Composite membrane for membrane distillation with volatile substance interception characteristics and preparation method thereof

By using electrospinning fiber membrane combined with interfacial polymerization and spin-dipping technology in membrane distillation technology to prepare a double-layer ultra-thin dense cortex composite membrane, the problem of the inability of existing technology to intercept volatile substances is solved, and efficient volatile substance interception is achieved. and high-throughput distillation effects.

CN115382403BActive Publication Date: 2024-10-08NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211081207.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-06
Publication Date
2024-10-08
Estimated Expiration
2042-09-06

AI Technical Summary

Technical Problem

Existing membrane distillation technology cannot effectively intercept volatile substances in high-salt wastewater, especially due to the high Henry's constant and large membrane pores, which cannot achieve the interception of volatile small molecules, and increasing the membrane thickness to improve the interception efficiency will lead to flux reduce.

Method used

A composite membrane with a double-layer ultra-thin dense skin layer is prepared by combining interfacial polymerization technology and spin-dipping technology on an electrospun fiber membrane. The super-hydrophobic layer, super-hydrophilic layer and interfacial interlayer effect are used to achieve volatile and non-volatile substances. interception while maintaining high throughput.

Benefits of technology

It achieves efficient interception of volatile substances in high-salt wastewater, with a phenol interception rate of more than 90%, a water flux maintained at 27L/m²h, and a salt interception rate of nearly 100%, while maintaining high distillation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115382403B_ABST
    Figure CN115382403B_ABST
Patent Text Reader

Abstract

A composite membrane for membrane distillation with volatile substance interception characteristics and a preparation method thereof belong to the field of polymer membrane preparation. The purpose of the present invention is to solve the problem that the current distillation membrane technology cannot achieve the interception of volatile substances in high-salt wastewater. The method uses interfacial polymerization technology and spin drop coating technology on an electrospun fiber membrane to prepare a composite membrane with a double-layer ultra-thin dense cortex, and uses the interfacial interlayer effect between the double-layer thin film composite membrane to achieve the interception of volatile and non-volatile substances in the membrane distillation process, while maintaining the high flux of the composite membrane. The composite membrane includes a super-hydrophobic layer, a super-hydrophilic layer and two FTC layers from bottom to top, and there is an interfacial interlayer effect between the two FTC layers. The composite membrane with a double-layer ultra-thin dense cortex prepared by the present invention can be used in the treatment of complex high-salt wastewater, and the specific application method is as follows: industrial high-salt wastewater is concentrated using a direct contact membrane distillation (DCMD) device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer membrane preparation, and in particular relates to a composite membrane for membrane distillation with volatile substance interception characteristics and a preparation method thereof. Background Art

[0002] Treatment and reuse of industrial high-salinity wastewater can effectively alleviate environmental pollution and the freshwater crisis. Reverse osmosis desalination technology is considered to be the most cost-effective technology for desalinating high-salinity wastewater, but it cannot treat highly concentrated brine, polar small molecules and volatile compounds. Membrane distillation (MD) is a high-water recovery technology that uses low-quality thermal energy (such as production waste heat, etc.) to intercept non-volatile substances. Its principle is to use the vapor pressure difference formed by the temperature difference on both sides of the membrane as the mass transfer power. Water vaporizes on the hot side membrane surface to form steam, which enters the cold side through the membrane pores for condensation and enrichment, and at the same time achieves the purpose of harvesting distilled water and concentrating wastewater. Although it has a nearly perfect interception of non-volatile substances, due to the complexity of the components of high-salinity wastewater, MD also faces the challenge of complex components of high-salinity wastewater when desalinating high-salinity wastewater. In recent years, membrane wetting, fouling and scaling have become current research hotspots, and great progress has been made by combining the design of new special wettable membranes with common water treatment processes. However, due to the high Henry constant and large membrane pores, it is impossible to intercept volatile small molecules. In order to separate fresh water from high-salinity wastewater containing volatile substances, the MD membrane should have two design criteria: (1) From the perspective of molecular sieving, it should have an appropriate pore size. Taking phenol as an example, the pore size of the selective permeable membrane should theoretically be in the range of 0.29 to 0.69 nm, because it allows water molecules to pass through the membrane while rejecting phenol molecules; (2) From the perspective of solubility and diffusion, the membrane should have high water molecule diffusion but inhibit the evaporation of volatile substances. Although increasing the thickness of the dense membrane can effectively improve the interception efficiency of volatile substances, the flux will be greatly reduced due to the increase in mass transfer resistance. Summary of the invention

[0003] The purpose of the present invention is to solve the problem that the current distillation membrane technology cannot achieve the interception of volatile substances in high-salt wastewater, and to provide a composite membrane for membrane distillation with volatile substance interception characteristics and a preparation method thereof. The method uses interfacial polymerization technology and spin drop coating technology on an electrospun fiber membrane to prepare a composite membrane with a double-layer ultra-thin dense skin layer, and utilizes the interfacial interlayer effect between the double-layer thin film composite membranes to achieve the interception of volatile and non-volatile substances in the membrane distillation process, while maintaining the high flux of the composite membrane.

[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0005] A composite membrane for membrane distillation with volatile substance interception characteristics, the composite membrane comprises a super hydrophobic layer, a super hydrophilic layer and two FTC layers from bottom to top, and there is an interface interlayer effect between the two FTC layers.

[0006] A method for preparing the composite membrane for membrane distillation with volatile substance interception characteristics is as follows: a fiber membrane with a hydrophobic layer is used as a substrate, and a super-hydrophilic layer is prepared on this basis by water-oil phase interface polymerization and spin drop coating. The specific steps of the method are as follows:

[0007] Step 1: adding a hydrophobic polymer and a hydrophobic additive to a solvent, heating in a water bath at 80° C. and stirring for 3 h to prepare a base membrane spinning solution, and preparing a base membrane by continuously electrospinning the base membrane spinning solution;

[0008] Step 2: Adding a hydrophilic polymer and nanoparticles to a solvent, heating in a water bath at 80° C. and stirring for 3 h to prepare a super-hydrophilic layer spinning solution, and preparing a Janus membrane with a super-hydrophilic protective layer by continuously electrospraying the super-hydrophilic layer spinning solution based on step 1;

[0009] Step 3: prepare a 1-5wt% m-phenylenediamine solution as an aqueous solution, add an alkaline reagent to adjust the pH and an acidic reagent to absorb the alkaline substances after the reaction, stir and ultrasonicate, pour the aqueous solution onto the surface of the Janus membrane in step 2, and after soaking for 2 minutes, remove the excess aqueous solution on the surface;

[0010] Step 4: prepare an organic phase solution of trimesoyl chloride with a concentration of 0.02-0.50wt% and stir it with ultrasound, pour the organic phase solution of trimesoyl chloride onto the surface of the membrane treated in step 3 for no more than 60s, remove excess organic phase solvent from the surface of the membrane, then place it in an oven at 60°C for 15min to completely volatilize the solvent, and then place it in an oven at 120°C for 1h to obtain a distillation membrane with a nanofiltration layer;

[0011] Step 5: Prepare one or two hydrophilic polymer solutions with a concentration of 1.00-20wt% and spin-coat them on the composite membrane prepared in step 4, dry them at room temperature and then place them in a 100°C forced air drying oven for heat treatment for 60 minutes to achieve thermal crosslinking of the hydrophilic polymers to obtain a composite membrane.

[0012] Furthermore, in step 1, the hydrophobic polymer is one or more of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyvinylidene fluoride (PVDF), and polyurethane (PU), the hydrophobic additive is one or more of functionalized fluorinated polyhedral oligomeric silsesquioxane (F-POSS), fluorinated polyurethane, and polydimethylsiloxane, the solvent is N, N-dimethylacetamide (DMAc) and / or acetone, and the mass fraction of the hydrophobic additive in the solution to the hydrophobic polymer is 5 to 20 wt%.

[0013] Furthermore, in step one, the continuous electrospinning is: first use four syringes to absorb 5 mL of spinning solution respectively, and then perform electrostatic spinning or electrostatic spraying; the continuous electrospinning parameters are as follows: the injection distance is 10-25 mm, the positive voltage is 10-30 kV, the negative voltage is 5-20 kV, the temperature is 20°C-30°C, the humidity is 40-60%, the injection speed is 0.05-0.5 cm / min, the receiving speed is 10-50 r / min, and the distance between the syringe needle tip and the receiver is 5-50 cm.

[0014] Furthermore, in step 2, the hydrophilic polymer is one or more of polyacrylonitrile (PAN), chitosan (CS), polyacrylic acid (PAA), and polyvinyl alcohol (PVA); the nanoparticles are one or more of silicon oxide, titanium oxide, and zirconium oxide; the solvent is one or more of N,N-dimethylacetamide (DMAc), acetone, and water; and the mass fraction of the nanoparticles in the hydrophilic polymer in the solution is 5 to 20 wt%.

[0015] Furthermore, in step 2, the continuous electrospinning is: first use four syringes to absorb 5 ml of spinning solution respectively, and then perform electrostatic spinning or electrostatic spraying; the continuous electrospinning parameters are as follows: the injection distance is 10-25 mm, the positive voltage is 10-30 kV, the negative voltage is 5-20 kV, the temperature is 20°C-30°C, the humidity is 40-60%, the injection speed is 0.05-0.5 cm / min, the receiving speed is 10-50 r / min, and the distance between the syringe needle tip and the receiver is 5-50 cm.

[0016] Furthermore, in step three, the alkaline reagent is triethylamine, and the acidic reagent is camphorsulfonic acid.

[0017] Furthermore, in step 4, the solvent used for the organic phase solution is n-hexane.

[0018] Furthermore, in step five, the spin coating rate is 20-200 rpm.

[0019] The composite membrane with a double-layer ultra-thin dense skin prepared by the present invention can be applied to the treatment of complex high-salinity wastewater. The specific application method is as follows: the industrial high-salinity wastewater is concentrated by using a direct contact membrane distillation (DCMD) device.

[0020] In view of the problem that volatile pollutants cannot be effectively intercepted in the current membrane distillation field, the present invention proposes a new method for preparing a double-layer ultra-thin dense skin composite membrane on the surface of a distillation membrane by using interfacial polymerization and spin coating technology. This method uses electrospinning to prepare a hydrophilic protective layer on the surface of the distillation membrane to solve the wetting problem of interfacial polymerization oil relative to the distillation membrane, thereby obtaining a composite distillation membrane with a double-layer ultra-thin dense skin. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a surface scanning electron microscope image of a composite distillation membrane with a double-layer ultra-thin and dense skin.

[0022] Figure 2 This is the interface diagram of the polyvinyl alcohol / polyacrylic acid layer in the composite distillation membrane with double ultra-thin dense skin.

[0023] Figure 3 This is the interface diagram of the polyamide layer in the composite distillation membrane with double ultra-thin and dense skin.

[0024] Figure 4 The water flux change diagrams of Janus membrane substrate, single-layer polyamide layer, single-layer polyvinyl alcohol / polyacrylic acid layer and double-layer polyamide layer and polyvinyl alcohol / polyacrylic acid.

[0025] Figure 5 The retention rate change diagram of Janus membrane substrate, single-layer polyamide layer, single-layer polyvinyl alcohol / polyacrylic acid layer, double-layer polyamide layer and polyvinyl alcohol / polyacrylic acid salt.

[0026] Figure 6 This is a graph showing the changes in the retention rate of volatile substances for the Janus membrane substrate, a single-layer polyamide layer, a single-layer polyvinyl alcohol / polyacrylic acid layer, and a double-layer polyamide layer and polyvinyl alcohol / polyacrylic acid.

[0027] Figure 7 This is a comparison chart of the retention rate of other common volatile substances by Janus membrane substrate, double polyamide layer and polyvinyl alcohol / polyacrylic acid. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention that does not depart from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.

[0029] Embodiment 1:

[0030] A method for preparing a composite membrane for membrane distillation having volatile substance interception characteristics, the method comprising the following steps:

[0031] Step 1: Prepare base membrane spinning solution: weigh 6.375 g of acetone and 14.875 g of DMAc, mix them, weigh 3.75 g of PVDF-HFP and 0.5625 g of F-POSS, add them to the above solution, heat in a water bath at 80° C. and stir until mixed, to obtain a solution as the base membrane spinning solution.

[0032] Step 2: Prepare super hydrophilic layer spinning solution: weigh 19.2 g of DMAc, then weigh 0.8 g of PAN and 0.048 g of SiO2, add them to the above solution, heat in a water bath at 60°C and stir until mixed, to obtain a solution as super hydrophilic layer spinning solution.

[0033] Step 3: Take four 10ml syringes and draw 5mL of basement membrane spinning liquid respectively for electrospinning to obtain basement membrane. The injection distance is 25mm. The control process parameters are positive voltage of 30kV, negative voltage of 5kV, temperature of 22℃-24℃, humidity of 55±2%, injection speed of 0.15cm / min, receiving speed of 30r / min, and the distance between the syringe needle tip and the receiver is 18cm.

[0034] Step 4: Take four 10ml syringes to draw 5mL of super hydrophilic layer spinning solution respectively for electrostatic spraying to spray the super hydrophilic layer spinning solution onto the double-layer membrane to form a super hydrophilic layer. The injection distance is 20mm, and the control process parameters are positive voltage 25kV, negative voltage 5kV, temperature 24℃-26℃, humidity 40±2%, injection speed 0.05cm / min, receiving speed 30r / min, and the distance between the syringe needle tip and the receiver is 20cm to obtain a Janus membrane with a super hydrophilic layer.

[0035] Step 5: Prepare an aqueous solution: dissolve m-phenylenediamine in distilled water to prepare a 2 wt % m-phenylenediamine (MPD) solution as an aqueous solution, add an alkaline agent and an acidic agent to adjust the pH, and stir with ultrasound.

[0036] Step 6: Prepare oil phase solution: dissolve trimesoyl chloride (TMC) in an organic solvent to prepare a trimesoyl chloride organic phase solution with a concentration of 0.06 wt % and stir with ultrasound.

[0037] Step 7: Pour the aqueous solution prepared in step 5 onto the surface of the Janus membrane and completely soak it for 2 minutes, then remove excess aqueous solution on the surface of the Janus membrane.

[0038] Step 8: Pour the oil phase solution prepared in step 6 onto the surface of the Janus membrane treated in step 7 and completely soak it. The soaking time shall not exceed 60 seconds. Remove the excess organic phase solution from the membrane surface. Then, place the treated membrane in a 60°C oven and dry it for 15 minutes to completely evaporate the solvent. Then, heat treat the treated membrane in a 120°C oven for 1 hour to obtain a distillation membrane with a nanofiltration layer.

[0039] Step 9: PVA 0.379 g and PAA 0.621 g were added to water 9.00 g, heated and stirred evenly, 2 g of the polymer solution was taken out and spin-coated at 100 rpm on the composite membrane prepared in step 8, dried at room temperature and then placed in a blast drying oven at 100°C for 60 min. The cross-sectional structure of the obtained double-layer dense composite membrane is as follows: Figure 1-3 shown.

[0040] The prepared composite distillation membrane with ultra-thin and dense skin was used to distill high-salt wastewater (1L) containing 20ppm phenol. The membrane distillation parameters were set as 60℃ for the feed side temperature, 40℃ for the permeate side temperature, and 240ml / min for the flow rate. An electronic balance was used to record the amount of water collected on the distillation side per minute. A conductivity meter was used to monitor the conductivity of the water on the distillation side and record the effluent quality. The distillation effect of the ultra-thin and dense skin composite distillation membrane on high-salt wastewater containing 20ppm phenol is shown in Figure 2. Figure 2-5 As shown in Figure 2, the water flux of the dense double-layer ultra-thin dense skin composite distillation membrane has been maintained at 27Lm -2 h -1 about( Figure 4 ), the salt retention rate is nearly 100% ( Figure 5 ), phenol retention rate exceeds 90% ( Figure 6 ).

[0041] Embodiment 2:

[0042] A method for preparing a composite membrane for membrane distillation having volatile substance interception characteristics, the method comprising the following steps:

[0043] Step 1: Prepare base membrane spinning solution: weigh 6.375 g of acetone and 14.875 g of DMAc, mix them, weigh 3.3 g of PVDF and 0.495 g of F-POSS, add them to the above solution, heat in a water bath at 80° C. and stir until mixed, to obtain a solution as the base membrane spinning solution.

[0044] Step 2: Prepare super hydrophilic layer spinning solution: weigh 19.2 g of DMAc, then weigh 0.8 g of PAN and 0.048 g of SiO2, add them to the above solution, heat in a water bath at 60°C and stir until mixed, to obtain a solution as super hydrophilic layer spinning solution.

[0045] Step 3: Take four 10ml syringes and draw 5mL of basement membrane spinning liquid respectively for electrospinning to obtain basement membrane. The injection distance is 25mm. The control process parameters are positive voltage of 25kV, negative voltage of 10kV, temperature of 25℃, humidity of 60±2%, injection speed of 0.10cm / min, receiving speed of 50r / min, and the distance between the syringe needle tip and the receiver is 18cm.

[0046] Step 4: Take four 10ml syringes to absorb 5mL of super hydrophilic layer spinning liquid respectively for electrostatic spraying to spray the super hydrophilic layer spinning liquid onto the double-layer membrane to form a super hydrophilic layer. The injection distance is 15mm, and the control process parameters are positive voltage 25kV, negative voltage 5kV, temperature 25℃, humidity 55%, injection speed 0.05cm / min, receiving speed 30r / min, and the distance between the syringe needle tip and the receiver is 10cm to obtain a Janus membrane with a super hydrophilic layer.

[0047] Step 5: preparing an aqueous solution: preparing a 0.3 wt % m-phenylenediamine solution as an aqueous solution, adding an alkaline agent and an acidic agent to adjust the pH and stirring with ultrasound.

[0048] Step 6: Prepare oil phase solution: dissolve trimesoyl chloride in an organic solvent to prepare a 0.09 wt % trimesoyl chloride organic phase solution and stir with ultrasound.

[0049] Step 7: Pour the aqueous solution prepared in step 5 onto the surface of the Janus membrane and completely soak it for 2 minutes, then remove excess aqueous solution on the surface of the Janus membrane.

[0050] Step 8: Pour the oil phase solution prepared in step 6 onto the surface of the Janus membrane treated in step 7 and completely soak it. The soaking time shall not exceed 60 seconds. Remove the excess organic phase solution from the membrane surface. Then, place the treated membrane in a 60°C oven and dry it for 15 minutes to completely evaporate the solvent. Then, heat treat the treated membrane in a 120°C oven for 1 hour to obtain a distillation membrane with a nanofiltration layer.

[0051] Step nine: Add 0.5685 g of PVA and 0.9315 g of PAA to 8.5 g of water, heat and stir until evenly mixed, take out 2 g of the polymer solution and spin-coat it at 100 rpm on the composite film prepared in step eight, dry it at room temperature and then place it in a 100° C. forced air drying oven for heat treatment for 60 min.

[0052] The prepared double-layer ultra-thin and dense skin composite distillation membrane was used to distill high-salinity wastewater (1L) containing 20ppm phenol. The membrane distillation parameters were set to a feed side temperature of 60°C, a permeate side temperature of 40°C, a flow rate of 240ml / min, an electronic balance was used to record the amount of water collected on the distillation side per minute, a conductivity meter was used to monitor the conductivity of the water on the distillation side, and the quality of the effluent was recorded. When the ultra-thin and dense skin composite distillation membrane was used to distill high-salinity wastewater containing 20ppm ethanol, the ethanol retention rate was as high as 92% ( Figure 7 ).

[0053] Embodiment 3:

[0054] A method for preparing a composite membrane for membrane distillation having volatile substance interception characteristics, the method comprising the following steps:

[0055] Step 1: Prepare base membrane spinning solution: weigh 47.75 g of DMAc, 4.5 g of polyurethane (PU) and 0.675 g of F-POSS, add them to the above solution, heat in a water bath at 80°C and stir until mixed, to obtain a solution as the base membrane spinning solution.

[0056] Step 2: Prepare super hydrophilic layer spinning solution: weigh 17 g of water, then weigh 3.00 g of PVA and 0.3 g of SiO2, add them to the above solution, heat in a water bath at 60°C and stir until mixed, to obtain a solution as super hydrophilic layer spinning solution.

[0057] Step 3: Take four 10ml syringes and draw 5mL of basement membrane spinning liquid respectively for electrospinning to obtain basement membrane. The injection distance is 25mm. The control process parameters are positive voltage of 20kV, negative voltage of 5kV, temperature of 23℃, humidity of 45%, injection speed of 0.4cm / min, receiving speed of 50r / min, and the distance between the syringe needle tip and the receiver is 18cm.

[0058] Step 4: Take four 10ml syringes to absorb 5mL of super hydrophilic layer spinning liquid respectively for electrostatic spraying to spray the super hydrophilic layer spinning liquid onto the double-layer membrane to form a super hydrophilic layer. The injection distance is 25mm, and the control process parameters are positive voltage 25kV, negative voltage 5kV, temperature 25℃, humidity 45%, injection speed 0.15cm / min, receiving speed 30r / min, and the distance between the syringe needle tip and the receiver is 20cm to obtain a Janus membrane with a super hydrophilic layer.

[0059] Step 5: preparing an aqueous phase solution: preparing a 0.2 wt% m-phenylenediamine solution as an aqueous phase solution, adding an alkaline agent and an acidic agent to adjust the pH and stirring with ultrasound.

[0060] Step 6: Prepare oil phase solution: dissolve trimesoyl chloride in an organic solvent to prepare an organic phase solution of trimesoyl chloride with a concentration of 0.06 wt % and stir with ultrasound.

[0061] Step 7: Pour the aqueous solution prepared in step 5 onto the surface of the Janus membrane and completely soak it for 2 minutes, then remove excess aqueous solution on the surface of the Janus membrane.

[0062] Step 8: Pour the oil phase solution prepared in step 6 onto the surface of the Janus membrane treated in step 7 and completely soak it. The soaking time shall not exceed 60 seconds. Remove the excess organic phase solution from the membrane surface. Then, place the treated membrane in a 60°C oven and dry it for 15 minutes to completely evaporate the solvent. Then, heat treat the treated membrane in a 120°C oven for 1 hour to obtain a distillation membrane with a nanofiltration layer.

[0063] Step nine: Add 0.379 g of PVA and 0.621 g of PAA to 9.00 g of water, heat and stir until evenly mixed, take out 2 g of the polymer solution and spin-coat it at 100 rpm on the composite film prepared in step eight, dry it at room temperature and then place it in a 100° C. forced air drying oven for heat treatment for 60 min.

[0064] The prepared double-layer ultra-thin dense skin composite distillation membrane was used to distill high-salt wastewater (1L) containing 20ppm phenol. The membrane distillation parameters were set as 60℃ on the feed side, 40℃ on the permeate side, and 240ml / min on the flow rate. An electronic balance was used to record the amount of water collected on the distillation side per minute. A conductivity meter was used to monitor the conductivity of the water on the distillation side and record the effluent quality. The distillation effect of the double-layer ultra-thin dense skin composite distillation membrane on high-salt wastewater containing 20ppm of various volatile organic compounds is shown in Figure 2. Figure 5 As shown, the ultra-thin and dense double-layer composite distillation membrane has a very good retention rate of about 90% for other volatile organic compounds.

Claims

1. A method for preparing a composite membrane for membrane distillation having volatile substance interception characteristics, characterized in that: The method steps are: Step 1: preparing a base membrane spinning solution: weighing 6.375 g of acetone and 14.875 g of N, N-dimethylacetamide, mixing them, weighing 3.75 g of polyvinylidene fluoride-hexafluoropropylene and 0.5625 g of functionalized fluorinated polyhedral oligomeric silsesquioxane, adding them to the above solution, heating in a water bath at 80°C and stirring until mixed, to obtain a solution as the base membrane spinning solution; Step 2: Prepare a super hydrophilic layer spinning solution: weigh 19.2 g of N, N-dimethylacetamide, weigh 0.8 g of polyacrylonitrile and 0.048 g of SiO2, add them to the above solution, heat in a water bath at 60 °C and stir until mixed, and obtain a solution as a super hydrophilic layer spinning solution; Step 3: Take four 10 ml syringes and draw 5 mL of the basement membrane spinning solution for electrospinning to obtain the basement membrane. The injection distance is 25 mm. The control process parameters are positive voltage of 30 kV, negative voltage of 5 kV, temperature of 22 ℃-24 ℃, humidity of 55±2%, injection speed of 0.15 cm / min, receiving speed of 30 r / min, and the distance between the syringe needle tip and the receiver is 18 cm. Step 4: Take four 10 ml syringes and draw 5 ml of the super-hydrophilic layer spinning solution respectively for electrostatic spraying to spray the super-hydrophilic layer spinning solution onto the double-layer membrane to form a super-hydrophilic layer. The injection distance is 20 mm. The control process parameters are positive voltage 25 kV, negative voltage 5 kV, temperature 24 ℃-26 ℃, humidity 40±2%, injection speed 0.05 cm / min, receiving speed 30 r / min, and the distance between the syringe needle tip and the receiver is 20 cm, so as to obtain a Janus membrane with a super-hydrophilic layer. Step 5: preparing an aqueous phase solution: dissolving m-phenylenediamine in distilled water to prepare a m-phenylenediamine solution with a concentration of 2 wt % as the aqueous phase solution, adding an alkaline reagent and an acidic reagent to adjust the pH and stirring with ultrasound; Step 6: preparing an oil phase solution: dissolving trimesoyl chloride in an organic solvent to prepare a 0.06 wt% trimesoyl chloride organic phase solution and stirring with ultrasound; Step 7: Pour the aqueous solution prepared in step 5 onto the surface of the Janus membrane and completely soak it for 2 min, then remove the excess aqueous solution on the surface of the Janus membrane; Step 8: pour the oil phase solution prepared in step 6 onto the surface of the Janus membrane treated in step 7 and completely infiltrate it. The infiltration time does not exceed 60 s. Remove the excess organic phase solution on the membrane surface. Then, place the treated membrane in a 60 °C oven for 15 min to completely evaporate the solvent. Then, heat treat the treated membrane in a 120 °C oven for 1 h to obtain a distillation membrane with a nanofiltration layer. Step nine: Add 0.379 g of polyvinyl alcohol and 0.621 g of polyacrylic acid to 9.00 g of water, heat and stir until evenly mixed, then take out 2 g of the polymer solution and spin-coat it at 100 rpm on the distillation membrane prepared in step eight, dry it at room temperature, and then place it in a forced air drying oven at 100 °C for heat treatment for 60 min to obtain a composite membrane for membrane distillation having volatile substance retention characteristics.