary
In the production process of low carbon steel hot-rolled strips, there are problems such as poor cross-section shape control and poor crown and wedge adjustment capabilities. This results in severe convex edges of the cold-rolled product, which cannot meet customer requirements, and the existing technical solutions are complex. And the investment is high and difficult to promote.
By optimizing the temperature control, reduction rate and roll gap deviation adjustment during the rolling process, the rough rolling outlet temperature is controlled at 1050~1080°C, the finishing rolling inlet temperature is controlled at 1040~1070°C, and the rough rolling passes are 4 to 6 passes. Secondary reduction rate control, the reduction rate of the first two stands of finishing rolling is controlled at 47% to 53%, and the roll gap deviation of the rolling mill is distributed from large to small proportions to improve the cross-sectional shape of the hot-rolled strip.
It effectively improves the cross-sectional shape of hot-rolled strip steel and reduces the incidence of ridges in cold-rolled products. The implementation is relatively simple, low-cost, and has significant effects.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of strip steel production, and in particular to a production method for improving the cross-sectional shape of hot-rolled strip steel. Background Art
[0002] Low-carbon or ultra-low-carbon steel with a C content of ≤0.02% is relatively soft and has high requirements for plate shape quality. However, during the production process, the following problems are prone to occur in terms of plate shape: (1) The cross-sectional shape of the hot-rolled strip is poorly controlled, mainly due to the presence of local high points at the edge of the strip; (2) The ability to ensure convexity and wedge shape is poor, which is often manifested as the convexity control being too small and the wedge shape control being too large, that is, the wedge shape value is greater than the convexity value.
[0003] Hot rolled steel coils with the above problems have serious edge ridge problems after cold rolling and galvanizing. The edge is seriously wavy after uncoiling and cannot meet the use requirements of customers. The thinner the thickness of the cold rolled product, the higher the ridge occurrence rate, which seriously affects the delivery time and yield rate of the product.
[0004] The Chinese invention patent with the authorization announcement number CN 112122359 B discloses "a control method for dynamically improving the shape of strip steel", which belongs to the field of hot rolling line shape control technology. According to the cross-sectional thickness of the strip steel measured by the convexity meter, the thickness of two positions on both sides of the strip steel is obtained, and the thickness difference is used as the edge drop of the strip steel; according to the measured strip steel convexity and the calculated strip steel edge drop, the measured strip steel convexity is optimized and used as the actual strip steel convexity. The optimized actual strip steel convexity is defined as the actual convexity of the instrument-strip steel edge drop*edge drop adjustment coefficient. The purpose of this technical solution is to overcome the defect that the convexity detected by the instrument is larger than the actual convexity, which causes the actual convexity of the strip steel to become smaller in the convexity control. By optimizing the actual detected convexity of the strip steel, the hot rolling finishing plate shape model can more accurately calculate the position of the roller shifting and the predicted value of the bending roll force of each finishing stand, thereby improving the convexity and end face control accuracy of the strip steel.
[0005] The Chinese patent application with application publication number CN 102145348 A discloses a "plate shape control technology in ultra-wide thin plate hot continuous rolling production", and its core technologies mainly include: AVC roll application, AVC roll curve design, plate shape control strategy formulation and implementation, rolling mill accuracy, accurate prediction calculation of roll wear and thermal expansion, optimization and improvement of model control system, etc. The first four rolling mills of the ultra-wide thin plate hot continuous rolling finishing mill adopt AVC roll shape, and the last three rolling mills adopt conventional roll shape, and the axial movement system of the working rolls and the model control function are optimized, so that the first three rolling mills can form a good proportional convexity to maintain the plate shape, and at the same time, the proportional convexity of the rear rolling mills can be changed very little or not, which can ensure that the flatness index of the finished rolling export strip is good.
[0006] The above technical solution is relatively complex, difficult to implement and has high investment costs, and is difficult to promote in existing steel rolling mills. Summary of the invention
[0007] The present invention provides a production method for improving the cross-sectional shape of hot-rolled steel strip. By optimizing the production process parameters, the cross-sectional shape of the hot-rolled steel strip is effectively improved, and the incidence of ridges in cold-rolled products is reduced. Combined with the actual situation on site, the method is easy to implement, has low investment cost, and has significant effect.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] A production method for improving the cross-sectional shape of a hot-rolled steel strip, comprising:
[0010] 1) Strip crown control:
[0011] (1) Temperature control during rolling: the rough rolling outlet temperature is controlled at 1050-1080°C; the finishing rolling inlet temperature is controlled at 1040-1070°C;
[0012] (2) Rough rolling reduction rate control: Rough rolling is performed in 4 to 6 passes, with a reduction rate of 20% to 28% for each pass;
[0013] (3) Finishing rolling reduction rate control: The reduction rate of at least the first two stands of finishing rolling is 47% to 53%, and the bending roll force of the corresponding stand is controlled at 55 to 75 tons;
[0014] (4) Strip convexity control index: The convexity of hot-rolled strip is controlled at 45-65 μm;
[0015] 2) Wedge control:
[0016] The wedge value is adjusted by the roll gap deviation of the rolling mill; the side bending of rough rolling is controlled within the range of ±30mm; the roll gap deviation adjustment amount of the first three stands of finishing rolling is distributed in proportion from large to small, among which the adjustment amount of the first stand accounts for 40% to 50% of the total adjustment amount, the adjustment amount of the second stand accounts for 35% to 45% of the total adjustment amount, and the adjustment amount of the third stand accounts for 5% to 15% of the total adjustment amount.
[0017] Furthermore, the strip steel is low carbon steel or ultra-low carbon steel with a carbon content of ≤0.02%.
[0018] Furthermore, the thickness of the finished strip steel is 2.5 to 3.5 mm.
[0019] Furthermore, the thickness of the rough-rolled intermediate billet is 44 to 48 mm.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1) By controlling the rough rolling reduction rate and the finishing rolling reduction rate, as well as the reasonable setting of the finishing rolling bending roll force, the cross-sectional shape of the hot-rolled strip is effectively improved, and the local high points on the edge of the strip are eliminated.
[0022] 2) By controlling the rough rolling outlet temperature and the finishing rolling inlet temperature and adjusting the roller gap deviation of the finishing mill, the adjustment and control capabilities of the convexity and wedge shape of the hot-rolled strip are improved.
[0023] 3) By optimizing the process parameters of the production process, the cross-sectional shape of the hot-rolled strip is effectively improved, and the incidence of ridges in cold-rolled products is reduced; combined with the actual situation on site, it is easy to implement, has low investment costs, and has significant effects. DETAILED DESCRIPTION
[0024] The present invention provides a production method for improving the cross-sectional shape of a hot-rolled steel strip, comprising:
[0025] 1) Strip crown control:
[0026] (1) Temperature control during rolling: the rough rolling outlet temperature is controlled at 1050-1080°C; the finishing rolling inlet temperature is controlled at 1040-1070°C;
[0027] (2) Rough rolling reduction rate control: Rough rolling is performed in 4 to 6 passes, with a reduction rate of 20% to 28% for each pass;
[0028] (3) Finishing rolling reduction rate control: The reduction rate of at least the first two stands of finishing rolling is 47% to 53%, and the bending roll force of the corresponding stand is controlled at 55 to 75 tons;
[0029] (4) Strip shape control index: The convexity of hot-rolled strip is controlled at 45-65 μm;
[0030] 2) Wedge control:
[0031] The wedge value is adjusted by the roll gap deviation of the rolling mill; the side bending of rough rolling is controlled within the range of ±30mm; the roll gap deviation adjustment amount of the first three stands of finishing rolling is distributed in proportion from large to small, among which the adjustment amount of the first stand accounts for 40% to 50% of the total adjustment amount, the adjustment amount of the second stand accounts for 35% to 45% of the total adjustment amount, and the adjustment amount of the third stand accounts for 5% to 15% of the total adjustment amount.
[0032] Furthermore, the strip steel is low carbon steel or ultra-low carbon steel with a carbon content of ≤0.02%.
[0033] Furthermore, the thickness of the finished strip steel is 2.5 to 3.5 mm.
[0034] Furthermore, the thickness of the rough-rolled intermediate billet is 44 to 48 mm.
[0035] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.
[0036] [Example]
[0037] In this embodiment, the rolling material is IF steel, and the size specification is 3.0mm×1200mm hot-rolled strip steel; the specific control process is as follows:
[0038] 1. Strip crown control:
[0039] 1) Temperature control during rolling: The rough rolling outlet temperature is controlled at 1060±5℃, and the finishing rolling inlet temperature is controlled at 1050±5℃.
[0040] 1) Rough rolling reduction rate control: The rough rolling adopts the "1+3" rolling mode. The R1 rolling mill and the R2 rolling mill roll a total of 4 passes. The reduction rates of the 4 passes are 23%, 28%, 26% and 28% respectively. The thickness of the rough rolling intermediate billet is 46mm.
[0041] 3) Finishing rolling reduction rate control: The reduction rates of the first two stands of finishing rolling are 49.5% and 49%, and the bending roll forces of the corresponding stands are both 65t.
[0042] 4) Strip convexity control index: The convexity of hot-rolled strip is controlled at 55±5μm.
[0043] 2. Strip wedge control
[0044] The wedge value is adjusted through the roll gap deviation of the rolling mill, with the roll gap deviation adjustment of the first three stands of finishing rolling as the main focus. The roll gap deviation adjustment of the first three stands is distributed according to the principle of 4.5:4:1.5; the roll gap deviation adjustment of roughing rolling is mainly to cooperate with the adjustment of side bending, and the roughing side bending is controlled within the range of ±30mm.
[0045] [Example 2]
[0046] In this embodiment, the rolling material is st14, and the size specification is 2.75mm×1230mm hot-rolled strip steel; the specific control process is as follows:
[0047] 1. Strip crown control
[0048] 1) Temperature control during rolling: The rough rolling outlet temperature is controlled at 1055±5℃, and the finishing rolling inlet temperature is controlled at 1045±5℃.
[0049] 2) Rough rolling reduction rate control: The rough rolling adopts the "3+3" rolling mode. The R1 rolling mill and the R2 rolling mill roll a total of 6 passes. The reduction rates of the 4 passes are 20%, 21%, 21%, 22%, 23%, and 28% respectively. The thickness of the rough rolling intermediate billet is 44mm.
[0050] 3) Finishing rolling reduction rate control: The reduction rates of the first two stands of finishing rolling are 51% and 48%, and the bending roll forces of the corresponding stands are 55t and 60t respectively.
[0051] 4) Strip convexity control index: The convexity of hot-rolled strip is controlled at 53±5μm.
[0052] 2. Strip wedge control
[0053] The wedge value is adjusted through the roll gap deviation of the rolling mill, with the roll gap deviation adjustment of the first three stands of finishing rolling as the main focus. The roll gap deviation adjustment of the first three stands is distributed according to the principle of 5:4.5:0.5; the roll gap deviation adjustment of roughing rolling is mainly to cooperate with the adjustment of side bending, and the roughing side bending is controlled within the range of ±30mm.
[0054] [Example 3]
[0055] In this embodiment, the rolling material is SAE1001, and the size specification is 4.5mm×1150mm hot-rolled strip steel; the specific control process is as follows:
[0056] In this embodiment, the rolling material is SAE1001, and the size specification is 4.5mm×1150mm hot-rolled strip steel; the specific control process is as follows:
[0057] 1. Strip crown control
[0058] 1) Temperature control during rolling: The rough rolling outlet temperature is controlled at 1055±5℃, and the finishing rolling inlet temperature is controlled at 1050±5℃.
[0059] 2) Rough rolling reduction rate control: The rough rolling adopts the "1+3" rolling mode. The R1 rolling mill and the R2 rolling mill roll a total of 4 passes. The reduction rates of the 4 passes are 22%, 26%, 25% and 26% respectively. The thickness of the rough rolling intermediate billet is 48mm.
[0060] 3) Finishing rolling reduction rate control: The reduction rates of the first two stands of finishing rolling are 47% and 47%, and the corresponding bending roll forces of the stands are 50t and 55t respectively.
[0061] 4) Strip convexity control index: The convexity of hot-rolled strip is controlled at 58±5μm.
[0062] 2. Strip wedge control
[0063] The wedge value is adjusted through the roll gap deviation of the rolling mill, with the roll gap deviation adjustment of the first three stands of finishing rolling as the main focus. The roll gap deviation adjustment of the first three stands is distributed according to the principle of 4:3.5:2.5; the roll gap deviation adjustment of roughing rolling is mainly to cooperate with the adjustment of side bending, and the roughing side bending is controlled within the range of ±30mm.
[0064] The hot-rolled steel strip products produced in Examples 1-3 have good cross-sectional shapes, and the ridge incidence rate of the subsequent cold-rolled products is reduced from about 35% to about 1%.
[0065] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A production method for improving the cross-sectional shape of hot-rolled steel strip, characterized in that: include: 1) Strip crown control: (1) Temperature control during rolling: the rough rolling outlet temperature is controlled at 1050-1080°C; the finishing rolling inlet temperature is controlled at 1040-1070°C; (2) Rough rolling reduction rate control: Rough rolling is performed in 4 to 6 passes, with a reduction rate of 20% to 28% for each pass; (3) Finishing rolling reduction rate control: The reduction rate of at least the first two stands of finishing rolling is 47% to 53%, and the bending roll force of the corresponding stand is controlled at 55 to 75 tons; (4) Strip convexity control index: The strip convexity is controlled at 45-65 μm; 2) Wedge control: The wedge value is adjusted by the roll gap deviation of the rolling mill; the side bending of rough rolling is controlled within the range of ±30mm; the roll gap deviation adjustment amount of the first three stands of finishing rolling is distributed in proportion from large to small, among which the adjustment amount of the first stand accounts for 40% to 50% of the total adjustment amount, the adjustment amount of the second stand accounts for 35% to 45% of the total adjustment amount, and the adjustment amount of the third stand accounts for 5% to 15% of the total adjustment amount.
2. A production method for improving the cross-sectional shape of hot-rolled steel strip according to claim 1, characterized in that: The strip steel is low carbon steel or ultra low carbon steel with a carbon content of ≤0.02%.
3. A production method for improving the cross-sectional shape of hot-rolled steel strip according to claim 1, characterized in that: The thickness of the finished strip steel is 2.5 to 3.5 mm.
4. A production method for improving the cross-sectional shape of hot-rolled steel strip according to claim 1, characterized in that: The thickness of the rough rolling intermediate billet is 44 to 48 mm.
Citation Information
Patent Citations
Sheet shape control technology used in hot strip rolling of super-wide sheets
CN102145348A
A method for controlling the shape of dynamically lifted steel strip
CN112122359B
Method for improving rolling stability of container thin material
CN101927263A
Automatic control method for camber and wedge shape of rough rolling intermediate blank of hot rolling strip steel
CN102441576A
Rolling method for preventing hot-rolled strip steel with thickness of 4mm or less from deviating