A method for preparing ceramic-insulated aluminum winding based on arc-surface oxidation grooves
Through the arc surface oxidation tank technology, the aluminum conductor is generated in the oxidation tank and wrapped around the insulating cylinder, which solves the problem of falling off caused by high curvature bending in the winding preparation, and realizes the ceramic Stable forming of insulated aluminum windings and simplification of production processes.
Patent Information
- Application Number
- CN202210970948.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-08-14
AI Technical Summary
Ceramic insulated aluminum conductors are prone to fall off due to large curvature bending during the preparation of traditional windings, and the prior art is difficult to effectively solve this problem.
The aluminum wire is concave into an arc-shaped oxidation tank by using arc-surface oxidation tank. The aluminum wire is used to form ceramic insulated aluminum wires in the oxidation tank through the introduction wheel and the lead-out wheel, and is directly wound on the rotating insulating cylinder to reduce bending. Amplitude, realizes a single-forming ceramic insulated aluminum winding.
The production process of windings is simplified, the production difficulty and cost of ceramic insulated aluminum windings is reduced, the large bending of ceramic insulated aluminum wires is avoided, and the stability of the product is improved.
Smart Images

Figure CN115312322B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a ceramic insulated aluminum winding, and in particular to a method for preparing a ceramic insulated aluminum winding based on an oxidation groove with a circular arc surface. Background Art
[0002] In the conventional winding preparation process, the wire manufacturer produces insulated wires, and then the transformer manufacturer uses the insulated wires to produce windings and assemble them into transformers. From a roll of wire to a finished winding, it needs to go through multiple links such as unwinding-insulation treatment-rewinding-transportation to the transformer manufacturer-rewinding-winding. Aluminum wire with a ceramic insulating film layer is a new type of insulating wire, but the insulating film layer on the surface of this ceramic insulated aluminum wire is relatively fragile and cannot withstand large curvature bending. When using this ceramic insulated aluminum wire to prepare windings using traditional methods, the winding, unwinding and winding processes can easily cause the ceramic film layer on the surface of the ceramic insulated aluminum wire to fall off and become scrapped. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a ceramic insulated aluminum winding based on an oxidation groove with a circular arc surface, so that the aluminum wire is formed into a winding in one step after unwinding, insulating and winding without significantly bending the ceramic insulated aluminum wire, so as to overcome the defects of the prior art.
[0004] To achieve the above-mentioned purpose, the technical solution of the present invention is as follows:
[0005] A method for preparing a ceramic-insulated aluminum winding based on an oxidation groove with a circular arc surface, comprising the steps of:
[0006] (1) An inlet wheel and an outlet wheel are arranged at both ends of the arc surface of the oxidation tank with an arc surface, and a wire inlet hole, a wire outlet hole, a water inlet hole and a water outlet hole are respectively opened on the side wall of the oxidation tank connected to the two ends of the arc surface, and the side surfaces of the oxidation tank on both sides of the arc surface are surrounded by electrode plates;
[0007] (2) introducing the aluminum wire from the wire entry hole into the oxidation tank through the introduction wheel, and then leading the aluminum wire out of the wire exit hole through the lead-out wheel; adjusting the length of the aluminum wire between the introduction wheel and the lead-out wheel so that the aluminum wire in the oxidation tank is concave into an arc coaxial with the arc surface; fixing the insulating cylinder on the winding mechanism so that the arc surface surrounds the insulating cylinder;
[0008] (3) The oxidation tank is connected to the electrolyte circulation system through the water inlet, outlet and pipeline, the electrolyte is injected into the oxidation tank through the electrolyte circulation system, and the electrolyte in the oxidation tank is circulated through the external electrolyte circulation system to remove the gas and excess heat generated by the oxidation reaction of the aluminum wire. The electrode plate and the aluminum wire are respectively connected to the micro-arc oxidation / thermal electrochemical oxidation power supply, and the introduction wheel and the outlet wheel are rotated synchronously to make the aluminum wire pass through the oxidation tank continuously and unread in a fixed arc shape. When the aluminum wire passes through the oxidation tank, a curved ceramic insulated aluminum wire is generated, and the curved ceramic insulated aluminum wire is directly wound on the rotating insulation cylinder. After unwinding, insulation treatment and winding, the aluminum wire can be formed into a ceramic insulated aluminum winding at one time.
[0009] Furthermore, step (4) includes: controlling the rotation speed of the insulating drum by adjusting the winding mechanism so that the ceramic insulated aluminum wire between the insulating drum and the wire outlet hole is kept in an arc shape, and the ceramic insulated aluminum wire between the insulating drum and the wire outlet hole and the aluminum wire in the oxidation tank are located on the same circular ring.
[0010] Furthermore, the step (4) comprises:
[0011] The rotation speed of the insulating cylinder is controlled by adjusting the winding mechanism so that the ceramic insulated aluminum conductor between the insulating cylinder and the outlet hole is kept in an arc shape, and the ceramic insulated aluminum conductor between the insulating cylinder and the outlet hole and the aluminum conductor in the oxidation tank are located on the same circular ring; and the relative position of the insulating cylinder and the oxidation tank is adjusted so that the ceramic insulated aluminum conductor is tangent to the outer periphery of the insulating cylinder.
[0012] Furthermore, the step (4) comprises:
[0013] The rotation speed of the insulating drum is controlled by adjusting the winding mechanism, so that the ceramic insulated aluminum wire between the insulating drum and the outlet hole is kept in an arc shape, and the ceramic insulated aluminum wire between the insulating drum and the outlet hole and the aluminum wire in the oxidation tank are located on the same circular ring; and the relative position of the insulating drum and the oxidation tank is adjusted so that the ceramic insulated aluminum wire is tangent to the outer circumference of the insulating drum, and an elastic pressure roller is arranged at the tangent point of the ceramic insulated aluminum wire to the outer circumference of the insulating drum, and the ceramic insulated aluminum wire is wound tightly against the outer circumference of the insulating drum through the elastic pressure roller.
[0014] Furthermore,
[0015] The step (1) comprises:
[0016] Two pairs of introduction wheels and a pair of outlet wheels are arranged at both ends of the arc surface of the oxidation tank with an arc surface, and a wire inlet hole, a wire outlet hole, a water inlet hole and a water outlet hole are respectively opened on the side wall of the oxidation tank connected to the two ends of the arc surface, and the side surfaces of the oxidation tank on both sides of the arc surface are surrounded by electrode plates; the rotating shafts of the two pairs of introduction wheels are cross-shaped;
[0017] The step (2) comprises:
[0018] The aluminum wire is introduced into the oxidation tank from the wire entry hole in a straight line through two pairs of introduction wheels, and then led out of the wire exit hole through the lead-out wheel; the length of the aluminum wire between the introduction wheel and the lead-out wheel is adjusted so that the aluminum wire in the oxidation tank is concave into an arc coaxial with the arc surface; the insulating cylinder is fixed on the winding mechanism so that the arc surface surrounds the insulating cylinder.
[0019] Compared with the prior art, the beneficial technical effects of the present invention are:
[0020] The method of the present invention uses an oxidation groove with a circular arc surface to concave the aluminum wire into a circular arc for oxidation treatment. After the aluminum wire passes through the oxidation groove, it is naturally formed into a ring-shaped ceramic insulated aluminum wire. The ceramic insulated aluminum wire is directly wound on an insulating cylinder to form a ceramic insulated aluminum winding; the circular arc surface can make the oxidation groove arranged around the winding structure or the insulating cylinder of the winding, thereby minimizing the bending amplitude of the ceramic insulated aluminum wire during the production and winding process.
[0021] The method of the present invention can simplify the existing process of unwinding - insulation treatment - rewinding - transportation to the transformer manufacturer - rewinding - winding into unwinding - insulation treatment - winding, and can avoid large bending of the ceramic insulated aluminum wire, which can greatly reduce the production difficulty and cost of the ceramic insulated aluminum winding. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic structural diagram of an oxidation tank with a circular arc surface according to the present invention;
[0023] Figure 2 It is a schematic diagram of the structure of the equipment used in the method of the present invention. DETAILED DESCRIPTION
[0024] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Embodiment 1:
[0026] like Figure 1As shown, an oxidation tank with an arc surface, the oxidation tank 1 contains electrolyte, one side of the oxidation tank 1 is an arc surface 101, and the side walls of the oxidation tank connected to the two ends of the arc surface 101 are respectively provided with a wire entry hole 102, a wire exit hole 103, a water inlet hole 104 and a water outlet hole 105. The sides of the oxidation tank on both sides of the arc surface 101 are electrode plates made of stainless steel. In actual use, the aluminum wire passes through the oxidation tank 1 from the wire entry hole 102 and passes through the wire exit hole 103, and the aluminum wire in the oxidation tank 1 is concave into a ring by adjusting the length of the aluminum wire in the oxidation tank 1. After passing through the oxidation tank 1, the aluminum wire is naturally formed into a ring-shaped ceramic insulated aluminum wire. The water inlet hole 104 and the water outlet hole 105 are connected to the electrolyte circulation system to circulate the electrolyte in the oxidation tank 1 to take away the gas and excess heat generated by the oxidation reaction of the aluminum wire.
[0027] like Figure 2 As shown, the production equipment used in the present invention includes an oxidation tank 1, an inlet wheel 2, an outlet wheel 3, a sealing plug 4, an electrolyte circulation system, a micro-arc oxidation / thermal electrochemical oxidation power supply, an insulating tube 6, a winding mechanism and an elastic pressure roller 7.
[0028] The introduction wheel 2 is located at the wire entry hole 102, the lead-out wheel 3 is located at the wire exit hole 103, the water outlet pipe of the electrolyte circulation system is connected to the water entry hole 104, and the water inlet pipe of the electrolyte circulation system is connected to the water exit hole 105. The aluminum wire 5 is introduced into the oxidation tank 1 from the wire entry hole 102 via the introduction wheel 2, and then led out of the oxidation tank 1 from the wire exit hole 103 via the lead-out wheel 3. The aluminum wire 5 and the arc surface 101 in the oxidation tank 1 are coaxial. The electrode plate and the aluminum wire are respectively connected to the micro-arc oxidation / thermal electrochemical oxidation power supply. After the power is turned on, the aluminum wire 5 passes through the oxidation tank 1 with the arc surface and is naturally formed into a ring-shaped ceramic insulated aluminum wire 5' bent into circles. As a preferred embodiment, the introduction wheel 2 is two pairs of conductive copper wheels, and the aluminum wire 5 is connected to the micro-arc oxidation / thermal electrochemical oxidation power supply through the conductive copper wheels. The aluminum conductor 5 is stuck between two pairs of conductive copper wheels, and the rotating shafts of the two pairs of conductive copper wheels are cross-shaped. The conductive copper wheels actually play the role of guide wheels, so that the aluminum conductor 5 passes into the oxidation tank 1 in a straight line. In addition, there are sealing plugs 4 on the wire entry hole 102 and the wire exit hole 103. The sealing plug 4 is formed by wrapping the aluminum conductor 5 with a silicone pad or a polyurethane foam pad and then clamping it on the wire entry hole and the wire exit hole. The sealing plug 4 blocks the wire entry hole 102 and the wire exit hole 103 to prevent the electrolyte from flowing out of the oxidation tank 1. At the same time, since the sealing plug 4 is stuck on the wire entry hole 102 and the wire exit hole 103 and cannot move, the aluminum conductor 5 can slide through the wound silicone pad or polyurethane foam pad.
[0029] The insulating cylinder 6 is fixed on the rotating shaft of the winding mechanism, the arc surface 101 surrounds the insulating cylinder 6, and the ceramic insulated aluminum wire 5' is wound on the insulating cylinder 6. The rotation direction of the insulating cylinder 6 is consistent with the direction in which the ceramic insulated aluminum wire 5' slides out of the outlet hole 103. Try to keep the ceramic insulated aluminum wire 5' and the aluminum wire in the oxidation tank 1 on the same ring, and make the ceramic insulated aluminum wire 5' tangent to the outer periphery of the insulating cylinder 6 to minimize the bending of the ceramic insulated aluminum wire 5'. The elastic pressure roller 7 is located at the tangent point between the ceramic insulated aluminum wire 5' and the outer periphery of the insulating cylinder 6. The setting method of the elastic pressure roller 5 is the prior art. For details, please refer to the lower pressure roller in patent CN202121354504.5 for setting. After unwinding, insulation treatment and winding, the aluminum wire 5 can be formed into a ceramic insulated aluminum winding at one time. The ceramic insulated aluminum wire 5' is wound tightly around the outer periphery of the insulating cylinder 6 by the elastic pressure roller 7.
[0030] The preparation method of the present invention comprises:
[0031] (1) Two pairs of introduction wheels and one pair of outlet wheels are arranged at both ends of the arc surface of the oxidation tank with an arc surface, and a wire inlet hole, a wire outlet hole, a water inlet hole and a water outlet hole are respectively opened on the side wall of the oxidation tank connected to the two ends of the arc surface, and the side surfaces of the oxidation tank on both sides of the arc surface are surrounded by electrode plates; the rotating shafts of the two pairs of introduction wheels are cross-shaped;
[0032] (2) The aluminum wire is introduced into the oxidation tank from the wire entry hole along a straight line by two pairs of introduction wheels, and then the aluminum wire is led out from the wire exit hole by the lead-out wheel; the length of the aluminum wire between the introduction wheel and the lead-out wheel is adjusted so that the aluminum wire in the oxidation tank is concave into an arc coaxial with the arc surface; the insulation cylinder is fixed on the winding mechanism so that the arc surface surrounds the insulation cylinder;
[0033] (3) The oxidation tank is connected to the electrolyte circulation system through the water inlet, outlet and pipeline, the electrolyte is injected into the oxidation tank through the electrolyte circulation system, and the electrolyte in the oxidation tank is circulated through the external electrolyte circulation system to remove the gas and excess heat generated by the oxidation reaction of the aluminum wire. The electrode plate and the aluminum wire are respectively connected to the micro-arc oxidation / thermal electrochemical oxidation power supply, and the introduction wheel and the outlet wheel are rotated synchronously, so that the aluminum wire passes through the oxidation tank continuously and unread in a fixed arc shape. When the aluminum wire passes through the oxidation tank, a curved ceramic insulated aluminum wire is generated, and the curved ceramic insulated aluminum wire is directly wound on the rotating insulating cylinder.
[0034] (4) The rotation speed of the insulating cylinder is controlled by adjusting the winding mechanism, so that the ceramic insulated aluminum wire between the insulating cylinder and the outlet hole is kept in an arc shape, and the ceramic insulated aluminum wire between the insulating cylinder and the outlet hole and the aluminum wire in the oxidation tank are located on the same circular ring; and the relative position of the insulating cylinder and the oxidation tank is adjusted so that the ceramic insulated aluminum wire is tangent to the outer periphery of the insulating cylinder, and an elastic pressure roller is set at the tangent point of the ceramic insulated aluminum wire to the outer periphery of the insulating cylinder, and the ceramic insulated aluminum wire is wound tightly against the outer periphery of the insulating cylinder through the elastic pressure roller. After unwinding, insulation treatment and winding, the aluminum wire can be formed into a ceramic insulated aluminum winding at one time.
Claims
1. A method for preparing a ceramic insulated aluminum winding based on an oxidation groove with a circular arc surface, characterized in that: Includes steps: (1) An inlet wheel and an outlet wheel are arranged at both ends of the arc surface of the oxidation tank with an arc surface, and a wire inlet hole, a wire outlet hole, a water inlet hole and a water outlet hole are respectively opened on the side wall of the oxidation tank connected to the two ends of the arc surface, and the side surfaces of the oxidation tank on both sides of the arc surface are surrounded by electrode plates; (2) introducing the aluminum wire from the wire entry hole into the oxidation tank through the introduction wheel, and then leading the aluminum wire out of the wire exit hole through the lead-out wheel; adjusting the length of the aluminum wire between the introduction wheel and the lead-out wheel so that the aluminum wire in the oxidation tank is concave into an arc coaxial with the arc surface; fixing the insulating cylinder on the winding mechanism so that the arc surface surrounds the insulating cylinder; (3) connecting the oxidation tank to an electrolyte circulation system through a water inlet, a water outlet and a pipeline, injecting electrolyte into the oxidation tank through the electrolyte circulation system, connecting the electrode plate and the aluminum wire to a micro-arc oxidation / thermal electrochemical oxidation power source respectively, and synchronously rotating the introduction wheel and the output wheel so that the aluminum wire continuously passes through the oxidation tank in an arc shape, and the aluminum wire generates a curved ceramic insulated aluminum wire when passing through the oxidation tank, and the curved ceramic insulated aluminum wire is directly wound on the rotating insulating cylinder; (4) The rotation speed of the insulating drum is controlled by adjusting the winding mechanism so that the ceramic insulated aluminum wire between the insulating drum and the outlet hole is kept in an arc shape, and the ceramic insulated aluminum wire between the insulating drum and the outlet hole and the aluminum wire in the oxidation tank are located on the same circular ring.
2. The method according to claim 1, characterized in that The step (4) comprises: The rotation speed of the insulating cylinder is controlled by adjusting the winding mechanism so that the ceramic insulated aluminum conductor between the insulating cylinder and the outlet hole is kept in an arc shape, and the ceramic insulated aluminum conductor between the insulating cylinder and the outlet hole and the aluminum conductor in the oxidation tank are located on the same circular ring; and the relative position of the insulating cylinder and the oxidation tank is adjusted so that the ceramic insulated aluminum conductor is tangent to the outer periphery of the insulating cylinder.
3. The method according to claim 2, characterized in that The step (4) comprises: The rotation speed of the insulating drum is controlled by adjusting the winding mechanism, so that the ceramic insulated aluminum wire between the insulating drum and the outlet hole is kept in an arc shape, and the ceramic insulated aluminum wire between the insulating drum and the outlet hole and the aluminum wire in the oxidation tank are located on the same circular ring; and the relative position of the insulating drum and the oxidation tank is adjusted so that the ceramic insulated aluminum wire is tangent to the outer circumference of the insulating drum, and an elastic pressure roller is arranged at the tangent point of the ceramic insulated aluminum wire to the outer circumference of the insulating drum, and the ceramic insulated aluminum wire is wound tightly against the outer circumference of the insulating drum through the elastic pressure roller.
4. The method according to claim 1, characterized in that The step (1) comprises: Two pairs of introduction wheels and a pair of outlet wheels are arranged at both ends of the arc surface of the oxidation tank with an arc surface, and a wire inlet hole, a wire outlet hole, a water inlet hole and a water outlet hole are respectively opened on the side wall of the oxidation tank connected to the two ends of the arc surface, and the side surfaces of the oxidation tank on both sides of the arc surface are surrounded by electrode plates; the rotating shafts of the two pairs of introduction wheels are cross-shaped; The step (2) comprises: The aluminum wire is introduced into the oxidation tank from the wire entry hole in a straight line through two pairs of introduction wheels, and then led out of the wire exit hole through the lead-out wheel; the length of the aluminum wire between the introduction wheel and the lead-out wheel is adjusted so that the aluminum wire in the oxidation tank is concave into an arc coaxial with the arc surface; the insulating cylinder is fixed on the winding mechanism so that the arc surface surrounds the insulating cylinder.
Citation Information
Patent Citations
Winding equipment for light-color home textile decorative cloth
CN214934567U
Electric motor
CN109690924A
Continuous electroplating device for metallic strip
JP1995268685A