A low-cost shape control method for 355MPa yield strength thin steel plate
Through high-temperature heating, segmented cooling and thermal straightening treatment during the steel plate production process, the plate shape control problem of yield strength of 355MPa grade thin steel plate with a thickness specification of 6 to 10mm and a width greater than 3000mm is solved, and the low-cost steel plate pass rate is achieved Improved straightness.
Patent Information
- Application Number
- CN202210897032.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-07-28
AI Technical Summary
The existing technology is difficult to effectively control the plate shape of a 355MPa grade thin steel plate with a thickness specification of 6 to 10 mm and a width greater than 3000 mm, resulting in wave defects, high scrap rolling rate, and deformation problems caused by uneven temperature drop during the production process, affecting the steel plate. one pass rate and cost.
Heat the cast billet to 1220~1245℃, and control the cooling water volume of the rolling roll in stages during the rolling process. Combined with high-pressure water descaling, optimized rolling pressure rate and final rolling temperature, thermal straightening and air-cooling treatment are carried out to ensure the steel plate During the cooling process, the temperature drop is uniform, which reduces internal stress, and reduces the flatness requirements of the steel plate through the cooling control process and preheating of the cold bed.
The plate-shaped control of the yield strength of 355MPa grade thin steel plate with a thickness specification of 6 to 10mm and a width greater than 3000mm is achieved, which reduces the scrap rate and production costs, ensures that the straightness of the steel plate is below 5mm/2m, and meets the mass production requirements.
Smart Images

Figure BDA0003769304590000071 
Figure BDA0003769304590000072 
Figure BDA0003769304590000073
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel plate production, and in particular to a plate shape control method for a low-cost thin steel plate with a yield strength of 355 MPa and a thickness specification of 6 to 10 mm and a width greater than 3000 mm. Background Art
[0002] The main chemical elements of the yield strength 355MPa grade steel plate are C, Si, Mn, Al, Nb, etc. In general, the wide and thick plate mills above 4m mainly produce steel plates of this grade with a thickness greater than 10mm. For steel plates with a thickness of 6-10mm, they are generally produced on hot-rolled thin plate continuous rolling mills. The width of the finished steel plate is narrow and it is a coil. For products such as ship plates, boiler container plates, and steel plates for construction, since the width of the steel plate is required to be wider (to reduce the weld during the welding process), only flat plates can be produced. Since the rolled pieces of such steel plates are thin and the temperature drops quickly, they are very sensitive to temperature changes. In the production process, wave defects and rolling waste are very likely to occur, and the scrap rate is high. After rolling, the steel plate is prone to a plate shape similar to that of a corrugated plate, resulting in excessive flatness and difficulty in forming mass production capacity. The plate shape of this type of steel plate usually needs to be leveled by a subsequent cold straightening machine, which seriously affects the one-time pass rate of the steel plate.
[0003] In addition, during the cooling process of the cooling bed, the upper surface of the steel plate is in contact with the air and the lower surface is in contact with the cooling bed, resulting in different heat transfer rates on the upper and lower surfaces of the steel plate, different temperature drops and different thermal stresses, which eventually cause the steel plate to deform and fail to meet the straightness requirements. For steel plates that fail to meet the straightness requirements, they can only be straightened again by a cold straightening machine, which increases production costs and prolongs the delivery cycle.
[0004] It can be seen that how to solve the plate shape problem of thin steel plates with a thickness of 6 to 10 mm, a width greater than 3000 mm, and a yield strength of 355 MPa, and improve the one-time pass rate of steel plates, is the key to the development and application of this type of steel plate.
[0005] So far, there are few studies on the shape control of the above-mentioned thin-gauge, wide-width steel plates with a yield strength greater than 355MP at home and abroad. The Chinese patent application with publication number CN103722023A discloses "a TMCP high-strength ship plate shape control method", which is effective for the shape control of high-strength ship plates after rolling. However, this method is applicable to steel plates with a thickness of 30 to 60 mm, and does not involve the shape control of thin steel plates. The Chinese patent application with publication number CN101885004A discloses a "shape control method for low-alloy high-strength steel plates in the controlled cooling stage". This method has a certain effect on the shape control of steel plates that need to be cooled after rolling, but it does not involve the shape control of thin-gauge steel plates that do not require water spray cooling after rolling. The Chinese patent application with publication number CN101450353A discloses "a method for controlling the shape of a steel plate", which is a method for controlling the shape of a medium and thick plate. However, the method is aimed at the rolled shape of the steel plate, and does not involve the problem of poor shape that occurs during the cooling process on the cooling bed after the steel plate is flattened by a straightening machine after rolling.
[0006] In the journal article "Optimization Control of Hot-rolled Thin-Gauge Plate Production Process" ("Henan Metallurgy" 2020.8), the problem of plate shape control of thin-gauge steel plates with a thickness of 6 to 10 mm was solved by optimizing the heating, rolling and pressing procedures. However, the width of the steel plates produced was less than 3000 mm, and its production method could not meet the control requirements of the plate shape of steel plates with a width of more than 3000 mm. Summary of the invention
[0007] The present invention provides a low-cost plate shape control method for thin steel plates with a yield strength of 355 MPa. The method is suitable for controlling the plate shape of thin steel plates with a thickness of 6 to 10 mm, a width greater than 3000 mm, and a yield strength of 355 MPa. The method can meet the plate shape control requirements of the steel plates without subsequent cold straightening treatment, and solves the problems that such steel plates are prone to wave shapes during production due to thin rolled pieces and fast temperature drop, which affects the one-time pass rate and cost reduction rate of the steel plates.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] A low-cost plate shape control method for a 355MPa yield strength thin steel plate, wherein the steel plate production process includes heating of the ingot, rolling, cooling, hot straightening and air cooling; specifically, the following steps are included:
[0010] 1) Heating the ingot: The ingot is heated to 1220-1245°C, the total heating time of the soaking section and the heating section is 3-4 hours, and the total time in the furnace is 4.5-5.5 hours;
[0011] 2) Rolling: During rolling, the rollers are cooled in sections. When rolling the 1 / 6L length section of the billet head, the roller cooling water is not turned on; when rolling the 1 / 6L length section of the billet tail, the roller cooling water volume is controlled at 20-35m 3 / h, when rolling the remaining length of the billet, the roller cooling water volume is controlled at 40~60m 3 / h; where L is the length of the billet in the rolling direction during each rolling pass; during rolling, at least the first three passes adopt a large reduction rate, and the reduction rate of each pass is not less than 20%, and at least the last two passes adopt a small reduction rate, and the reduction rate of each pass is not more than 5%; the final rolling temperature is 750-860℃, and the rolling speed is controlled at 5-6.5m / s; at the same time, the roller cooling water flow rate from the rolling mill to the pre-straightening machine is adjusted to 200-250m 3 / h;
[0012] 3) Cooling; the cooling temperature is 730-840℃, the return temperature is 600-680℃, the cooling system head and tail shielding is put into operation; the upper header opening correction value is -1000-1200mm, the lower header opening correction value is -1800-2000mm; the header opens 2-4 groups of water, each group of water volume is 180-220m 3 / h, the water volume ratio between the lower header and the upper header is 2-3; the roller speed is 2.0-3m / s, and the acceleration is 0.001-0.005m / s 2 ;
[0013] 4) Hot straightening; the position of the lead-in roller is -0.8~-2.5mm, the position of the lead-out roller is -2.7~-3.3mm, the final straightening temperature is ≤550℃, and the straightening force is 18000~20000kN;
[0014] 5) Air cool to room temperature.
[0015] The chemical composition of the steel plate is as follows by weight percentage: C 0.14%-0.17%, Si 0.3%-0.4%, Mn 0.55%-0.75%, P≤0.03%, S≤0.025%, Al 0.015%-0.04%, N≤0.012%, the remainder is Fe and unavoidable impurities, O in the impurities is ≤0.0050%, and the total amount of other impurities is less than 0.05%.
[0016] The steel plate has a thickness of 6 to 10 mm and a width of more than 3000 mm, and is obtained by rolling a cast billet with a thickness of less than 250 mm through a medium and thick plate reciprocating rolling mill;
[0017] In the step 2), before rolling, the heated ingot is descaled by high-pressure water, the descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa.
[0018] In the step 2), the last two passes of rolling are descaled by using the cooling water of the rolling mill before rolling, the descaling time is 0.2 to 0.5 min, and the descaling machine pressure is 20 to 25 MPa.
[0019] The straightness of the finished steel plate is below 5mm / 2m.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1) The ingot is heated at a relatively high temperature, and the furnace time of the soaking section and the heating section is ensured at the same time, which shortens the temperature difference between the surface and the core of the ingot and improves the uniformity of the metal flow in the horizontal and vertical directions on the surface of the steel plate; the total furnace time is controlled to effectively inhibit the excessive growth of austenite grains and ensure the performance of the steel plate;
[0022] 2) Control the cooling water flow of the rollers, and use a segmented cooling process to prevent a large amount of cooling water from flowing on the surface of the steel plate, causing an uncontrolled temperature drop on the surface of the steel plate and increasing the number of rolling passes; reasonably control the cooling water volume of the rollers, effectively control the roller shape, and greatly improve the irregular deviation and sickle bend caused by the uneven temperature distribution of the head, middle and tail of the steel billet during the rolling process. In addition, optimize the pass reduction rate at different stages of rolling and control the final rolling temperature and rolling speed, effectively ensuring the initial shape of the rolled steel plate and reducing the internal stress of the steel plate;
[0023] 3) By optimizing the controlled cooling process, the temperature uniformity of the head, middle and tail of the steel plate is achieved to avoid warping caused by uneven temperature at different positions of the steel plate after controlled cooling; three-pass hot straightening is adopted to set the initial lead-in roller, lead-out roller position, straightening temperature and pressure to ensure that the steel plate is straight and has a good shape after straightening; at the same time, a lower final straightening temperature is set to reduce the temperature drop range of the steel plate during the cooling process to avoid large internal stress due to rapid phase change;
[0024] 4) Through measures such as rolling auxiliary steel plate preheating step cooling bed, the temperature drop range of the product steel plate is small during the cooling process, and the temperature drop of the upper and lower surfaces is uniform, avoiding thermal deformation, ensuring that the final straightness of the steel plate meets the requirement of less than 5mm / 2m, and saving the cost of subsequent cold straightening process. DETAILED DESCRIPTION
[0025] The present invention discloses a low-cost 355MPa yield strength thin steel plate shape control method, wherein the steel plate production process includes heating of the ingot, rolling, cooling, hot straightening and air cooling; specifically, the following steps are included:
[0026] 1) Heating the ingot: The ingot is heated to 1220-1245°C, the total heating time of the soaking section and the heating section is 3-4 hours, and the total time in the furnace is 4.5-5.5 hours;
[0027] 2) Rolling: During rolling, the rollers are cooled in sections. When rolling the 1 / 6L length section of the billet head, the roller cooling water is not turned on; when rolling the 1 / 6L length section of the billet tail, the roller cooling water volume is controlled at 20-35m 3 / h, when rolling the remaining length of the billet, the roller cooling water volume is controlled at 40~60m 3 / h; where L is the length of the billet in the rolling direction during each rolling pass; during rolling, at least the first three passes adopt a large reduction rate, and the reduction rate of each pass is not less than 20%, and at least the last two passes adopt a small reduction rate, and the reduction rate of each pass is not more than 5%; the final rolling temperature is 750-860℃, and the rolling speed is controlled at 5-6.5m / s; at the same time, the roller cooling water flow rate from the rolling mill to the pre-straightening machine is adjusted to 200-250m 3 / h;
[0028] 3) Cooling; the cooling temperature is 730-840℃, the return temperature is 600-680℃, the cooling system head and tail shielding is put into operation; the upper header opening correction value is -1000-1200mm, the lower header opening correction value is -1800-2000mm; the header opens 2-4 groups of water, each group of water volume is 180-220m 3 / h, the water volume ratio between the lower header and the upper header is 2-3; the roller speed is 2.0-3m / s, and the acceleration is 0.001-0.005m / s 2 ;
[0029] 4) Hot straightening; the position of the lead-in roller is -0.8~-2.5mm, the position of the lead-out roller is -2.7~-3.3mm, the final straightening temperature is ≤550℃, and the straightening force is 18000~20000kN;
[0030] 5) Air cool to room temperature.
[0031] The chemical composition of the steel plate is as follows by weight percentage: C 0.14%-0.17%, Si 0.3%-0.4%, Mn 0.55%-0.75%, P≤0.03%, S≤0.025%, Al 0.015%-0.04%, N≤0.012%, the remainder is Fe and unavoidable impurities, O in the impurities is ≤0.0050%, and the total amount of other impurities is less than 0.05%.
[0032] The steel plate has a thickness of 6 to 10 mm and a width of more than 3000 mm, and is obtained by rolling a cast billet with a thickness of less than 250 mm through a medium and thick plate reciprocating rolling mill;
[0033] In the step 2), before rolling, the heated ingot is descaled by high-pressure water, the descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa.
[0034] In the step 2), the last two passes of rolling are descaled by using the cooling water of the rolling mill before rolling, the descaling time is 0.2 to 0.5 min, and the descaling machine pressure is 20 to 25 MPa.
[0035] The straightness of the finished steel plate is below 5mm / 2m.
[0036] The working principle of the low-cost 355MPa yield strength thin steel plate shape control method described in the present invention is as follows:
[0037] 1. Billet heating process;
[0038] The ingot (thickness less than 250mm, preferably continuous casting ingot) is fed into a walking beam heating furnace for heating. The ingot is heated to 1220-1245°C. The total heating time of the soaking section and the heating section is 3-4 hours, and the total time in the furnace is 4.5-5.5 hours. The present invention adopts a higher heating temperature and ensures the time of the soaking section and the heating section in the furnace at the same time, so as to shorten the temperature difference between the surface and the core of the ingot and improve the uniformity of the metal flow in the horizontal and vertical directions on the surface of the steel plate. The purpose of controlling the total time in the furnace is to effectively inhibit the excessive growth of austenite grains and ensure the mechanical properties of the steel plate.
[0039] 2. High-pressure water descaling and rolling process;
[0040] Before rolling, high-pressure water is used to descale the ingot after leaving the heating furnace. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa.
[0041] During rolling, reduce the cooling water volume of the roller table from the rolling mill to the pre-straightening machine to 200-250m 3 / h, to avoid a large amount of cooling water flowing on the surface of the steel plate, which may cause uncontrolled temperature drop on the surface of the steel plate and increase the number of rolling passes; the rollers are controlled by segmented cooling. When the length section of the head of the rolling billet is set, the roller cooling water is not turned on. When the length section of the middle of the rolling billet is set, the roller water volume is set at 40-60m 3 / h, when rolling the set length section at the tail of the billet, the water volume of the roller is 20~35m 3 / h. By adjusting the amount of cooling water for the rolls, the roll shape can be effectively controlled, which greatly improves the irregular deviation and sickle bend defects that are easy to occur during the rolling process due to the uneven temperature distribution of the head, middle and tail of the billet. In addition, at least the first three passes of rolling use a large reduction rate, and the reduction rate of each pass is not less than 20%, and at least the last two passes use a small reduction rate, and the reduction rate of each pass is controlled below 5%. Before the last two passes are rolled, the mill cooling water is used for descaling, the descaling time is 0.2-0.5min, and the descaling machine pressure is 20-25MPa. The first few passes of rolling use a large reduction rate to maximize the capacity of the rolling mill. The last few passes use a small reduction rate to flatten the shape of the steel plate and reduce the internal stress of the steel plate due to the uncontrolled temperature drop of the steel plate. In order to ensure that the final rolling temperature of the steel plate is between 750 and 860℃, the rolling speed is controlled at 5-6.5m / s.
[0042] 3. Cooling and heat straightening process;
[0043] Cooling temperature 730~840℃, return to red temperature 600~680℃, cooling system head and tail shielding input; upper header opening correction value -1000~-1200mm, lower header opening correction value -1800~-2000mm; fully automatic cooling control: water volume per group 180~220m 3 / h, 2 to 4 water groups are opened in the header, and the water volume ratio between the lower header and the upper header is 2 to 3; roller speed is 2.0 to 3 m / s, and the acceleration is 0.001 to 0.005 m / s 2 .
[0044] The hot straightening is carried out in three passes, with the lead-in roller position of -0.8 to -2.5mm, the lead-out roller position of -2.7 to -3.3mm, the final straightening temperature not exceeding 550℃, and the straightening force between 18000 and 20000 kN. The production path of replacing part of the Mn addition with water is adopted to reduce the alloy cost of 355MPa grade steel plates, and at the same time, the cooling control parameters are limited. By setting the appropriate roller gap, straightening force and straightening passes, the straightened steel plates are guaranteed to be straight and have good plate shape; at the same time, a lower final straightening temperature is set to reduce the temperature drop range of the steel plates during the cooling process, avoiding large internal stresses due to rapid phase changes.
[0045] 4. Steel plate air cooling process;
[0046] Since the cooling rate of the lower surface of the thin gauge steel plate is faster than that of the upper surface, the internal stress of the steel plate is not fully released during the cooling process of the cooling bed, and bulging deformation is likely to occur. The present invention adopts a method of preheating the cooling bed to solve the above problem. Before rolling a thin steel plate with a yield strength of 355MPa (hereinafter referred to as the product steel plate), first roll no less than 20 steel plates with a thickness greater than 15mm and a width greater than 3000mm (hereinafter referred to as the auxiliary steel plate), and the length of the auxiliary steel plate is greater than the length of the product steel plate subsequently rolled. The auxiliary steel plates are placed side by side on the walking cooling bed in the rolling order, and the walking cooling bed is preheated by the residual heat of the auxiliary steel plates; then the product steel plates are rolled; while rolling the product steel plates, the auxiliary steel plates are continuously pushed in the shearing or fire cutting direction to vacate the position for placing the product steel plates on the walking cooling bed. After the rolling of the product steel plates is completed, they are immediately placed side by side on the preheated walking cooling bed.
[0047] The present invention combines the chemical composition of steel with the controlled rolling and controlled cooling process, overcomes the shortcomings of the prior art, and solves the problem of shape control of thin steel plates with a thickness of 6 to 10 mm, a width greater than 3000 mm, and a yield strength of 355 MPa. The flatness of the steel plate is controlled to be below 5 mm / 2 m, meeting the technical requirements.
[0048] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.
[0049] [Example]
[0050] In this embodiment, Table 1 is the chemical composition of the steel plate, Table 2 is the heating system of the ingot and the high-pressure water descaling process parameters before rolling; Table 3 is the rolling process parameters of the steel plate; Table 4 is the steel plate controlled cooling process parameters; Table 5 is the steel plate straightening process parameters and the flatness of the finished steel plate.
[0051] Table 1 Chemical composition of steel plates (wt, %)
[0052] Example C Si Mn Al Ceq 1 0.14 0.35 0.55 0.021 0.23 2 0.16 0.40 0.65 0.033 0.27 3 0.14 0.32 0.73 0.039 0.26 4 0.17 0.31 0.75 0.027 0.30 5 0.15 0.37 0.59 0.035 0.25 6 0.16 0.39 0.56 0.019 0.25
[0053] Note: Impurity elements in steel are P≤0.03%, S≤0.025%; 0≤0.0050%, and the total amount of other impurity elements is less than 0.05%.
[0054] Table 2 Billet heating system and pre-rolling high pressure water descaling process parameters
[0055]
[0056] Table 3 Rolling process parameters of steel plates
[0057]
[0058] Table 4 Steel plate controlled cooling process parameters
[0059] Example Cooling temperature / ℃ Red return temperature / ℃ Upper header correction value / mm Lower header correction value / mm Number of header opening groups Roller speed m / s 1 770 620 -1200 -1900 3 2.3 2 820 630 -1100 -2000 3 2.5 3 810 680 -1000 -1800 2 3.0 4 740 601 -1050 -1950 3 2.6 5 798 625 -1130 -1830 2 2.7 6 730 630 -1160 -1950 2 2.8
[0060] Table 5 Steel plate straightening process parameters and finished steel plate straightness
[0061]
[0062] It can be seen that the method of the present invention solves the plate shape problem of producing hot-rolled steel plates with a thickness of 6 to 10 mm, a width of more than 3000 mm, and a yield strength of 355 MPa using continuous casting billets with a thickness of less than 250 mm, and the straightness of the steel plates meets the technical requirements of less than 5 mm / 2 m.
[0063] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A low-cost plate shape control method for a thin steel plate with a yield strength of 355 MPa, characterized in that: The finished steel plate has a thickness of 6-8mm, a width greater than 3000mm, and a straightness of less than 5mm / 2m; it is obtained by rolling a cast billet with a thickness of less than 250mm through a medium and thick plate reciprocating rolling mill; The chemical composition of the steel plate is as follows by weight percentage: C 0.14% to 0.17%, Si 0.3% to 0.4%, Mn 0.55% to 0.75%, P≤0.03%, S≤0.025%, Al 0.015% to 0.04%, N≤0.012%, the remainder being Fe and unavoidable impurities, O in the impurities≤0.0050%, and the total amount of other impurities being less than 0.05%; The steel plate production process includes heating, rolling, cooling, hot straightening and air cooling of the ingot; specifically, it includes the following steps: 1) Heating the ingot: The ingot is heated to 1220-1245°C. The total heating time in the soaking section and the heating section is 3-4 hours, and the total time in the furnace is 4.5-5.5 hours. 2) Rolling: Before rolling, the heated ingot is descaled with high-pressure water. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa. During rolling, the rollers are cooled in sections. When rolling the 1 / 6L length section of the billet head, the roller cooling water is not turned on. When rolling the 1 / 6L length section of the billet tail, the roller cooling water volume is controlled at 20 to 35 m 3 / h, when rolling the remaining length of the billet, the roller cooling water volume is controlled at 40~60m 3 / h; where L is the length of the billet in the rolling direction during each rolling pass; during rolling, at least the first three passes use a large reduction rate, with a reduction rate of no less than 20% for each pass, and at least the last two passes use a small reduction rate, with a reduction rate of no more than 5% for each pass; the final rolling temperature is 750-850℃, and the rolling speed is controlled at 5-6.5m / s; at the same time, the roller cooling water flow rate from the rolling mill to the pre-straightening machine is adjusted to 200-250m 3 / h; the last two passes of rolling are descaled by mill cooling water before rolling, the descaling time is 0.2-0.5min, and the descaling machine pressure is 20-25MPa; 3) Cooling; the cooling temperature is 730~820℃, the return temperature is 600~630℃, the cooling system head and tail shielding is put into operation; the upper header opening correction value is -1000~-1200mm, the lower header opening correction value is -1800~-2000mm; the header opens 2~4 groups of water, each group of water volume is 180~220m 3 / h, the water volume ratio between the lower header and the upper header is 2-3; the roller speed is 2.0-3m / s, and the acceleration is 0.001-0.005m / s 2 ; 4) Hot straightening; the position of the lead-in roller is -0.8~-2.5mm, the position of the lead-out roller is -2.7~-3.3mm, the final straightening temperature is ≤550℃, and the straightening force is 18000~20000kN; 5) Air cool to room temperature.
Citation Information
Cited By
Strip shape control method for low-carbon-equivalent 355MPa-grade normalized rolled thin-gauge steel plate
CN116713325A
A method for controlling the shape of a low carbon equivalent 355mpa grade normalized rolled thin gauge steel plate