A method for recycling BN board
By coating the BN plate with carbon-containing slurry and performing high-temperature sintering, the YAG impurities are migrated to the surface layer, followed by thinning and grinding, which solves the problem of large grinding thickness of the BN plate in the existing technology, prolongs the life of the plate and improves the performance.
Patent Information
- Application Number
- CN202211003211.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-19
AI Technical Summary
In the existing technology, when processing used BN plates, it is necessary to grind 0.4 to 0.8 mm to remove YAG impurities on the surface, which leads to waste of resources and increased production costs, and affects the sintered appearance, thermal conductivity, and strength properties of the aluminum nitride substrate.
The used BN plate is coated with carbon-containing slurry (such as graphite slurry, carbon black slurry, activated carbon slurry, etc.), and after high-temperature sintering, the reaction between carbon and YAG is used to migrate impurities to the surface layer, and then is reduced. For thin grinding, impurities can be removed by grinding only 30~50um.
It effectively reduces the grinding thickness of the BN plate, extends its service life, improves the sintered appearance, thermal conductivity and strength performance of the aluminum nitride substrate, and reduces production costs.
Smart Images

Figure CN115351629B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramics, and in particular to a method for recycling a BN plate. Background Art
[0002] BN plates are usually used in the sintering process of aluminum nitride substrates to support the sintering process. Yttrium aluminum garnet (YAG) is produced during the sintering process of aluminum nitride. During the sintering process, a small amount of impurities such as yttrium aluminum garnet and aluminum oxide penetrate into the BN plate. At the same time, yttrium aluminum garnet also adsorbs a small amount of aluminum nitride on the surface of the BN plate, affecting the subsequent sintering appearance and thermal conductivity, strength and other properties of the aluminum nitride substrate. At the same time, it also greatly reduces the service life of the BN plate and increases the production cost.
[0003] The existing process usually directly uses grinding to polish the BN plate to remove YAG impurities on the surface, but grinding requires grinding 0.4 to 0.8 mm, which greatly affects the use of the BN plate and causes resource waste. Therefore, how to treat the used BN plate to remove the YAG on the surface so that it can continue to be used has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for recycling BN plates, which can effectively remove impurities. After treatment, the grinding thickness is greatly reduced (without treatment, 0.4 to 0.8 mm is required for grinding), so that it can continue to be used.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for recycling a BN plate comprises the following steps:
[0007] coating a carbon-containing slurry on a used BN plate;
[0008] Sintering the BN plate coated with the slurry;
[0009] After sintering, the BN plate is thinned to a thickness of 30 to 50 um.
[0010] The inventors of the present invention have found through extensive research that the used BN plates contain impurities on their surface, which affects their appearance and performance. As a result, their continued use will affect the sintering appearance, thermal conductivity, strength and other properties of the aluminum nitride substrate. Therefore, the BN plates need to be recycled.
[0011] The present invention can effectively remove impurities by coating a carbon-containing slurry on a used BN plate, sintering it, and grinding it after sintering. After the above treatment, the grinding thickness is greatly reduced (without treatment, 0.4 to 0.8 mm of grinding is required), so that it can continue to be used.
[0012] The inventors further explored its mechanism and found that under high temperature (sintering), YAG has a certain fluidity and migrates from areas with high concentration to areas with low concentration. The inventors used carbon to react with the YAG on the surface to promote the migration of the internal YAG to the surface. Only 30 to 50 um of grinding is required to remove impurities, thereby greatly improving the service life of the BN plate.
[0013] As a preferred embodiment of the present invention, the carbon-containing slurry includes at least one of graphite slurry, carbon black slurry, activated carbon slurry, carbon nanotube slurry, and graphene slurry.
[0014] The inventors explored a large number of carbon sources and found that the inorganic carbon source slurry described above can effectively react with YAG, thereby grinding it away. However, since the organic carbon source contains H and O, H and O need to be removed before sintering, which greatly increases the processing steps and increases the cost. Therefore, in the present invention, it is necessary to select inorganic carbon sources such as graphite, carbon black, activated carbon, carbon nanotubes, and graphene.
[0015] As a preferred embodiment of the present invention, the carbon-containing slurry includes at least one of graphite slurry, carbon black slurry, and activated carbon slurry.
[0016] As a preferred embodiment of the present invention, the carbonaceous slurry is graphite slurry.
[0017] As a preferred embodiment of the present invention, the mass concentration of the graphite slurry is 10-50%; the mass concentration of the carbon black slurry is 10-50%; the mass concentration of the activated carbon slurry is 10-50%; the mass concentration of the carbon nanotube slurry is 10-50%; and the mass concentration of the graphene slurry is 10-50%.
[0018] It should be noted that in the present invention, there is no particular limitation on the mass concentration of graphite slurry, carbon black slurry, activated carbon slurry, carbon nanotube slurry, and graphene slurry, as long as the migration of internal YAG to the surface is promoted.
[0019] That is, those skilled in the art can select a specific coating amount according to the mass concentration of graphite slurry, carbon black slurry, activated carbon slurry, carbon nanotube slurry, and graphene slurry, so as to achieve the effect of promoting the migration of internal YAG to the surface layer. When the mass concentration of the slurry is low, the coating amount can be increased (greater than 10 mg / cm2 ), when the slurry concentration is high, the coating amount can be appropriately reduced (greater than 10mg / cm 2 ).
[0020] As a preferred embodiment of the present invention, the coating amount of the carbon-containing slurry is ≥10 mg / cm 2 The inventors investigated the coating amount of carbon-containing slurry and found that the coating amount of carbon-containing slurry ≥ 10 mg / cm 2 When the coating amount is less than 10 mg / cm 2 When grinding 30-50 μm, the YAG impurities inside the BN plate are not completely removed. Therefore, in the present invention, the coating amount of the carbon-containing slurry needs to be strictly controlled.
[0021] As a preferred embodiment of the present invention, the BN plate is sintered in a nitrogen atmosphere. In the nitrogen atmosphere, the carbon and YAG react to form YN (sintered product), which can then be removed by grinding. The reaction equation is as follows:
[0022] C+N2+Y2O3·Al2O3→YN+AlN+CO.
[0023] As a preferred embodiment of the present invention, the BN plate is sintered in a graphite furnace. There are generally only two types of sintering furnaces, metal furnaces and graphite furnaces. When a metal furnace is used, H2 needs to be introduced to protect the heating element and the frame, and H2 will react with C, so sintering needs to be carried out in a graphite furnace.
[0024] As a preferred embodiment of the present invention, the sintering temperature is 1400-1900°C, preferably 1400-1700°C, and the sintering time is 4-8h. The present invention further investigates the influence of sintering temperature and time on the migration effect of YAG, and finds that if the sintering temperature is lower than 1400°C and / or the sintering time is lower than 4h, the impurities inside the BN plate cannot be well migrated, and impurities still exist after grinding 50um. If the sintering temperature is higher than 1900°C and / or the sintering time is higher than 8h, the energy consumption is too large, thereby increasing the processing cost.
[0025] As a preferred embodiment of the present invention, the thinning treatment is grinding with a grinding wheel.
[0026] As a preferred embodiment of the present invention, before sintering, the BN plates coated with the slurry are stacked. It should be noted that in the present invention, the BN plates coated with the slurry can be stacked and sintered, or can be sintered alone.
[0027] As a preferred embodiment of the present invention, the thinning thickness is 30 to 50 um.
[0028] The beneficial effects of the present invention are as follows: (1) the present invention can effectively remove impurities by coating a carbon-containing slurry on a used BN plate, sintering it, and grinding it after sintering. After treatment, the grinding thickness is greatly reduced (without treatment, 0.4 to 0.8 mm of grinding is required), so that it can continue to be used; (2) Under high temperature (sintering), YAG has a certain fluidity and there is a phenomenon of migration from a high concentration area to a low concentration area. The present invention utilizes the reaction of carbon with the YAG on the surface layer to promote the migration of the internal YAG to the surface layer. Only 30 to 50 um of grinding is required to remove impurities, thereby greatly improving the service life of the BN plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the BN board diagram used;
[0030] Figure 2 This is a picture of a BN plate treated after high temperature sintering in Example 1;
[0031] Figure 3 This is a picture of the BN plate after the grinding process in Example 1;
[0032] Figure 4 This is a stacking diagram of the BN plate of Example 2;
[0033] Figure 5 This is a picture of the BN plate after grinding treatment in Comparative Example 1;
[0034] Figure 6 This is a picture of the BN plate after grinding treatment in comparative example 3;
[0035] Figure 7 This is the BN plate image after grinding 50um in comparative example 4. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The reagents or instruments used in the present invention without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.
[0038] The used BN plates described in the present invention are all BN plates from the same batch used for sintering aluminum nitride substrates. Figure 1 As shown, there are a lot of impurities on the surface of the used BN plate.
[0039] Example 1
[0040] A method for recycling a BN plate comprises the following steps:
[0041] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 10 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 40% graphite powder, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0042] The BN plate coated with the slurry was placed in a graphite furnace and sintered in a nitrogen atmosphere at a sintering temperature of 1600°C for 6 hours. Figure 2 As shown, it can be seen that after sintering, a large amount of impurities migrate to the surface;
[0043] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 30 μm. Figure 3 As shown, it can be seen that after grinding 30um, there is no impurity on the surface and it can be used normally.
[0044] Example 2
[0045] A method for recycling a BN plate comprises the following steps:
[0046] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 10 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 40% graphite powder, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0047] The BN plates coated with the slurry were stacked, 50 layers / stack. The stacked BN plates were as follows: Figure 4 As shown, it was placed in a graphite furnace and sintered in a nitrogen atmosphere at a sintering temperature of 1600°C and a sintering time of 6 hours;
[0048] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0049] Example 3
[0050] A method for recycling a BN plate comprises the following steps:
[0051] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 15 mg / cm 2, the graphite slurry comprises the following components in percentage by mass: 40% graphite powder, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0052] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1600°C and a sintering time of 6 hours;
[0053] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0054] Example 4
[0055] A method for recycling a BN plate comprises the following steps:
[0056] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 20 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 40% graphite powder, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0057] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1600°C and a sintering time of 6 hours;
[0058] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0059] Example 5
[0060] A method for recycling a BN plate comprises the following steps:
[0061] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 15 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 40% graphite powder, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0062] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1400°C and a sintering time of 8 hours;
[0063] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0064] Example 6
[0065] A method for recycling a BN plate comprises the following steps:
[0066] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 15 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 40% graphite powder, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0067] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1700°C and a sintering time of 4 hours;
[0068] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0069] Example 7
[0070] A method for recycling a BN plate comprises the following steps:
[0071] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 20 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 10% graphite powder, 88% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0072] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1600°C and a sintering time of 6 hours;
[0073] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0074] Example 8
[0075] A method for recycling a BN plate comprises the following steps:
[0076] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 10 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 50% graphite powder, 48% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0077] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1600°C and a sintering time of 6 hours;
[0078] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0079] Example 9
[0080] A method for recycling a BN plate comprises the following steps:
[0081] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 10 mg / cm 2 , the graphite slurry includes the following components in percentage by mass: 40% activated carbon, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0082] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1600°C and a sintering time of 6 hours;
[0083] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0084] Example 10
[0085] A method for recycling a BN plate comprises the following steps:
[0086] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 10 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 40% carbon black, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0087] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1600°C and a sintering time of 6 hours;
[0088] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0089] Comparative Example 1
[0090] A method for recycling a BN plate comprises the following steps:
[0091] In the used BN board (such as Figure 1 ) is coated with graphite slurry, and the coating amount of the graphite slurry is 8 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 40% graphite powder, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0092] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1600°C and a sintering time of 6 hours;
[0093] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50 μm. Figure 5 As shown in the figure, due to the low coating amount of graphite slurry, there are still a lot of impurities on the surface after thinning by 50um.
[0094] Comparative Example 2
[0095] A method for recycling a BN plate comprises the following steps:
[0096] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 10 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 40% graphite powder, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0097] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1300°C and a sintering time of 6 hours;
[0098] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50um.
[0099] Comparative Example 3
[0100] A method for recycling a BN plate comprises the following steps:
[0101] In the used BN board (such as Figure 1 ) is coated with graphite slurry, wherein the coating amount of the graphite slurry is 10 mg / cm 2 , the graphite slurry comprises the following components in percentage by mass: 40% graphite powder, 58% anhydrous ethanol (solvent), and 2% polyvinyl butyral (dispersant);
[0102] The BN plates coated with the slurry were stacked, 50 layers / stack, placed in a graphite furnace, and sintered in a nitrogen atmosphere at a sintering temperature of 1700°C and a sintering time of 2h;
[0103] After sintering, the BN plate is ground and thinned with a grinding wheel to a thickness of 50 μm. Figure 6 As shown in the figure, due to the short sintering time, there are still a lot of impurities on the surface after thinning by 50um.
[0104] Comparative Example 4
[0105] Comparative Example 4 is a used BN plate (such as Figure 1 ), but without any treatment, after grinding 50um, such as Figure 7 As shown, there are still a lot of impurities on the surface.
[0106] Test Case
[0107] In the recycling methods described in Examples 1 to 10 and Comparative Examples 1 to 4, the coating slurry, coating amount, number of layers, sintering temperature, and sintering time are shown in Table 1, and the experimental results are shown in Table 2. In the table, YN is the sintering product, which is the product of the reaction between carbon and YAG.
[0108] Table 1
[0109]
[0110]
[0111] Table 2 Test results
[0112]
[0113] It can be seen from Table 1 that the BN plate recycling method of the present invention can effectively remove impurities and enable it to be reused after treatment.
[0114] By comparing Examples 1 to 10 with Comparative Example 4, it can be seen that after grinding 50 um, the untreated BN plate still has many impurities on the surface, while after the treatment of the present invention, the impurities are removed after grinding 50 um, the surface is smooth and can be reused.
[0115] Comparison of Example 2 and Comparative Example 1 shows that if the coating amount is less than 10 mg / m 2 If the coating amount is too low, the impurities cannot be completely migrated to the surface and removed. Therefore, the coating amount needs to be strictly controlled in the present invention.
[0116] By comparing Example 2 with Comparative Example 2, it can be seen that if the sintering temperature is too low, the fluidity of YAG is poor and the impurities cannot be completely migrated to the surface to be removed. Therefore, in the present invention, the sintering temperature needs to be strictly controlled.
[0117] By comparing Example 2 with Comparative Example 3, it can be seen that if the sintering time is too short, the impurities cannot be completely migrated to the surface and thus removed. Therefore, it is necessary to control the sintering time so that the impurities can migrate to the surface.
[0118] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for recycling a BN plate, characterized in that: The following steps are involved: A used BN plate is coated with a carbon-containing slurry; the used BN plate is a BN plate used for sintering an aluminum nitride substrate, and the used BN plate contains yttrium aluminum garnet impurities; the BN plate coated with the slurry is placed in a graphite furnace and sintered in a nitrogen atmosphere; during the sintering of the BN plate in a nitrogen atmosphere, the yttrium aluminum garnet has a certain fluidity, and the carbon-containing slurry is used to react with the yttrium aluminum garnet on the surface of the BN plate to promote the migration of the yttrium aluminum garnet inside the BN plate to the surface of the BN plate; After sintering, the BN plate is thinned to a thickness of 30~50um; The carbonaceous slurry includes at least one of graphite slurry, carbon black slurry and activated carbon slurry; The coating amount of the carbon-containing slurry is ≥10 mg / cm 2 ; When the BN plate is sintered in a nitrogen atmosphere, the sintering temperature is 1400~1900℃ and the sintering time is 4~8h.
2. The method for recycling a BN plate according to claim 1, characterized in that: The carbon-containing slurry is graphite slurry.
3. The method for recycling BN plates according to claim 1, characterized in that: When the BN plate is sintered in a nitrogen atmosphere, the sintering temperature is 1400~1700℃.
4. The method for recycling BN plates according to claim 1, characterized in that: The thinning process is grinding with a grinding wheel.
5. The method for recycling BN plates according to claim 1, characterized in that: Before sintering in a nitrogen atmosphere, the BN plates coated with the slurry are stacked.