A plate shape control method for 235MPa thick steel plate with a thickness greater than 60mm
Through the casting billet heating, rolling, heat straightening and slow cooling processes, the 235MPa grade steel plate shape control problem with thickness greater than 60mm and width greater than 3000mm is solved, efficient production and cost savings of steel plates are achieved, and the straightness of finished steel plates is ensured. Spend.
Patent Information
- Application Number
- CN202210897293.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-07-28
AI Technical Summary
The 235MPa grade steel plate with a thickness greater than 60mm and a width greater than 3000mm is prone to poor plate shape during the production process, resulting in low pass rate at one time and high cost reduction rate, and difficult to effectively control. The existing technology cannot completely solve this problem.
The process of heating, rolling, heat straightening and slow cooling of steel plate stacking is adopted. The specific steps include heating the casting billet to 1235~1265℃, cooling in sections during rolling to control the rolling water volume, heat straightening and setting Appropriate straightening force and temperature, and finally perform asbestos insulation treatment in the cooled area to ensure the straightness of the steel plate.
The plate-shaped control of 235MPa grade steel plate with a thickness greater than 60mm is achieved without subsequent cold correction treatment, which improves the steel plate one-time pass rate, reduces production costs, and ensures that the straightness of the finished steel plate is below 5mm/2m.
Smart Images

Figure BDA0003769420760000061 
Figure BDA0003769420760000062 
Figure BDA0003769420760000071
Abstract
Description
Technical Field
[0001] The present invention relates to the field of steel plate production, and in particular to a plate shape control method for a steel plate with a thickness greater than 60 mm, a width greater than 3000 mm, and a yield strength of 235 MPa. Background Art
[0002] The yield strength of 235MPa grade steel plate belongs to the low-strength grade steel plate. The main chemical elements of this grade of steel are C, Si, Mn, Al, etc. In general, when a wide and thick plate mill with a width of more than 4m produces thin (less than 8mm) or thick (more than 60mm) steel plates of this grade, hard bending or poor plate shape is easy to occur during rolling, especially for steel plates with a thickness of more than 60mm and a width of more than 3000mm. The plate shape usually needs to be flattened by a flattening machine to save it. If it cannot be flattened, it has to be re-rolled, which wastes raw materials, affects production efficiency, increases production costs, and seriously affects the one-time pass rate of steel plates. At the same time, due to the limitation of the protection parameters set by the straightening machine, the straightening roller is prone to disconnection or unsatisfactory straightening effect during steel plate straightening, resulting in excessive unevenness of the steel plate. The above reasons have led to a significant increase in the manufacturing cost of this type of extra-thick steel plate and extended the delivery cycle.
[0003] It can be seen that how to solve the plate shape problem of the above-mentioned steel plates with a thickness of more than 60mm, a width greater than 3000mm, and a yield strength of 235MPa, and improve the one-time pass rate of the steel plates, is the key to the development and application of steel plates of this specification level.
[0004] So far, there has been little research on the shape control of steel plates with a thickness greater than 60mm, a width greater than 3000mm, and a yield strength of 235MPa at home and abroad. The Chinese patent application with publication number CN103722023A discloses "a TMCP high-strength ship plate shape control method", which is effective for the shape control of high-strength ship plates after rolling. However, this method is applicable to steel plates with a thickness of 30-60mm, and does not involve the shape control of steel plates with a thickness of more than 60mm. The Chinese patent application with publication number CN101069896A discloses "a medium and thick plate shape control method", which can reduce the wave shape of 30mm thick steel plates after rolling. However, this method cannot completely eliminate the wave shape of the steel plate because there is no reduction in the last pass; and because the rolling mill only contacts the steel plate through the upper and lower rollers, when there is no reduction in the last pass, the shape defects such as warping caused by the previous rolling pass cannot be eliminated.
[0005] In the journal article "Optimization Control of Hot-Rolled Thin-Gauge Plate Production Process" (Henan Metallurgy, 2020.8), the problem of plate shape control of thin-gauge steel plates with a thickness of 6-10mm was solved by optimizing the heating, rolling and pressing procedures. However, this method cannot meet the plate shape control requirements of steel plates with a thickness of more than 60mm. Summary of the invention
[0006] The present invention provides a plate shape control method for 235MPa grade thick steel plates with a thickness greater than 60mm, which can meet the plate shape control requirements of the steel plates without subsequent cold straightening treatment, and solves the problems that wave shapes are very likely to occur in the production of such extra-thick steel plates, affecting the one-time pass rate and cost reduction rate of the steel plates.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for controlling the shape of a 235MPa thick steel plate with a thickness greater than 60mm, wherein the steel plate production process includes heating of the ingot, rolling, hot straightening, and slow cooling of the steel plate stacking; the specific steps are as follows:
[0009] 1) Billet heating: heat the billet to 1235-1265°C, the total heating time of the soaking section and the heating section is 4.5-5.5h, and the total time in the furnace is 6.5-7h; ensure that the temperature difference between the upper and lower surfaces of the billet after heating is less than 30°C;
[0010] 2) Rolling: The roller cooling water volume from the rolling mill to the pre-straightening machine is 150-200m 3 / h; During the rolling stage, the rollers are cooled in sections. When rolling the 1 / 6L length section of the billet head, the roller cooling water is not turned on; when rolling the 1 / 6L length section of the billet tail, the roller cooling water volume is controlled at 35-50m 3 / h; when rolling the remaining length of the middle section of the billet, the water volume of the roll is controlled at 50~80m 3 / h; where L is the length of the billet in the rolling direction during each rolling pass; during rolling, at least the first three passes use a large reduction rate, and the reduction rate of each pass is not less than 15%, and at least the last three passes use a small reduction rate, and the reduction rate of each pass is controlled at 1% to 1.5%; the sled plate coefficient SKI value of the rolling mill is controlled in the rolling widening stage, and the SKI value is set to +4 to +8; the final rolling temperature of the steel plate is 850 to 930°C; the billet bite speed is 2 to 3m / s;
[0011] 3) Hot straightening; the roll gap tilt value is set to 8-12mm; the lead-in roll position is -2.1-2.5mm, the lead-out roll position is -4.1-4.9mm, the final straightening temperature is not more than 600℃, and the straightening force is 8000-10000kN;
[0012] 4) Slow cooling of steel plate stacking: The hot straightened steel plates are immediately transported to the slow cooling area for stacking. The slow cooling rate of the steel plate stacking is 5-10℃ / h and the time is 24-48h.
[0013] The chemical composition of the steel plate is as follows by weight percentage: 0.12%≤C≤0.18%, Si≤0.35%, Mn0.75%~0.95%, P≤0.035%, S≤0.035%, Al 0.015%~0.045%, Ceq≤0.4% and Ceq=C+Mn / 6, the remainder is Fe and unavoidable impurities, O≤0.0050% among the impurities, and the total amount of other impurities is less than 0.05%.
[0014] The steel plate has a width greater than 3000 mm and is obtained by rolling a cast billet with a thickness of 250 to 360 mm through a medium and thick plate reciprocating rolling mill.
[0015] In the step 2), before rolling, high-pressure water is used to descale the ingot after it leaves the heating furnace. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa.
[0016] The straightness of the finished steel plate is below 5mm / 2m.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1) Use a higher heating temperature and ensure that the soaking section and the heating section are in the furnace for a certain time, so that the temperature difference between the upper and lower surfaces of the ingot after heating is controlled within 30°C, which reduces the temperature difference between the surface and the core of the ingot and improves the uniformity of the metal flow in the horizontal and vertical directions on the surface of the steel plate; control the total time in the furnace, thereby effectively inhibiting the excessive growth of austenite grains and ensuring the performance of the steel plate.
[0019] 2) Control the cooling water flow of the roller table, and adopt a segmented cooling process for the rollers to avoid a large amount of cooling water flowing on the surface of the steel plate, which will cause uncontrolled temperature drop on the surface of the steel plate, thereby increasing the number of rolling passes; Reasonably control the cooling water volume of the rollers, effectively control the roller shape, and greatly improve the problems of irregular deviation and sickle bending during the rolling process due to uneven temperature distribution of the head, middle and tail of the steel billet; At the same time, optimize the pass reduction at different stages of rolling, and control the final rolling temperature and rolling speed, effectively ensure the initial plate shape of the rolled steel plate, and reduce the internal stress of the steel plate; In addition, limit the SKI value of the rolling mill sled plate coefficient, the billet bite and the rolling speed in the rolling widening stage, so that the intermediate billet remains horizontal or slightly upturned, ensuring the initial plate shape of the rolled steel plate.
[0020] 3) Adopt three-pass hot straightening, semi-automatic straightening mode, manual input of steel plate thickness and other methods to realize inclined roller gap straightening. By setting the initial lead-in roller position, lead-out roller position, straightening temperature and pressure, the straightening steel plate is guaranteed to be straight and in good shape. At the same time, a lower final straightening temperature is set to reduce the temperature drop range of the steel plate during the cooling process, avoiding large internal stress due to phase change, which is beneficial to the control of the steel plate shape, reducing the probability of buckle head and buckle tail shape problems, and saving the subsequent cold straightening equipment investment cost.
[0021] 4) The hot straightened steel plates are immediately transported to the slow cooling area for stacking, and the steel plates are slowly cooled and insulated with asbestos. At the same time, the slow cooling temperature and stacking speed of the steel plates are strictly limited to ensure that the temperature drop of the steel plates tends to be consistent. At the same time, the phase change interval with large internal stress at 400°C is avoided to ensure that the final straightness of the finished steel plates meets the requirements below 5mm / 2m, saving the cost of subsequent flattening and straightening processes. DETAILED DESCRIPTION
[0022] The present invention discloses a method for controlling the shape of a 235MPa thick steel plate with a thickness greater than 60mm. The steel plate production process includes heating of the ingot, rolling, hot straightening, and slow cooling of the steel plate stacking. The specific steps are as follows:
[0023] 1) Billet heating: heat the billet to 1235-1265°C, the total heating time of the soaking section and the heating section is 4.5-5.5h, and the total time in the furnace is 6.5-7h; ensure that the temperature difference between the upper and lower surfaces of the billet after heating is less than 30°C;
[0024] 2) Rolling: The roller cooling water volume from the rolling mill to the pre-straightening machine is 150-200m 3 / h; During the rolling stage, the rollers are cooled in sections. When rolling the 1 / 6L length section of the billet head, the roller cooling water is not turned on; when rolling the 1 / 6L length section of the billet tail, the roller cooling water volume is controlled at 35-50m 3 / h; when rolling the remaining length of the middle section of the billet, the water volume of the roll is controlled at 50~80m 3 / h; where L is the length of the billet in the rolling direction during each rolling pass; during rolling, at least the first three passes use a large reduction rate, and the reduction rate of each pass is not less than 15%, and at least the last three passes use a small reduction rate, and the reduction rate of each pass is controlled at 1% to 1.5%; the sled plate coefficient SKI value of the rolling mill is controlled in the rolling widening stage, and the SKI value is set to +4 to +8; the final rolling temperature of the steel plate is 850 to 930°C; the billet bite speed is 2 to 3m / s;
[0025] 3) Hot straightening; the roll gap tilt value is set to 8-12mm; the lead-in roll position is -2.1-2.5mm, the lead-out roll position is -4.1-4.9mm, the final straightening temperature is not more than 600℃, and the straightening force is 8000-10000kN;
[0026] 4) Slow cooling of steel plate stacking: The hot straightened steel plates are immediately transported to the slow cooling area for stacking. The slow cooling rate of the steel plate stacking is 5-10℃ / h and the time is 24-48h.
[0027] The chemical composition of the steel plate is as follows by weight percentage: 0.12%≤C≤0.18%, Si≤0.35%, Mn0.75%~0.95%, P≤0.035%, S≤0.035%, Al 0.015%~0.045%, Ceq≤0.4% and Ceq=C+Mn / 6, the remainder is Fe and unavoidable impurities, O≤0.0050% among the impurities, and the total amount of other impurities is less than 0.05%.
[0028] The steel plate has a width greater than 3000 mm and is obtained by rolling a cast billet with a thickness of 250 to 360 mm through a medium and thick plate reciprocating rolling mill.
[0029] In the step 2), before rolling, high-pressure water is used to descale the ingot after it leaves the heating furnace. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa.
[0030] The straightness of the finished steel plate is below 5mm / 2m.
[0031] The working principle of the plate shape control method of a 235MPa grade thick steel plate with a thickness greater than 60mm described in the present invention is as follows:
[0032] 1. Billet heating process;
[0033] The ingot (thickness 250-360 mm, preferably continuous casting ingot) is fed into a walking beam heating furnace for heating, and the ingot is heated to 1235-1265°C. The total heating time in the soaking section and the heating section is 4.5-5.5 hours, and the total time in the furnace is 6.5-7 hours. A higher heating temperature is used to ensure that the temperature difference between the upper and lower surfaces of the ingot after heating is less than 30°C, shorten the temperature difference between the surface and the core of the ingot, and improve the uniformity of the lateral and longitudinal metal flow on the surface of the steel plate. The total time in the furnace is controlled to effectively inhibit the excessive growth of austenite grains and ensure the mechanical properties of the steel plate.
[0034] 2) High-pressure water descaling and rolling process;
[0035] Before rolling, high-pressure water is used to descale the ingot after leaving the heating furnace. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa. At the same time, the roller cooling water from the rolling mill to the pre-straightening section is reduced to 150 to 200 m 3 / h, to avoid a large amount of cooling water flowing under the steel plate surface to cause uncontrolled temperature drop on the steel plate surface, increase the rolling pass, and also help to control the intermediate billet to maintain a horizontal or slightly warped state.
[0036] During the rolling stage, the rollers are cooled in sections; when the length section is set at the head of the billet, the roller cooling water is not turned on; when the length section is set at the middle of the billet, the roller cooling water volume is set at 50-80m 3 / h; when rolling the tail of the billet to set the length, the roller cooling water volume is 35~50m 3 / h. By adjusting the amount of cooling water for the rolls, the roll shape can be effectively controlled, and the irregular deviation and sickle bend caused by the uneven temperature distribution of the head, middle and tail of the billet can be greatly improved. In addition, it is preferred to use a large reduction rate in the first three passes of rolling, with a reduction rate of not less than 15% for each pass, and the reduction rate in the last three passes of rolling is controlled at 1% to 1.5%; the first three passes of rolling should give full play to the capacity of the rolling mill and use a large reduction rate. In the last three passes, due to the increase in the deformation resistance of the steel plate due to temperature drop, a small reduction rate is used for rolling, which can flatten the shape of the steel plate and reduce the internal stress of the steel plate. Control the SKI value of the rolling mill sled coefficient in the rolling widening stage, set the SKI value to +4 to +8, so that the intermediate billet remains horizontal or slightly upturned, which is conducive to the rapid bite of the billet in the rolling stage. Control the final rolling temperature of the steel plate at 850 to 930 ° C. In order to ensure the shape of the steel plate after rolling, the billet bite speed is controlled at 2 to 3 m / s.
[0037] 3. Heat straightening process;
[0038] After rolling, the steel plate is subjected to three hot straightenings, and the semi-automatic straightening mode is adopted. The roll gap tilting value is set to 8-12mm; the position of the lead-in roll is -2.1-2.5mm, the position of the lead-out roll is -4.1-4.9mm, the final straightening temperature is not more than 600℃, and the straightening force is between 8000 and 10000kN. By setting the straightening mode, the appropriate roll gap, the straightening force and the number of straightening passes, the straightening steel plate is guaranteed to be straight and in good shape. At the same time, a lower final straightening temperature is set to reduce the temperature drop range of the steel plate during the cooling process, avoid the generation of large internal stress due to phase change, reduce the probability of buckle head and buckle tail problems of the steel plate, and save the subsequent cold straightening and flattening equipment investment costs.
[0039] 4. Steel plate stacking and slow cooling process;
[0040] The hot straightened steel plates are immediately transported to the slow cooling area for stacking. The temperature of the stacked steel plates should be greater than 450℃, and the number of stacked steel plates should be no less than 10. At the same time, the upper, lower and both sides of the stacked steel plates are insulated with asbestos. The steel plates are stacked for 24 to 48 hours, and then plasma cutting is performed. Since the cooling speeds of the lower surface, upper surface and both sides of thick-gauge steel plates are different, the use of steel plate stacking slow cooling and asbestos insulation can ensure that the temperature drop of the steel plates tends to be consistent, and at the same time avoid the phase change interval with large internal stress at 400℃, ensuring the final plate shape of the finished steel plate.
[0041] The present invention combines chemical composition with controlled rolling and controlled cooling technology to overcome the shortcomings of the prior art and solve the problem of plate shape control for steel plates with a thickness of more than 60 mm, a width of more than 3000 mm, and a yield strength of 235 MPa. The straightness of the finished steel plate is less than 5 mm / 2 m, meeting the technical requirements.
[0042] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.
[0043] [Example]
[0044] In this embodiment, Table 1 is the chemical composition of the steel plate, Table 2 is the heating system of the ingot and the high-pressure water descaling process parameters before rolling; Table 3 is the rolling process parameters of the steel plate; Table 4 is the hot straightening and slow cooling process parameters of the steel plate and the flatness of the finished steel plate.
[0045] Table 1 Chemical composition of steel plate (wt, %)
[0046] Example C Si Mn Al Ceq 1 0.13 0.33 0.95 0.016 0.289 2 0.14 0.27 0.82 0.035 0.276 3 0.18 0.25 0.88 0.040 0.326 4 0.12 0.26 0.93 0.043 0.345 5 0.16 0.35 0.76 0.026 0.286 6 0.17 0.28 0.79 0.015 0.301
[0047] Note: Impurity elements in steel are P≤0.035%, S≤0.035%; 0≤0.0050%, and the total amount of other impurity elements is less than 0.05%.
[0048] Table 2 Heating system of ingot and process parameters of high pressure water descaling before rolling
[0049]
[0050] Table 3 Rolling process parameters of steel plates
[0051]
[0052] Table 4 Hot straightening and slow cooling process parameters of steel plates and straightness of finished steel plates
[0053]
[0054] It can be seen that the method of the present invention solves the plate shape problem of producing hot-rolled steel plates with a thickness of more than 60 mm, a width of more than 3000 mm, and a yield strength of 235 MPa using 250-360 mm thick ingots, and the straightness of the steel plates meets the technical requirements of less than 5 mm / 2 m.
[0055] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for controlling the shape of a 235MPa thick steel plate with a thickness greater than 60mm, characterized in that: The chemical composition of the steel plate is calculated by weight percentage: 0.12%≤C≤0.18%, Si≤0.35%, Mn 0.75%~0.95%, P≤0.035%, S≤0.035%, Al 0.015%~0.045%, Ceq≤0.4% and Ceq=C+Mn / 6, the balance is Fe and unavoidable impurities, O≤0.0050% among the impurities, and the total amount of other impurities is less than 0.05%; the width of the steel plate is greater than 3000mm, and the steel plate is obtained by rolling the slab with a thickness of 250~360mm through a medium and thick plate reciprocating rolling mill, and the straightness of the finished steel plate is less than 5mm / 2m; the steel plate production process includes slab heating, rolling, hot straightening, and steel plate stacking and slow cooling; the specific steps are as follows: 1) Billet heating: heat the billet to 1235-1265°C, the total heating time of the soaking section and the heating section is 4.5-5.5h, the total time in the furnace is 6.5-7h, and the temperature difference between the upper and lower surfaces of the billet after heating is ensured to be less than 30°C; 2) Before rolling, high-pressure water is used to descale the ingot after leaving the heating furnace. The descaling time is 0.5 to 1 min, and the descaling machine pressure is 20 to 25 MPa; the roller cooling water volume from the rolling mill to the pre-straightening machine is 150 to 200 m 3 / h; During the rolling stage, the rollers are cooled in sections. When rolling the 1 / 6L length section of the billet head, the roller cooling water is not turned on; when rolling the 1 / 6L length section of the billet tail, the roller cooling water volume is controlled at 35-50m 3 / h; when rolling the remaining length of the middle section of the billet, the water volume of the roll is controlled at 50-80m 3 / h; where L is the length of the billet in the rolling direction during each rolling pass; during rolling, at least the first three passes use a large reduction rate, and the reduction rate of each pass is not less than 15%, and at least the last three passes use a small reduction rate, and the reduction rate of each pass is controlled at 1% to 1.5%; control the SKI value of the rolling mill sled coefficient during the rolling widening stage, and set the SKI value to +4 to +8; the final rolling temperature of the steel plate is 850 to 930°C; the billet bite speed is 2 to 3m / s; 3) Hot straightening: The roll gap tilt value is set to 8-12mm; the lead-in roll position is -2.1-2.5mm, the lead-out roll position is -4.1-4.9mm, the final straightening temperature is not more than 600℃, and the straightening force is 8000-10000KN; 4) Slow cooling of steel plate stacking: The hot straightened steel plates are immediately transported to the slow cooling area for stacking. The slow cooling rate is 5-10℃ / h and the time is 24-48h.