A manufacturing method for improving the strength and toughness of 1100MPa grade engineering structure steel extra thick plate

By optimizing the smelting, heating, rolling and heat treatment processes, the problem of poor low-temperature impact toughness performance of the steel extra-thick plate core for 1100MPa grade engineering structures is solved, high-strength and low-cost production is achieved, and the plate shape control of the steel plate is met. Require.

CN118639144BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118543.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-03
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The prior art cannot effectively improve the low-temperature impact toughness of steel extra-thick plates for 1100MPa grade engineering structures, especially the core performance, and the traditional heat treatment process cannot meet the technical requirements of the steel plates, resulting in high manufacturing costs and impact on welding performance.

Method used

By optimizing the smelting, heating, rolling, cold control and heat treatment processes, the chemical composition and production process of steel plates are controlled, including water-molding smelting, outside furnace refining, micro-Ti treatment, B alloying, continuous casting, and casting billet heating slowing down Reheating of cold and casting billets, controlled rolling and cooling, heat straightening, slow cooling and quenching of steel plates, and preparing 1100MPa grade steel extra-thickness plates for engineering structures with a thickness of 60 to 100mm.

Benefits of technology

The high yield strength, tensile strength and low-temperature impact toughness of the steel plate are achieved, the core performance requirements are met, the manufacturing cost is reduced, and subsequent offline flattening and straightening treatment is required, ensuring the plate shape control of the plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a manufacturing method for improving the strength and toughness of a 1100MPa grade engineering structure steel extra-thick plate. The chemical composition of the steel plate comprises: C 0.16%-0.19%, Si 0.2%-0.35%, Mn 1.05%-1.35%, P≤0.02%, S≤0.005%, Nb 0.010%-0.040%, Ti 0.010%-0.025%, Mo 0.5%-0.8%, Als 0.02%-0.05%, B 0.0008%-0.0018%, Cr 0.35%-0.5%, Ni 0.3%-0.5%, Ceq 0.57%~0.65%, the balance is Fe and impurities; the production process of the steel plate includes molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, heating and slow cooling of the ingot into the pit, reheating of the ingot, controlled rolling and cooling, hot straightening, slow cooling of steel plate stacking and quenching. The present invention solves the problem of poor low-temperature impact toughness of the core of the extra-thick steel plate of this steel grade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of engineering structure steel production, and in particular to a manufacturing method for improving the strength and toughness of 1100MPa-level engineering structure steel extra-thick plates (60-100mm). Background Art

[0002] In recent years, with the rapid development of industries such as hydropower, engineering machinery, and wind power construction, the demand for thick steel plates has increased. However, due to the lack of necessary production equipment and technical support, the mechanical properties (such as negative temperature impact toughness) of thick, heavy, and high-strength steels are not good, especially the toughness index requirements of the core (1 / 2 thickness) cannot be met, resulting in the current 1100MPa-grade engineering structure steel not being able to meet market demand. Thick steel plates for hydropower, engineering machinery, and wind power can only be produced by forging, which seriously restricts the development of construction in the fields of hydropower, engineering machinery, and wind power stations.

[0003] Since engineering structural steel is often in a special service environment, there are strict requirements for the steel's low-temperature impact toughness and lamellar tearing resistance. Among them, low-temperature impact toughness is one of the important indicators of its service performance. The traditional heat treatment process cannot meet the technical requirements of steel plates. It is necessary to control the structure of the steel plate during the heat treatment process, so as to achieve good strength and toughness matching while achieving performance uniformity, especially the uniformity of low-temperature impact toughness. At present, the thick-gauge and high-strength grade extra-thick plates at home and abroad are mainly regulated by increasing the thickness of the ingot and the alloy composition, but this leads to a significant increase in manufacturing costs, and the increase in the content of alloy elements such as Mn and Cu will lead to serious segregation and affect welding performance.

[0004] The Chinese invention patent with publication number CN101984119B discloses a "NV-F690 ultra-high strength ship plate steel and its preparation method", which adopts optimized chemical composition ratio, controlled rolling, cooling process and various subsequent heat treatment methods to produce ship plate steel with ultra-high strength and low temperature toughness. The maximum thickness of the ship plate steel can reach 50mm. Through different heat treatment methods, the mechanical properties can meet the certification indicators of F690 grade ship plate steel in the Norwegian Classification Society (DNV). However, its Cu content (1.00-1.70%) is relatively high. In order to avoid the "copper brittleness" phenomenon, it is necessary to add an appropriate proportion of Ni elements, resulting in a high alloy cost. At the same time, with the revision of the classification society specifications in recent years, it is stipulated that the Cu content of TMCP steel plates cannot be higher than 0.55wt.%, which limits the scope of use of this method. In addition, the strength grade of the ship plate steel is 690MPa, the upper limit of thickness is only 50mm, and there is no clear requirement for the core performance.

[0005] The Chinese invention patent with publication number CN114293110B discloses "a thick-gauge 800MPa-grade hydropower steel and its efficient and low-cost production method". It adopts an optimized chemical composition ratio, controlled rolling and various subsequent heat treatment methods to produce hydropower steel with ultra-high strength and low-temperature toughness. The maximum thickness of the steel plate can reach 65mm, which still cannot meet the production needs of thick-gauge steel plates. In addition, the alloy content in the steel is relatively high, and the core performance requirements are not clear. Summary of the invention

[0006] The present invention provides a manufacturing method for improving the strength and toughness of 1100MPa-level extra-thick plates for engineering structures. By optimizing the process of smelting, heating, rolling, controlled cooling and heat treatment, an extra-thick steel plate with a thickness of 60 to 100mm for 1100MPa-level engineering structures is finally prepared, which solves the problem of poor low-temperature impact toughness of the core of the extra-thick steel plate of this steel grade. The plate shape control requirements of the plate can be met without subsequent offline flattening and straightening treatment.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A manufacturing method for improving the strength and toughness of a 1100MPa grade engineering structure steel extra-thick plate, comprising chemical composition control and production process control; the chemical composition of the steel plate comprises, by weight percentage: C 0.16% to 0.19%, Si 0.2% to 0.35%, Mn 1.05% to 1.35%, P≤0.02%, S≤0.005%, Nb 0.010% to 0.040%, Ti 0.010% to 0.025%, Mo 0.5% to 0.8%, Als 0.02% to 0.05%, B 0.0008% to 0.0018%, Cr 0.35% to 0.5%, Ni 0.3% to 0.5%, Ceq 0.57%~0.65%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, the remainder is Fe and unavoidable impurities, and the total amount of impurity elements is less than 0.05%; the production process of steel plate includes molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, heating and slow cooling of ingot into the pit, reheating of ingot, controlled rolling and cooling, hot straightening, slow cooling and quenching of steel plate stacking.

[0009] Further, the production process control is as follows:

[0010] 1) Molten steel is smelted until the ingot is heated and slowly cooled;

[0011] The raw materials are pretreated with KR molten iron to control the S content ≤ 0.015%; the P content is controlled to be ≤ 0.02% in converter smelting, and the C content is controlled to be within the range of 0.16% to 0.19% at the converter smelting end point. Argon is blown for 20 to 35 minutes when the converter is tapped; RH vacuum degassing is maintained for more than 20 minutes after LF refining, and then Al is added; Ti-Fe is added for micro-titanium treatment, and B-Fe alloy is added for B alloying; the superheat is controlled to be 15 to 25 during slab continuous casting ℃, the continuous casting billet drawing rate is 0.8~1.3m / min; the electromagnetic stirring current intensity in the secondary cooling zone is 200~250A, the secondary cooling water volume is 1.3~2.0L / kg, and the billet is pressed down by 30~45mm under heavy pressure at the horizontal fan-shaped section, i.e. the end of solidification; the billet is put into the pit for slow cooling after it comes off the line, the pit temperature is not less than 600℃, the slow cooling temperature is 600~650℃, the slow cooling time is 24~36h, and the billet is cooled down to below 200℃ in the pit before leaving the pit;

[0012] 2) Reheating of the ingot: the temperature of the preheating section is 900-1050°C, the temperature of the soaking section and the heating section are both 1205-1230°C, the total heating time of the soaking section and the heating section is 4.5-6h, the total time in the furnace is 6.5-8h, the air-fuel ratio is controlled at 1:1.9-1:2.3, and the temperature difference between the upper and lower surfaces of the ingot is controlled within 15°C;

[0013] 3) Control rolling, cooling and hot straightening; Rolling in two stages; Rough rolling start temperature ≥ 1120℃, rough rolling final rolling temperature 980~1025℃, rough rolling no more than 6 passes, at least the first 2 passes reduction rate is above 15%; Spray descaling water 2 times during the intermediate billet waiting for temperature, the descaling time for each pass is 1~2min, and the descaling water pressure is 15~20MPa; Finish rolling start temperature is 860~920℃, finish rolling final rolling temperature is 830~860℃, finish rolling no more than 6 passes, at least the first 2 The reduction rate of each pass is above 20%; the finishing rolling speed is 1-2m / s, and the steel throwing speed is 5-6.5m / s; the steel plate is cooled directly after the relaxation before temperature relaxation, the start cooling temperature is 700-710℃, the final cooling temperature is 380-450℃, and the cooling speed is controlled at 45-65℃ / s; the hot straightening temperature is 650-700℃, the straightening force is 3000-4500kN, the bending roll amount is set to 1-1.6mm, and the tilting value is set to 3.5-5.5mm;

[0014] 4) Slow cooling of steel plate stacking; immediately after hot straightening, put the steel plate into the slow cooling tank, the temperature of the tank shall not be lower than 500℃, the slow cooling time shall not be less than 36h, and the upper part of the slow cooling tank shall be insulated with asbestos;

[0015] 5) Quenching; The first high-temperature quenching temperature is 880-910°C, and the time in the furnace is 1.6-2.0 min / mm; the second low-temperature quenching temperature is 770-820°C, and the time in the furnace is 1.1-1.5 min / mm; during the two quenching processes, the swing time of the steel plate in the high-pressure zone is controlled to be 1-1.5 min / mm, and the cooling rate is 50-65°C / s; the swing time of the steel plate in the low-pressure zone is controlled to be 2.0-2.5 min / mm, and the cooling rate is 25-35°C / s; during the two steel plate quenching processes, the upper and lower manifold water ratio is 1.6-2.2, the quenching machine roller speed is 1.2-2.0 m / s, and the quenching end temperature is 300-350°C, at which temperature the steel plate achieves low-temperature self-tempering.

[0016] Furthermore, the thickness of the finished steel plate is 60 to 100 mm.

[0017] Furthermore, the thickness of the cast billet is 300 to 360 mm; the thickness of the intermediate billet is 2.5 to 3.5 times the thickness of the finished steel plate.

[0018] Furthermore, the mechanical properties of the finished steel plate are: yield strength ≥1120MPa, tensile strength ≥1400MPa, elongation ≥12%, Z-direction section shrinkage ≥50%, transverse Charpy impact energy at -40°C at 1 / 2 thickness ≥100J; the straightness of the steel plate ≤3mm / 2m.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1) By blowing argon, controlling the continuous casting superheat, billet drawing rate, electromagnetic stirring current intensity in the secondary cooling zone, and secondary cooling water volume, the surface and corner quality defects of the billet are effectively reduced, the average carbon segregation index is reduced, and segregation is inhibited; at the end of solidification, the billet is put under heavy pressure to effectively reduce the central looseness level and segregation of the billet, refine the austenite grains, reduce internal structural defects, and slowly cool the billet into the pit, which helps to reduce the central segregation of the billet and ensure the core performance of the rolled steel plate.

[0021] 2) By controlling the preheating temperature, the carbides of Ti and Nb are ensured to be quickly and fully dissolved in the matrix and fully diffused; by adopting a high heating temperature, the furnace time of the soaking section and the heating section is ensured, the air-fuel ratio is controlled, the temperature difference between the surface and the core of the continuous casting billet is shortened, the uniformity of the lateral and longitudinal metal flow on the surface of the steel plate is improved, and the temperature uniformity of the upper and lower surfaces of the billet in the subsequent rolling process is ensured; by controlling the total furnace time, the elements such as C, Mn, and Mo are effectively promoted to fully diffuse, and the plate shape of the rolled steel plate is ensured to be good.

[0022] 3) A two-stage controlled rolling process is adopted. By controlling the final rolling temperature in the rough rolling stage, the intermediate billet is always kept in the austenite recrystallization temperature range during the warming process to ensure the uniformity of the structure. By limiting the reduction rate and thickness of the intermediate billet in the two-stage rolling process, the uniformity of the structure in the thickness direction of the rolled steel plate is ensured. During the warming process of the intermediate billet, water is sprayed to remove scales to inhibit the growth of austenite grains. At the same time, a temperature gradient is generated on the inner and outer surfaces of the billet, which promotes the penetration of rolling deformation to the center of the thickness and refines the grains at 1 / 2 of the thickness, which is beneficial to improve the core structure of thick-gauge steel plates. Slow rolling is adopted to increase the deformation penetration of the core of the steel plate. Through post-rolling relaxation, a large amount of Ti and Nb carbides are ensured to precipitate, increase the nucleation position of ferrite, effectively improve the yield strength of the steel plate, and improve toughness. By controlling the cooling temperature, the amount of ferrite first precipitated in the structure is ensured, and the plastic toughness of the core of the steel plate is ensured. By optimizing the straightening process, the internal stress is fully released, and the appropriate roll gap, bending roll amount and tilting value are set to ensure the good straightness of the straightened plate.

[0023] 4) The steel plate adopts the stacking slow cooling process, and the slow cooling time and temperature are limited. The upper part of the slow cooling tank is insulated with asbestos to accelerate the diffusion of C and Mn elements in the core of the steel plate, inhibit segregation, and improve the toughness at 1 / 2 of the thickness.

[0024] 5) A secondary quenching process is adopted. The second low-temperature quenching is adopted to inhibit the growth of austenite after re-nucleation, refine the original austenite grains, and increase the density of large-angle grain boundaries to ensure the core performance; a large cooling rate is adopted in the high-pressure area to promote the steel plate to quickly break through the film boiling area for rapid cooling, and then a small cooling rate is adopted to promote the surface temperature to the core temperature to gradually decrease. On this basis, quenching is performed to 300-350°C to ensure that the quenched steel plate is fully hardened, while also reducing the stress of the steel plate during the quenching process to ensure the shape of the steel plate; and quenching to 300-350°C can also use the low-temperature self-tempering effect of the steel plate to improve the internal strength and toughness, cancel the subsequent offline tempering process, and reduce the production cost; in addition, the upper and lower header water ratio, cooling rate and roller speed are controlled during the quenching process of the steel plate to ensure the uniformity of the upper and lower surface temperatures during the quenching process of the steel plate. After quenching, the steel plate does not need subsequent offline tempering and straightening treatment to meet the plate shape control requirements (straightness is below 3mm / 2m).

[0025] The mechanical properties of the steel plate produced by the present invention are as follows: yield strength ≥1120MPa, tensile strength ≥1400MPa, elongation ≥12%, Z-direction cross-sectional shrinkage ≥50%, and transverse Charpy impact energy at -40°C at 1 / 2 ≥100J. DETAILED DESCRIPTION

[0026] The invention discloses a manufacturing method for improving the strength and toughness of a 1100MPa grade engineering structure steel extra-thick plate. The chemical composition of the steel plate comprises, by weight percentage, C 0.16% to 0.19%, Si 0.2% to 0.35%, Mn 1.05% to 1.35%, P≤0.02%, S≤0.005%, Nb 0.010% to 0.040%, Ti 0.010% to 0.025%, Mo 0.5% to 0.8%, Als 0.02% to 0.05%, B 0.0008% to 0.0018%, Cr 0.35% to 0.5%, Ni 0.3% to 0.5%, Ceq 0.57%~0.65%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, the balance is Fe and unavoidable impurities, and the total amount of impurity elements is less than 0.05%.

[0027] The functions of the main elements in the steel plate are as follows:

[0028] C: Carbon is an important alloying element to ensure the hardenability of steel plates, and is also an important factor in determining carbon equivalent, which has a great influence on the strength, toughness, plasticity and weldability of steel. Too high carbon content affects the welding performance of steel plates. Too low carbon content affects the overall strength of steel plates. Under the premise of ensuring the required strength of steel plates, the present invention controls the carbon content to be in the range of 0.16% to 0.19%.

[0029] Si: an essential element for deoxidation, having a certain solid solution strengthening effect. Too high a content of Si will affect the toughness of steel, the uniformity of performance of extra thick plates and weldability. In the present invention, the silicon content is controlled within the range of 0.2% to 0.35%.

[0030] Mn: An important solid solution strengthening element in steel, which can reduce the phase transition temperature, refine the microstructure, strengthen the steel plate and improve the toughness, and at the same time improve the hardenability. Too high manganese content will cause segregation, which is not good for welding and toughness. The present invention controls the manganese content in the range of 1.05% to 1.35%.

[0031] Ni: can improve the low temperature toughness of steel and improve plasticity. For extra thick plates, it can improve the low temperature impact performance at 1 / 4 and 1 / 2 of the thickness, and is an indispensable alloy element; Ni can also delay pearlite transformation, promote the formation of medium temperature transformation structure, and reduce the cooling rate limit of thick specification steel plates; but the price of nickel is relatively high, so the present invention controls the Ni content to 0.3% to 0.5%.

[0032] Cr: can increase the hardenability of steel, refine the structure, and reduce the ductile-brittle transition temperature; the combination of chromium and manganese can improve the hardenability of steel and improve the mechanical properties of steel; chromium has a smaller segregation tendency than manganese, and replacing part of manganese with chromium can reduce the segregation in the core of the steel plate, improve the internal quality of the steel plate, and improve the uniformity of the mechanical properties; the present invention controls the chromium content range to 0.35% to 0.5%.

[0033] Mo: can significantly increase the hardenability and hardenability of steel, refine the microstructure of steel after quenching, and improve toughness. However, since molybdenum is a precious alloy, in order to reduce production costs, under the premise of ensuring performance, less or no molybdenum can be added according to the actual thickness of the steel plate. The present invention controls the molybdenum content range to 0.50% to 0.80%.

[0034] Nb: It is one of the commonly used elements in modern microalloyed steels, and has good fine grain strengthening and precipitation strengthening effects; it also delays austenite recrystallization; but excessive Nb will increase production costs and the difficulty of continuous casting process control. The present invention controls the Nb content range to 0.01% to 0.04%, and with a reasonable TMCP process, a uniform composite phase dominated by acicular ferrite structure can be obtained, so that the steel plate has good toughness.

[0035] Ti: It is a strong N-fixing element and exists in the form of TiN in the continuous casting billet. Fine TiN particles can effectively inhibit the growth of austenite grains during the reheating of the continuous casting billet, and help to increase the solid solubility of Nb in austenite and improve the impact toughness of the welding heat affected zone. When the Ti addition exceeds a certain value, the TiN particles will coarsen, increasing the stress concentration level between the particle interface and the matrix. Therefore, the present invention controls the Ti content range to be 0.01% to 0.025%.

[0036] B: An element that is effective in improving the hardenability of steel. It is very easy to segregate at the grain boundary to prevent carbon precipitation. A trace amount of boron can play a significant role. However, if the boron content is too high, it will easily form boron carbonitride, reduce toughness and cause hot brittleness. The present invention controls its content range to 0.0008% to 0.0018%.

[0037] Als: Usually used as a deoxidizer in steel, it can also refine the structure if AlN is formed. When the Al content exceeds 0.05%, excessive aluminum oxide inclusions will reduce the cleanliness of the steel. If the Al content is too low, deoxidation is insufficient, and easily oxidizable elements such as Ti will form oxides. Therefore, the present invention sets the lower limit of the Als content to 0.02%.

[0038] P and S: are inevitable impurity elements in steel. Too high P and S will affect the toughness and welding performance of the steel plate, so the lower the better. However, considering the cost of smelting process, it cannot be unlimitedly low. Therefore, the present invention sets the upper limit of P and S content to 0.02% and 0.005% respectively.

[0039] Mo, Ni and Cr all have a strengthening effect, increase the stability of austenite, and are beneficial to improving hardenability. In view of the fact that the present invention adopts a medium C design, the carbon equivalent Ceq is controlled at 0.57% to 0.65%, which can not only ensure the toughness of the steel plate, but also make the steel plate have suitable weldability.

[0040] The present invention discloses a manufacturing method for improving the toughness of a 1100MPa grade engineering structure steel extra-thick plate. The production process of the steel plate includes molten steel smelting → refining outside the furnace + RH vacuum degassing → micro-Ti treatment → B alloying → continuous casting → heating and slow cooling of the ingot into the pit → reheating of the ingot → controlled rolling and cooling → hot straightening → stacking and slow cooling of the steel plate → quenching and the like. The details are as follows:

[0041] 1) Steelmaking, continuous casting and slow cooling of ingot stacking;

[0042] According to the set chemical composition, the raw materials are pre-treated by KR molten iron to control the S content below 0.015%, and then enter the converter after slag removal; the converter smelting adopts double slag method to remove P, control the P content ≤ 0.02%, and the C content is controlled at 0.16% to 0.19% at the end of converter smelting. Argon is blown for 20 to 35 minutes when the converter is tapped. Argon blowing before continuous casting can promote the removal of inclusions in molten steel and improve the uniformity of molten steel composition.

[0043] Subsequently, LF refining and RH vacuum degassing are carried out, and the RH vacuum degassing is maintained for more than 20 minutes. After the degassing treatment is completed, sufficient Al is added according to the Als requirements. After adding sufficient Ti-Fe for micro-titanium treatment, B-Fe alloy is added for B alloying treatment. When adding materials, ensure that they are added into the molten steel to avoid floating on the slag layer.

[0044] During continuous casting of slabs, the continuous casting superheat is controlled at 15-25℃, and the continuous casting billet drawing rate is 0.8-1.3m / min; controlling the pouring superheat and the continuous casting billet drawing speed can effectively reduce the quality defects on the surface and corners of the billet. The electromagnetic stirring current intensity of the secondary cooling zone in the continuous casting stage is controlled to be 200-250A, and the secondary cooling water volume is controlled to be 1.3-2.0L / kg to reduce the average carbon segregation index and inhibit segregation; at the same time, the secondary cooling intensity is limited to inhibit the trend of the central crack of the billet to worsen. In the horizontal sector section, that is, the end of solidification, the continuous casting billet is pressed down by 30-45mm; putting it under heavy pressure helps to reduce billet segregation, refine austenite grains, and reduce internal structural defects.

[0045] After the ingot comes off the production line, it enters the pit for slow cooling. The temperature entering the pit is not less than 600℃, the slow cooling temperature is 600-650℃, the slow cooling time is 24-36h, and then it is cooled to below 200℃ in the slow cooling pit before leaving the pit. Slow cooling in the slow cooling pit helps to reduce the center segregation of the ingot and ensure the core performance of the steel plate after rolling.

[0046] 2) Reheating of ingot;

[0047] The ingot (thickness of 300-360mm) is sent into the walking beam heating furnace for heating. The temperature range of the preheating section is 900-1050℃, which promotes the rapid and full solid dissolution of Ti and Nb carbides in the matrix and full diffusion; the temperature range of the soaking section and the heating section is 1205-1230℃, the total heating time of the soaking section and the heating section is 4.5-6 hours, and the total furnace time is 6.5-8 hours; the upper and lower burner openings of the heating furnace are adjusted, the air-fuel ratio is controlled at 1:1.9-1:2.3, and the temperature difference between the upper and lower surfaces of the ingot is controlled within 15℃. The high heating temperature is adopted, and the furnace time of the soaking section and the heating section is ensured at the same time, in order to shorten the temperature difference between the surface and the core of the continuous casting ingot, improve the uniformity of the metal flow in the transverse and longitudinal directions on the surface of the steel plate, and ensure the shape of the rolled steel plate. Increasing the total furnace time is to promote the full diffusion of elements such as C, Mn, and Mo, and ensure the uniformity of the organization of the hot-rolled steel plate.

[0048] 3) Control rolling and cooling;

[0049] Rolling is divided into two stages: the first stage is recrystallization rolling (rough rolling), the rough rolling start temperature is ≥1120℃, the rough rolling final rolling temperature is 980~1025℃, the rough rolling is not more than 6 passes, and the pass reduction system is that at least the first 2 passes ensure that the reduction rate is above 15%; the thickness of the intermediate billet obtained is 2.5~3.5 times the thickness of the finished steel plate. During the intermediate billet waiting for temperature, 2 passes of descaling water are sprayed, each descaling time is 1~2min, and the descaling water pressure is 15~20MPa; the purpose is to inhibit the growth of austenite grains, and at the same time generate a temperature gradient on the inner and outer surfaces of the billet, promote the penetration of rolling deformation to the thickness center, refine the grains at 1 / 2 of the thickness, and help improve the core structure of thick specification steel plates.

[0050] The second stage is non-recrystallization rolling (finishing rolling), the starting temperature range of finishing rolling is 860-920℃, the final rolling temperature range of finishing rolling is 830-860℃, the finishing rolling is no more than 6 passes, and the pass reduction system is to ensure that the reduction rate is above 20% for at least the first two passes; by controlling the final rolling temperature of the rough rolling stage, the intermediate billet is in the austenite recrystallization temperature range during the waiting process to ensure the uniformity of the structure; the reduction rate of the two-stage rolling is limited to ensure the uniformity of the structure in the thickness direction of the steel plate after rolling. Slow rolling is adopted in the finishing rolling stage, with a rolling speed of 1-2m / s, and the steel is quickly cast after rolling, with a casting speed of 5-6.5m / s, and the steel is relaxed before controlled cooling. Slow rolling is adopted to increase the deformation penetration of the core of the steel plate, and the relaxation after rolling is to ensure the precipitation of a large amount of Ti and Nb carbides, increase the ferrite nucleation position, effectively improve the yield strength of the steel plate, and improve the toughness.

[0051] After relaxation, the steel plate is directly cooled, the start cooling temperature is 700-710℃, the final cooling temperature range is 380-450℃, and the cooling rate is controlled at 45-65℃ / s. The straightening temperature of hot straightening is 650-700℃, the straightening force is between 3000-4500kN, the bending roll amount is set at 1-1.6mm, and the tilting value is set at 3.5-5.5mm; by controlling the start cooling temperature, the amount of ferrite in the organization is guaranteed, the plastic toughness of the core of the steel plate is guaranteed, and the straightening process is optimized to promote the full release of internal stress; by setting the appropriate roll gap, bending roll amount and tilting value, the straightness of the straightened plate is guaranteed.

[0052] 4) Slow cooling of stacking;

[0053] After hot straightening, the steel plate is immediately placed in the slow cooling tank. The temperature entering the tank is not less than 500℃ and the slow cooling time is not less than 36h. The upper part of the slow cooling tank is insulated with asbestos to accelerate the diffusion of C and Mn elements in the core of the steel plate, inhibit segregation, and improve the toughness at 1 / 2 of the thickness.

[0054] 5) Quenching;

[0055] The first high-temperature quenching temperature is 880-910°C, and the furnace time is 1.6-2.0 min / mm. The second low-temperature quenching temperature is 770-820°C, and the furnace time is 1.1-1.5 min / mm. During the two quenching processes, the swing time of the steel plate in the high-pressure area is 1-1.5 min / mm, and the cooling rate is 50-65°C / s; the swing time of the steel plate in the low-pressure area is 2.0-2.5 min / mm, and the cooling rate is 25-35°C / s. During the two quenching processes, the upper and lower header water ratio is 1.6-2.2, the quenching machine roller speed is 1.2-2.0 m / s, and the quenching end temperature is 300-350°C. The second quenching adopts low-temperature quenching, which inhibits the growth of austenite after re-nucleation, refines the original austenite grains, and increases the density of large-angle grain boundaries to ensure the core performance; a large cooling rate is used in the high-pressure zone to promote the steel plate to quickly break through the film boiling zone for rapid cooling, and then a small cooling rate is used to promote the gradual decrease of the surface temperature to the core temperature. On this basis, quenching is carried out to 300-350°C. While ensuring that the quenched steel plate is fully hardened, it also reduces the stress level of the steel plate during the quenching process to ensure the shape of the steel plate; the purpose of quenching to 300-350°C is to utilize the low-temperature self-tempering effect of the steel plate, improve the internal strength and toughness, omit the subsequent offline tempering process, and reduce production costs.

[0056] The present invention optimizes the process of continuous casting, heating, rolling, controlled cooling and heat treatment, and finally prepares a 1100MPa-grade extra-thick plate for engineering structure with a thickness of 60-100mm, solves the problem of poor low-temperature impact toughness of the core of the steel plate of this steel grade and specification, and can meet the plate shape control requirements (straightness is below 3mm / 2m) without subsequent offline flattening and straightening treatment. The mechanical properties of the steel plate are as follows: yield strength ≥1120MPa, tensile strength ≥1400MPa, elongation ≥12%, Z-direction section shrinkage ≥50%, and transverse Charpy impact energy at -40°C at 1 / 2 thickness ≥100J.

[0057] In order to more intuitively embody the present invention, the embodiments of the present invention are further described in conjunction with examples. The following examples are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any technical solution that can be obviously obtained by a person skilled in the art within the technical scope disclosed in the present invention, including simple changes or equivalent replacements, is within the protection scope of the present invention. Example

[0058] Table 1 shows the chemical composition of the steel in each embodiment, Table 2 shows the process parameters of smelting molten steel to stacking and slow cooling in each embodiment, Table 3 shows the heating process parameters of the ingot in each embodiment, Table 4 shows the rolling process parameters of the steel plate in each embodiment, Table 5 shows the controlled cooling and slow cooling process parameters of the steel plate in each embodiment, Table 6 shows the heat treatment process parameters of the steel plate in each embodiment, and Table 7 shows the main performances and quality indicators of the steel plate in each embodiment.

[0059] Table 1 Chemical composition of steel (wt, %)

[0060] Example C Si Mn Mo Als B Ti Nb Ni Cr Ceq 1 0.17 0.26 1.21 0.56 0.033 0.0012 0.018 0.025 0.42 0.39 0.590 2 0.18 0.32 1.19 0.65 0.045 0.0008 0.021 0.034 0.39 0.42 0.618 3 0.16 0.28 1.33 0.71 0.025 0.0015 0.023 0.015 0.36 0.49 0.646 4 0.19 0.34 1.09 0.75 0.037 0.0010 0.019 0.036 0.49 0.38 0.630 5 0.17 0.23 1.26 0.62 0.044 0.0013 0.015 0.029 0.38 0.47 0.623 6 0.18 0.22 1.16 0.52 0.036 0.0009 0.017 0.026 0.32 0.37 0.572

[0061] Note: Impurity elements in steel: P≤0.02%, S≤0.005%.

[0062] Table 2 Process parameters for slow cooling from molten steel smelting to stacking

[0063] Example Argon blowing time / min RH vacuum degassing time / min Superheat / ℃ <![CDATA[Drawing speed / (m·min -1 )]]> Electromagnetic stirring current intensity / A Continuous casting billet reduction / mm Secondary cooling water volume / L / kg Pit entry temperature / ℃ Slow cooling temperature / ℃ Slow cooling time / h Outlet temperature / ℃ 1 22 23 17 0.9 220 36 1.6 620 630 32 180 2 25 25 23 1.3 240 33 2.0 635 650 26 150 3 26 27 25 1.2 210 39 1.5 622 640 30 155 4 32 22 21 1.1 250 40 1.8 605 635 35 170 5 20 23 22 1.1 235 42 1.3 640 650 25 180 6 27 28 20 1.0 225 38 1.7 630 645 29 190

[0064] Table 3 Heating process parameters of ingot

[0065] Table 4 Rolling process parameters of steel plates

[0066] Example Rough rolling start temperature / ℃ Rough rolling and final rolling temperature / ℃ Rough rolling pass Rough rolling first pass reduction rate / % Second pass reduction rate of rough rolling / % Finish rolling start temperature / ℃ Finish rolling temperature / ℃ Finishing rolling pass Finish rolling first pass reduction rate / % Second pass reduction rate in the stage / % Spray two times of descaling water time / min Two-pass descaling water pressure / MPa Intermediate billet thickness / mm Rolling speed / m / s Throwing speed / m / s 1 1130 1012 5 18 20 910 840 6 22 23 1、1.5 18、20 180 1.5 5.9 2 1125 1015 6 16 19 900 850 5 22 24 1.2、1.8 15、18 250 1.2 5.1 3 1120 1020 4 21 22 920 860 6 22 24 1.3、2.0 16、18 210 1.4 6.5 4 1125 1025 5 16 18 880 830 5 22 23 1.2、1.8 15、18 200 1.7 6.2 5 1135 1015 4 16 18 900 840 6 23 25 1.7、1.9 16、20 250 1.2 5.2 6 1130 995 5 17 16 890 845 5 22 25 1.2、1.6 18、20 220 1.3 5.7

[0067] Table 5 Controlled cooling and slow cooling process parameters of steel plate

[0068] Example Cooling temperature / ℃ Final cooling temperature / ℃ Cooling speed / ℃ Heat correction temperature / ℃ Straightening force / kN Roll bending amount / mm Tilt value / mm Stacking temperature / ℃ Stacking time / h 1 710 390 50 700 3200 1.2 3.6 500 50 2 705 430 55 685 4100 1.6 5.5 520 52 3 708 428 60 690 4500 1.4 4.8 530 38 4 710 445 48 680 3350 1.5 4.5 550 45 5 706 385 58 675 3600 1.5 3.8 525 42 6 710 430 63 695 4400 1.3 5.2 570 48

[0069] Table 6 Heat treatment process parameters of steel plate

[0070] Example First quenching temperature / ℃ First time in the furnace / min / mm Second quenching temperature / ℃ Second time in the furnace / min / mm High pressure area swing time / min / mm Cooling speed / ℃ / s Low pressure area swing time / min / mm Cooling speed / ℃ / s Roller speed / m / s Water ratio Quenching end temperature / ℃ 1 910 1.8 780 1.3 1.3 50 2.4 28 1.2 1.68 330 2 880 1.9 775 1.2 1.5 60 2.2 30 2.0 2.14 350 3 890 1.7 790 1.5 1.1 55 2.5 33 1.7 1.78 320 4 900 2.0 820 1.1 1.3 63 2.1 32 1.6 1.86 335 5 910 1.6 785 1.4 1.2 60 2.3 35 1.8 1.90 340 6 895 1.8 780 1.5 1.5 65 2.2 29 2.0 1.62 350

[0071] Table 7 Main properties and quality indicators of steel plates

[0072] Example Finished product thickness / mm Yield strength / MPa Tensile strength / MPa Elongation / % Z-axis section shrinkage / % -40℃ KV2 average value / J Straightness / mm / 2m 1 60 1135 1486 14 56 115 2 2 100 1160 1473 16 60 120 3 3 70 1182 1480 17 55 105 1 4 65 1156 1475 16 53 110 2 5 90 1148 1480 14 60 103 2 6 75 1139 1460 13 65 125 1

[0073] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for improving the toughness of 1100MPa grade engineering structure steel extra thick plate, characterized in that: Including chemical composition control and production process control; the chemical composition of the steel plate includes by weight percentage: C 0.16%~0.19%, Si0.2%~0.35%, Mn 1.05%~1.35%, P≤0.02%, S≤0.005%, Nb 0.010%~0.040%, Ti 0.010%~0.025%, Mo 0.5%~0.8%, Als 0.02%~0.05%, B 0.0008%~0.0018%, Cr 0.35%~0.5%, Ni0.3%~0.5%, Ceq 0.57%~0.65%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, the remainder is Fe and unavoidable impurities, and the total amount of impurity elements is less than 0.05%; the production process of steel plate includes molten steel smelting, refining outside the furnace + RH vacuum degassing, micro Ti treatment, B alloying, continuous casting, heating and slow cooling of ingot into the pit, ingot reheating, controlled rolling and cooling, hot straightening, slow cooling and quenching of steel plate stacking; the details are as follows: 1) Molten steel is smelted until the ingot is heated and slowly cooled; The raw materials are pretreated with KR molten iron to control the S content ≤ 0.015%; the P content is controlled to be ≤ 0.02% in converter smelting, and the C content is controlled to be within the range of 0.16% to 0.19% at the converter smelting end point. Argon is blown for 20 to 35 minutes when the converter is tapped; RH vacuum degassing is maintained for more than 20 minutes after LF refining, and then Al is added; Ti-Fe is added for micro-titanium treatment, and B-Fe alloy is added for B alloying; the superheat is controlled to be 15 to 25 during slab continuous casting ℃, the continuous casting billet drawing rate is 0.8~1.3m / min; the electromagnetic stirring current intensity in the secondary cooling zone is 200~250A, the secondary cooling water volume is 1.3~2.0L / kg, and the billet is pressed down by 30~45mm under heavy pressure at the horizontal fan-shaped section, i.e. the end of solidification; the billet is put into the pit for slow cooling after it comes off the line, the pit temperature is not less than 600℃, the slow cooling temperature is 600~650℃, the slow cooling time is 24~36h, and the billet is cooled down to below 200℃ in the pit before leaving the pit; 2) Reheating of the ingot: the temperature of the preheating section is 900-1050°C, the temperature of the soaking section and the heating section are both 1205-1230°C, the total heating time of the soaking section and the heating section is 4.5-6h, the total time in the furnace is 6.5-8h, the air-fuel ratio is controlled at 1:1.9-1:2.3, and the temperature difference between the upper and lower surfaces of the ingot is controlled within 15°C; 3) Control rolling, cooling and hot straightening; Rolling in two stages; Rough rolling start temperature ≥ 1120℃, rough rolling final rolling temperature 980~1025℃, rough rolling no more than 6 passes, at least the first 2 passes reduction rate is above 15%; Spray descaling water 2 times during the intermediate billet waiting for temperature, the descaling time for each pass is 1~2min, and the descaling water pressure is 15~20MPa; Finish rolling start temperature is 860~920℃, finish rolling final rolling temperature is 830~860℃, finish rolling no more than 6 passes, at least the first 2 The reduction rate of each pass is above 20%; the finishing rolling speed is 1-2m / s, and the steel throwing speed is 5-6.5m / s; the steel plate is cooled directly after the relaxation before temperature relaxation, the start cooling temperature is 700-710℃, the final cooling temperature is 380-450℃, and the cooling speed is controlled at 45-65℃ / s; the hot straightening temperature is 650-700℃, the straightening force is 3000-4500kN, the bending roll amount is set to 1-1.6mm, and the tilting value is set to 3.5-5.5mm; 4) Slow cooling of steel plate stacking; immediately after hot straightening, put the steel plate into the slow cooling tank, the temperature of the tank shall not be lower than 500℃, the slow cooling time shall not be less than 36h, and the upper part of the slow cooling tank shall be insulated with asbestos; 5) Quenching; The first high-temperature quenching temperature is 880-910°C, and the time in the furnace is 1.6-2.0 min / mm; the second low-temperature quenching temperature is 770-820°C, and the time in the furnace is 1.1-1.5 min / mm; during the two quenching processes, the swing time of the steel plate in the high-pressure area is controlled to be 1-1.5 min / mm, and the cooling rate is 50-65°C / s; the swing time of the steel plate in the low-pressure area is controlled to be 2.0-2.5 min / mm, and the cooling rate is 25-35°C / s; during the two steel plate quenching processes, the upper and lower manifold water ratio is 1.6-2.2, the quenching machine roller speed is 1.2-2.0 m / s, and the quenching end temperature is 300-350°C, at which temperature the steel plate achieves low-temperature self-tempering.

2. A method for improving the toughness of 1100MPa grade engineering structure steel extra thick plate according to claim 1, characterized in that: The thickness of the finished steel plate is 60 to 100 mm.

3. The manufacturing method for improving the toughness of 1100MPa grade engineering structure steel extra thick plate according to claim 1, characterized in that: The thickness of the cast billet is 300-360 mm; the thickness of the intermediate billet is 2.5-3.5 times the thickness of the finished steel plate.

4. The method for improving the toughness of 1100MPa grade engineering structure steel extra thick plate according to claim 1, characterized in that: The mechanical properties of the finished steel plate are: yield strength ≥1120MPa, tensile strength ≥1400MPa, elongation ≥12%, Z-axis section shrinkage ≥50%, transverse Charpy impact energy at -40℃ at 1 / 2 thickness ≥100J; the straightness of the steel plate ≤3mm / 2m.