A solvent-based acrylic resin and its application in high temperature resistant and electrolytic resistant hydraulic sensitive adhesive

By using solvent-based acrylic resin and epoxy monomers in the pressure-sensitive adhesive, the problem of insufficient durability of the pressure-sensitive adhesive in the high temperature and electrolyte environment in the prior art is solved, and higher high temperature resistance and Electrolyte resistance, suitable for high-demand industrial applications.

CN115386316BActive Publication Date: 2024-11-05DONGGUAN AOZON ELECTRONICS MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210973803.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-15
Publication Date
2024-11-05
Estimated Expiration
2042-08-15

AI Technical Summary

Technical Problem

Existing pressure-sensitive adhesives show imperfect durability in high temperature and electrolyte environments and cannot meet the needs of certain special places.

Method used

Solvent-based acrylic resin containing epoxy monomers and functional monomers can improve the high temperature and electrolyte resistance of the glue through cross-linking reactions, and enhance the internal convergence of the glue by reasonably regulating the ratio of soft monomers and hard monomers. Strength and bondability.

Benefits of technology

It significantly improves the high temperature and electrolyte resistance of pressure-sensitive adhesives, enhances the density and rigidity of the glue layer, and extends the service life of the glue in high temperature and electrolytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115386316B_ABST
    Figure CN115386316B_ABST
Patent Text Reader

Abstract

The invention provides a solvent-based acrylic resin, comprising the following components: 220-280 parts of acrylic monomers, 0.2-0.4 parts of initiators, and 360-380 parts of organic solvents; the acrylic monomers include epoxy monomers and functional monomers; the epoxy monomers contain epoxy functional groups, and the mass percentage of the epoxy monomers in the acrylic monomers is not less than 5.36%; the functional monomers contain at least one of hydroxyl functional groups and carboxyl functional groups, and the mass percentage of the functional monomers in the acrylic monomers is not less than 5.36%. The solvent-based acrylic resin in the invention undergoes a cross-linking reaction with an amino resin and an epoxy curing agent, and the formed pressure-sensitive adhesive layer is more compact and has more excellent high temperature resistance and electrolyte resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of glue, and in particular relates to a solvent-based acrylic resin and application thereof in a high-temperature resistant and electrolytic resistant pressure sensitive glue. Background Art

[0002] The full name of pressure-sensitive adhesive is pressure-sensitive adhesive, also commonly known as self-adhesive, or simply pressure-sensitive adhesive. Pressure-sensitive adhesive can be immediately bonded to the smooth surface of the adherend under a small pressure such as finger pressure. At the same time, when the pressure-sensitive adhesive is torn off the adherend surface, the pressure-sensitive adhesive will not pollute the adherend surface. Therefore, pressure-sensitive adhesive is widely used in industry, agriculture, transportation, medical treatment, national defense and daily life.

[0003] Among the commonly used pressure-sensitive adhesives, acrylic pressure-sensitive adhesives are particularly widely used, which have excellent adhesion and chemical stability, as well as the advantages of being non-toxic, harmless and low-cost. However, some special places have special requirements for the high temperature resistance and electrolyte resistance of pressure-sensitive adhesives, and general pressure-sensitive adhesives cannot meet their requirements. Therefore, it is of great practical significance to develop a pressure-sensitive adhesive that is resistant to high temperatures and electrolytes. Summary of the invention

[0004] In order to solve the shortcomings and deficiencies in the prior art, the present invention provides a high temperature resistant and electrolyte resistant pressure sensitive adhesive to improve the high temperature resistance and electrolyte resistance of the pressure sensitive adhesive.

[0005] According to a first aspect of the present invention, a solvent-based acrylic resin is provided, which comprises the following components, calculated in parts by weight: 220 to 280 parts of acrylic monomers, 0.2 to 0.4 parts of initiators, and 360 to 380 parts of solvents; the acrylic monomers comprise epoxy monomers and functional monomers; the epoxy monomers contain epoxy functional groups, and the mass percentage of the epoxy monomers in the acrylic monomers is not less than 5.36%; the functional monomers contain at least one of hydroxyl functional groups and carboxyl functional groups, and the mass percentage of the functional monomers in the acrylic monomers is not less than 5.36%.

[0006] Preferably, the epoxy monomer is 3,4-epoxycyclohexyl methacrylate.

[0007] Preferably, the functional monomer includes at least one of acrylic acid and hydroxyethyl acrylate.

[0008] In the above solvent-based acrylic resin, the epoxy monomer used has an epoxy functional group. On the one hand, the epoxy functional group can react with the carboxyl group in the acrylic resin at high temperature, which can make the cross-linking of the pressure-sensitive adhesive more compact, reduce the swelling rate of the pressure-sensitive adhesive prepared by acrylic glue in the electrolyte, and thus improve the electrolyte resistance of the pressure-sensitive adhesive; on the other hand, the epoxy monomer is 3,4-epoxycyclohexyl methacrylate, which has a rigid ring structure, which can improve the rigidity of the pressure-sensitive adhesive, thereby improving the high temperature resistance of the pressure-sensitive adhesive. In addition, in the above solvent-based acrylic resin, the functional monomer used contains a hydroxyl or carboxyl functional group, which can enhance the cross-linking degree of the pressure-sensitive adhesive and improve the high temperature resistance and electrolyte resistance of the pressure-sensitive adhesive prepared thereby.

[0009] Preferably, the acrylic monomer also includes a soft monomer and a hard monomer, and the mass ratio of the soft monomer to the hard monomer is 150-170:40-60. As the main synthetic monomer of acrylic glue, the soft monomer has a lower glass transition temperature, which gives the pressure-sensitive adhesive formed by the acrylic glue better flexibility and adhesion, and can promote the film formation of the acrylic glue. The hard monomer has a higher glass transition temperature, which can enhance the hardness of the pressure-sensitive adhesive formed by the acrylic glue and ensure that the pressure-sensitive adhesive has a certain cohesive strength. By reasonably regulating the ratio of the soft monomer and the hard monomer in the acrylic glue, it can be ensured that the pressure-sensitive adhesive formed thereby has good flexibility while ensuring that the pressure-sensitive adhesive has a certain cohesive strength, thereby improving the comprehensive performance of the pressure-sensitive adhesive.

[0010] Preferably, the soft monomer includes at least one of butyl acrylate and isooctyl acrylate.

[0011] Preferably, the hard monomer includes at least one of methyl acrylate, vinyl acetate, and isobornyl acrylate.

[0012] Preferably, the solvent-based acrylic resin is prepared according to the following method:

[0013] S1. The first part of the initiator A is mixed with the first part of the organic solvent to form a mixed solution A, the acrylate monomer is mixed with the second part of the organic solvent to form a mixed solution B, the mixed solution B is heated to 75-80° C. under the protection of nitrogen, and the temperature is kept, the mixed solution A is added to the mixed solution B, and the temperature is continued to be raised to 85-90° C., and the temperature is kept for 8-13 minutes to obtain an acrylate prepolymer A;

[0014] S2. The acrylate prepolymer is cooled to 65 to 70° C., the second part of the initiator A is mixed with the third part of the organic solvent to form a mixed solution C, the mixed solution C is added to the acrylate prepolymer A, and the mixture is kept warm for 2 to 3 hours to obtain an acrylate prepolymer B;

[0015] S3. The initiator B is mixed with the fourth part of the organic solvent to form a mixed solution D, the mixed solution D is added to the acrylate prepolymer B, and then the temperature is raised to 75 to 78 ° C, kept for 2.5 to 3.5 hours, and then cooled to 45 to 55 ° C, and the fifth part of the organic solvent is added thereto to obtain a solvent-based acrylic resin;

[0016] Among them, the reactivity of initiator A is lower than that of initiator B;

[0017] The total amount of initiator A is equal to the sum of the mass of the first part of initiator A and the mass of the second part of initiator A;

[0018] The total amount of the organic solvent is equal to the sum of the masses of the first portion of the organic solvent, the second portion of the organic solvent, the third portion of the organic solvent, the fourth portion of the organic solvent, and the fifth portion of the organic solvent.

[0019] In the above-mentioned method for preparing solvent-based acrylic resin, firstly, in the early stage of the reaction, a relatively low-activity initiator and a low reaction temperature are used, while in the later stage of the reaction, a relatively high-activity initiator and a high reaction temperature are used, so as to improve the conversion rate of the monomers participating in the reaction and ensure that the acrylic monomers can fully participate in the reaction to form acrylic resin; secondly, in the specific steps of the reaction of the acrylic resin, by adding the initiator step by step into the acrylic monomer or the acrylate prepolymer to initiate the reaction in batches, the acrylic resin can have a larger molecular weight, and at the same time, it can be ensured that the acrylic monomer is not prone to violent polymerization during the process of initiating polymerization, and the finally synthesized acrylic resin can be ensured to have a more uniform molecular weight distribution, so that the preparation process of the acrylic resin is easier to control.

[0020] Preferably, the mixed solution A is added to the mixed solution B by dropwise addition for 5 to 10 minutes.

[0021] Preferably, the dropwise addition time of adding mixed solution A to mixed solution B is 5 minutes.

[0022] Preferably, the mixed solution C is added to the acrylate prepolymer A by dropwise addition for a time of 1.5 to 3 hours.

[0023] Preferably, the mixed solution D is added to the acrylate prepolymer B by dropwise addition for 5 to 20 minutes.

[0024] In the process of using an initiator to initiate the polymerization of acrylic monomers or acrylate prepolymers step by step, the initiator is added dropwise, which can further control the polymerization rate of the reaction and prevent phenomena such as violent polymerization, which affect the stability and safety of the acrylic resin preparation process.

[0025] Preferably, the mass ratio of the first part initiator A, the second part initiator A and the initiator B is 1-2:5-7:1; the mass ratio of the first part solvent, the second part solvent, the third part solvent, the fourth part solvent and the fifth part solvent is 255-270:5-10:20-30:15-30:50-70.

[0026] Preferably, initiator A includes at least one of lauroyl peroxide and azobisisobutyronitrile, initiator B includes at least one of azobisisoheptanenitrile and tert-butyl peroxy-2-ethylhexanoate; and the organic solvent includes at least one of ethyl acetate, butanone and toluene.

[0027] According to a second aspect of the present invention, there is provided a high temperature resistant and electrolytic resistant pressure sensitive adhesive, which is prepared by using the above solvent-based acrylic resin.

[0028] Preferably, the above-mentioned high temperature resistant and electrolyte resistant hydraulic sensitive adhesive is calculated by weight and is a mixture of 90-98 parts of solvent-based acrylic resin, 1-4 parts of amino resin, 0.01-1 part of catalyst, and 0.1-1 part of epoxy curing agent.

[0029] The solvent-based acrylic resin, amino resin and epoxy curing agent undergo a cross-linking reaction, and the curing agent has a higher functionality. Therefore, the pressure-sensitive adhesive layer formed after curing with the curing agent has a higher density, which makes the pressure-sensitive adhesive layer have better cohesion, and thus the pressure-sensitive adhesive layer has stronger electrolyte resistance.

[0030] Preferably, the amino resin includes at least one of butylated melamine formaldehyde resin, isobutylated melamine formaldehyde resin and methylated melamine formaldehyde resin.

[0031] Preferably, the catalyst is p-toluenesulfonic acid.

[0032] Preferably, the epoxy curing agent is at least one of CVC GA240 and E-44.

[0033] Preferably, the epoxy curing agent is CVC GA240.

[0034] According to the third aspect of the present invention, a high-temperature resistant and electrolytically resistant pressure-sensitive adhesive tape is provided, which is composed of a release film layer, a pressure-sensitive adhesive layer and a base film layer compounded in sequence, and the pressure-sensitive adhesive layer is obtained by coating a high-temperature resistant and electrolytically resistant pressure-sensitive adhesive on the base film layer and then thermally curing it.

[0035] Preferably, the pressure-sensitive adhesive layer is obtained by coating a high-temperature resistant and electrolytically resistant pressure-sensitive adhesive on the corona surface of the base film layer and then thermally curing the resulting layer.

[0036] Preferably, the specific steps of the preparation method of the high-temperature resistant and electrolytically resistant pressure-sensitive adhesive tape are: apply the high-temperature resistant and electrolytically resistant pressure-sensitive adhesive on the corona surface of the base film layer, bake it at 110°C to 130°C for 2 to 3 minutes, and then adhere the release layer to obtain the high-temperature resistant and electrolytically resistant pressure-sensitive adhesive tape.

[0037] Preferably, the base film layer is made of PET.

[0038] Preferably, the release layer is made of PET.

[0039] In summary, the pressure-sensitive adhesive layer formed by the solvent-based acrylic resin, acrylic resin and amino resin for the pressure-sensitive adhesive tape prepared by the present invention under the curing of epoxy curing agent is more compact, and therefore has more excellent electrolyte resistance. In addition, the present invention uses an epoxy monomer containing an epoxy functional group, which can react with the carboxyl group in the resin at high temperature, can enhance the cross-linking degree of the colloid, reduce the swelling degree of the colloid in the electrolyte, and further improve the electrolyte resistance of the adhesive layer, and the cyclic structure contained in the epoxy monomer 3.4-epoxycyclohexyl methacrylate can improve the rigidity of the adhesive layer, thereby improving the high temperature resistance of the adhesive layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic diagram of the structure of the high temperature resistant and electrolytic resistant pressure sensitive adhesive tape of the present invention;

[0041] The above figures are marked as: 1. base film layer, 2. pressure-sensitive adhesive layer, 3. release film layer. DETAILED DESCRIPTION

[0042] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.

[0043] Example 1

[0044] Synthesis of solvent-based acrylic resin:

[0045] S1. Weigh 0.06 g of lauroyl peroxide and 5 g of ethyl acetate and mix them evenly to form a mixed solution A, weigh 105 g of butyl acrylate, 51.4 g of isooctyl acrylate, 48.6 g of vinyl acetate, 10 g of isobornyl acrylate, 6 g of acrylic acid, 11 g of hydroxyethyl acrylate, 18 g of 3,4-epoxycyclohexyl methacrylate, and 266.7 g of ethyl acetate, add them into a reactor and mix them evenly to form a mixed solution B, under nitrogen protection, continuously stir the mixed solution B and heat it to 78° C., add the mixed solution A dropwise to the mixed solution B over 5 min, continue to heat it to 90° C., and keep it warm for 10 min to obtain an acrylate prepolymer A;

[0046] S2. The acrylate prepolymer A was cooled to 67° C., 0.24 g of lauroyl peroxide and 21.6 g of ethyl acetate were weighed and mixed to form a mixed solution C, and the mixed solution C was added dropwise to the acrylate prepolymer A over 2 h, and the mixture was kept warm for 2 h to obtain an acrylate prepolymer B;

[0047] S3. Weigh 0.04 g of azobisisoheptanenitrile and 24.8 g of ethyl acetate and mix them evenly to form a mixed solution D. Add the mixed solution D dropwise into the acrylate prepolymer B over 20 min, heat it to 75°C, keep it warm for 3 h, then cool it to 50°C, add 56.9 g of ethyl acetate and mix evenly, remove the nitrogen, and obtain a solvent-based acrylic resin.

[0048] Example 2

[0049] Synthesis of solvent-based acrylic resin:

[0050] S1. Weigh 0.06 g of lauroyl peroxide and 5 g of ethyl acetate and mix them evenly to form a mixed solution A, weigh 131 g of butyl acrylate, 32.9 g of isooctyl acrylate, 42.1 g of vinyl acetate, 9 g of isobornyl acrylate, 8 g of acrylic acid, 11 g of hydroxyethyl acrylate, 16 g of 3,4-epoxycyclohexyl methacrylate, and 266.7 g of ethyl acetate, add them into a reactor and mix them evenly to form a mixed solution B, under nitrogen protection, continuously stir the mixed solution B and heat it to 78° C., add the mixed solution A dropwise to the mixed solution B over 5 min, continue to heat it to 88° C., and keep it warm for 10 min to obtain an acrylate prepolymer A;

[0051] S2. The acrylate prepolymer A was cooled to 67° C., 0.24 g of lauroyl peroxide and 21.6 g of ethyl acetate were weighed and mixed to form a mixed solution C, and the mixed solution C was added dropwise to the acrylate prepolymer A over 2 h, and the mixture was kept warm for 2 h to obtain an acrylate prepolymer B;

[0052] S3. Weigh 0.04 g of azobisisoheptanenitrile and 24.8 g of ethyl acetate and mix them evenly to form a mixed solution D. Add the mixed solution D dropwise into the acrylate prepolymer B over 20 min, raise the temperature to 78°C, keep the temperature for 3 h, then cool down to 50°C, add 56.9 g of ethyl acetate and mix evenly, remove the nitrogen, and obtain a solvent-based acrylic resin.

[0053] Example 3

[0054] Synthesis of solvent-based acrylic resin:

[0055] S1. Weigh 0.06 g of azobisisobutyronitrile and 5 g of ethyl acetate and mix them evenly to form a mixed solution A, weigh 105 g of butyl acrylate, 51.4 g of isooctyl acrylate, 48.6 g of vinyl acetate, 10 g of isobornyl acrylate, 6 g of acrylic acid, 11 g of hydroxyethyl acrylate, 18 g of 3,4-epoxycyclohexyl methacrylate, and 266.7 g of ethyl acetate, add them into a reactor and mix them evenly to form a mixed solution B, under nitrogen protection, stir the mixed solution B continuously and heat it to 78° C., add the mixed solution A dropwise to the mixed solution B over 5 min, continue to heat it to 90° C., and keep it warm for 10 min to obtain an acrylate prepolymer A;

[0056] S2. The acrylate prepolymer A was cooled to 67° C., 0.24 g of azobisisobutyronitrile and 21.6 g of ethyl acetate were weighed and mixed to form a mixed solution C, and the mixed solution C was added dropwise to the acrylate prepolymer A over 2 h, and the mixture was kept warm for 2 h to obtain an acrylate prepolymer B;

[0057] S3. Weigh 0.04 g of tert-butyl peroxide-2-ethylacetate and 24.8 g of ethyl acetate and mix them evenly to form a mixed solution D. Add the mixed solution D dropwise into the acrylate prepolymer B over 20 min, heat it to 75°C, keep it warm for 3 h, then cool it to 50°C, add 56.9 g of ethyl acetate and mix evenly, remove the nitrogen, and obtain a solvent-based acrylic resin.

[0058] Example 4

[0059] Synthesis of solvent-based acrylic resin:

[0060] S1. Weigh 0.04 g of lauroyl peroxide and 5 g of ethyl acetate and mix them evenly to form a mixed solution A, weigh 150.4 g of butyl acrylate, 48.6 g of vinyl acetate, 10 g of methyl acrylate, 10 g of acrylic acid, 5.8 g of hydroxyethyl acrylate, 26 g of 3,4-epoxycyclohexyl methacrylate, and 266.7 g of ethyl acetate, add them into a reactor and mix them evenly to form a mixed solution B, under nitrogen protection, continuously stir the mixed solution B and heat it to 75° C., add the mixed solution A dropwise to the mixed solution B over 5 min, continue to heat it to 90° C., and keep it warm for 10 min to obtain an acrylate prepolymer A;

[0061] S2. The acrylate prepolymer A was cooled to 67° C., 0.20 g of lauroyl peroxide and 21.6 g of ethyl acetate were weighed and mixed to form a mixed solution C, and the mixed solution C was added dropwise to the acrylate prepolymer A over 2 h, and the mixture was kept warm for 2 h to obtain an acrylate prepolymer B;

[0062] S3. Weigh 0.04 g of azobisisoheptanenitrile and 24.8 g of ethyl acetate and mix them evenly to form a mixed solution D. Add the mixed solution D dropwise into the acrylate prepolymer B over 20 min, heat it to 75°C, keep it warm for 3 h, then cool it to 50°C, add 56.9 g of ethyl acetate and mix evenly, remove the nitrogen, and obtain a solvent-based acrylic resin.

[0063] Example 5

[0064] Synthesis of solvent-based acrylic resin:

[0065] S1. Weigh 0.06 g of lauroyl peroxide and 5 g of ethyl acetate and mix them evenly to form a mixed solution A, weigh 105 g of butyl acrylate, 61.4 g of isooctyl acrylate, 38.6 g of vinyl acetate, 10.6 g of isobornyl acrylate, 8 g of acrylic acid, 11 g of hydroxyethyl acrylate, 16 g of 3,4-epoxycyclohexyl methacrylate, and 266.7 g of ethyl acetate, add them into a reactor and mix them evenly to form a mixed solution B, under nitrogen protection, continuously stir the mixed solution B and heat it to 78° C., add the mixed solution A dropwise to the mixed solution B over 5 min, continue to heat it to 90° C., and keep it warm for 10 min to obtain an acrylate prepolymer A;

[0066] S2. The acrylate prepolymer A was cooled to 67° C., 0.28 g of lauroyl peroxide and 21.6 g of ethyl acetate were weighed and mixed to form a mixed solution C, and the mixed solution C was added dropwise to the acrylate prepolymer A over 2 h, and the mixture was kept warm for 2 h to obtain an acrylate prepolymer B;

[0067] S3. Weigh 0.04 g of azobisisoheptanenitrile and 24.8 g of ethyl acetate and mix them evenly to form a mixed solution D. Add the mixed solution D dropwise into the acrylate prepolymer B over 20 min, heat it to 75°C, keep it warm for 3 h, then cool it to 50°C, add 56.9 g of ethyl acetate and mix evenly, remove the nitrogen, and obtain a solvent-based acrylic resin.

[0068] Comparative Example 1

[0069] Synthesis of solvent-based acrylic resin:

[0070] S1. Weigh 0.06 g of lauroyl peroxide and 5 g of ethyl acetate and mix them evenly to form a mixed solution A, weigh 105 g of butyl acrylate, 51.4 g of isooctyl acrylate, 48.6 g of vinyl acetate, 10 g of isobornyl acrylate, 6 g of acrylic acid, 11 g of hydroxyethyl acrylate, 18 g of 3,4-epoxycyclohexyl methacrylate, and 266.7 g of ethyl acetate, add them into a reactor and mix them evenly to form a mixed solution B, under nitrogen protection, continuously stir the mixed solution B and heat it to 78° C., add the mixed solution A dropwise to the mixed solution B over 5 min, continue to heat it to 88° C., and keep it warm for 10 min to obtain an acrylate prepolymer A;

[0071] S2. The acrylate prepolymer A was cooled to 67° C., 0.24 g of lauroyl peroxide and 21.6 g of ethyl acetate were weighed and mixed to form a mixed solution C, and the mixed solution C was added dropwise to the acrylate prepolymer A over 2 h, and the mixture was kept warm for 2 h to obtain an acrylate prepolymer B;

[0072] S3. Weigh 0.04 g of lauroyl peroxide and 24.8 g of ethyl acetate and mix them evenly to form a mixed solution D. Add the mixed solution D dropwise into the acrylate prepolymer B over 20 minutes, keep warm for 3 hours, then cool to 50°C, add 56.9 g of ethyl acetate and mix evenly, remove nitrogen, and obtain a solvent-based acrylic resin.

[0073] Comparative Example 2

[0074] Synthesis of solvent-based acrylic resin:

[0075] S1. Weigh 0.06 g of lauroyl peroxide and 5 g of ethyl acetate and mix them evenly to form a mixed solution A, weigh 105 g of butyl acrylate, 51.4 g of isooctyl acrylate, 48.6 g of vinyl acetate, 10 g of isobornyl acrylate, 6 g of acrylic acid, 11 g of hydroxyethyl acrylate, 18 g of 3,4-epoxycyclohexyl methacrylate, and 266.7 g of ethyl acetate, add them into a reactor and mix them evenly to form a mixed solution B, under nitrogen protection, continuously stir the mixed solution B and heat it to 78° C., add the mixed solution A dropwise to the mixed solution B over 5 min, continue to heat it to 88° C., and keep it warm for 10 min to obtain an acrylate prepolymer A;

[0076] S2. Weigh 0.24 g of lauroyl peroxide and 21.6 g of ethyl acetate and mix them evenly to form a mixed solution C. The mixed solution C was added dropwise to the acrylate prepolymer A over a period of 2 h, and the mixture was kept at reflux for 2 h to obtain an acrylate prepolymer B.

[0077] S3. Weigh 0.04 g of lauroyl peroxide and 24.8 g of ethyl acetate and mix them evenly to form a mixed solution D. Add the mixed solution D dropwise into the acrylate prepolymer B over 20 min, and keep it warm for 3 h while maintaining reflux. Then cool it to 50°C, add 56.9 g of ethyl acetate and mix them evenly. Remove the nitrogen to obtain a solvent-based acrylic resin.

[0078] Comparative Example 3

[0079] Synthesis of solvent-based acrylic resin:

[0080] S1. Weigh 0.06 g of lauroyl peroxide and 5 g of ethyl acetate and mix them evenly to form a mixed solution A, weigh 118 g of butyl acrylate, 51.4 g of isooctyl acrylate, 48.6 g of vinyl acetate, 10 g of isobornyl acrylate, 6 g of acrylic acid, 11 g of hydroxyethyl acrylate, 3 g of 3,4-epoxycyclohexyl methacrylate, and 266.7 g of ethyl acetate, add them into a reactor and mix them evenly to form a mixed solution B, under nitrogen protection, continuously stir the mixed solution B and heat it to 78° C., add the mixed solution A dropwise to the mixed solution B over 5 min, continue to heat it to 90° C., and keep it warm for 10 min to obtain an acrylate prepolymer A;

[0081] S2. The acrylate prepolymer A was cooled to 67° C., 0.24 g of lauroyl peroxide and 21.6 g of ethyl acetate were weighed and mixed to form a mixed solution C, and the mixed solution C was added dropwise to the acrylate prepolymer A over 2 h, and the mixture was kept warm for 2 h to obtain an acrylate prepolymer B;

[0082] S3. Weigh 0.04 g of azobisisoheptanenitrile and 24.8 g of ethyl acetate and mix them evenly to form a mixed solution D. Add the mixed solution D dropwise into the acrylate prepolymer B over 20 min, raise the temperature to 78°C, keep the temperature for 3 h, then cool down to 50°C, add 56.9 g of ethyl acetate and mix evenly, remove the nitrogen, and obtain a solvent-based acrylic resin.

[0083] Comparative Example 4

[0084] The preparation method of the solvent-based acrylic resin in this comparative example is consistent with that in Example 1, wherein this comparative example does not contain epoxy monomer, that is, does not contain 3,4-epoxycyclohexyl methacrylate, and the rest is consistent with that in Example 1.

[0085] Comparative Example 5

[0086] The preparation method of the solvent-based acrylic resin in this comparative example is consistent with that in Example 1, wherein this comparative example does not contain a functional monomer, that is, does not contain acrylic acid and hydroxyethyl acrylate, and the rest is consistent with that in Example 1.

[0087] Comparative Example 6

[0088] Synthesis of solvent-based acrylic resin:

[0089] S1. Weigh 0.06 g of azobisisoheptanonitrile and 5 g of ethyl acetate and mix them evenly to form a mixed solution A, weigh 105 g of butyl acrylate, 51.4 g of isooctyl acrylate, 48.6 g of vinyl acetate, 10 g of isobornyl acrylate, 6 g of acrylic acid, 11 g of hydroxyethyl acrylate, 18 g of 3,4-epoxycyclohexyl methacrylate, and 266.7 g of ethyl acetate, add them into a reactor and mix them evenly to form a mixed solution B, under nitrogen protection, stir the mixed solution B continuously and heat it to 78° C., add the mixed solution A dropwise to the mixed solution B over 5 min, continue to heat it to 88° C., and keep it warm for 10 min to obtain an acrylate prepolymer A;

[0090] S2. The acrylate prepolymer A was cooled to 67° C., 0.24 g of azobisisoheptanenitrile and 21.6 g of ethyl acetate were weighed and mixed to form a mixed solution C, and the mixed solution C was added dropwise to the acrylate prepolymer A over 2 h, and the mixture was kept warm for 2 h to obtain an acrylate prepolymer B;

[0091] S3. Weigh 0.04 g of lauroyl peroxide and 24.8 g of ethyl acetate and mix them evenly to form a mixed solution D, add the mixed solution D dropwise into the acrylate prepolymer B over 20 min, heat it to 78°C, keep it warm for 3 h, then cool it to 50°C, add 56.9 g of ethyl acetate and mix evenly, remove nitrogen, and obtain a solvent-based acrylic resin.

[0092] Example 6

[0093] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this embodiment is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, as shown in FIG. Figure 1 .

[0094] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this embodiment is as follows: weigh 100g of the solvent-based acrylic resin in Example 1, and mix them evenly with 2.5g of butylated melamine formaldehyde resin, 0.3g of CVC GA240, and 0.07g of p-toluenesulfonic acid, respectively, and apply them on the corona surface of the base film layer 1, bake at 130°C for 3min, obtain the cured pressure sensitive adhesive layer 2, and then bond it to the release film layer 2 to obtain the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape, and the thickness of the pressure sensitive adhesive layer 2 is 19±1μm. When the tape is used, tear off the release film layer 2. Among them, the materials of the base film layer 1 and the release film layer 2 in this embodiment are both PET, that is, polyethylene terephthalate.

[0095] Example 7

[0096] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this embodiment is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, as shown in FIG. Figure 1 .

[0097] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this embodiment is consistent with that in Embodiment 6, wherein the solvent-based acrylic resin used in this embodiment is the solvent-based acrylic resin prepared in Embodiment 2, and the rest is consistent with that in Embodiment 6.

[0098] Example 8

[0099] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this embodiment is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, as shown in FIG. Figure 1 .

[0100] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this embodiment is consistent with that in Embodiment 6, wherein the solvent-based acrylic resin used in this embodiment is the solvent-based acrylic resin prepared in Embodiment 3, and the rest is consistent with that in Embodiment 6.

[0101] Example 9

[0102] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this embodiment is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, as shown in FIG. Figure 1 .

[0103] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this embodiment is consistent with that in Embodiment 6, wherein the solvent-based acrylic resin used in this embodiment is the solvent-based acrylic resin prepared in Embodiment 4, and the rest is consistent with that in Embodiment 6.

[0104] Example 10

[0105] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this embodiment is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, as shown in FIG. Figure 1 .

[0106] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this embodiment is consistent with that in Embodiment 6, wherein the solvent-based acrylic resin used in this embodiment is the solvent-based acrylic resin prepared in Embodiment 5, and the rest is consistent with that in Embodiment 6.

[0107] Comparative Example 7

[0108] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this embodiment is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, as shown in FIG. Figure 1 .

[0109] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this comparative example is as follows: weigh 100g of the solvent-based acrylic resin in comparative example 1, and mix them evenly with 2.5g of butylated melamine formaldehyde resin, 0.3g of CVC GA240, and 0.07g of p-toluenesulfonic acid, respectively, and apply them on the corona surface of the base film layer 1, bake at 130°C for 3min, obtain the cured pressure sensitive adhesive layer 2, and then bond it to the release film layer 2 to obtain the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape, and the thickness of the pressure sensitive adhesive layer 2 is 19±1μm. When the tape is used, tear off the release film layer 2. Among them, the materials of the base film layer 1 and the release film layer 2 in this comparative example are both PET, that is, polyethylene terephthalate.

[0110] Comparative Example 8

[0111] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this comparative example is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, Figure 1 .

[0112] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this comparative example is the same as that in comparative example 7, wherein the solvent-based acrylic resin used in this comparative example is the solvent-based acrylic resin prepared in comparative example 2, and the rest is the same as that in comparative example 7.

[0113] Comparative Example 9

[0114] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this comparative example is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, Figure 1 .

[0115] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this comparative example is the same as that in comparative example 7, wherein the solvent-based acrylic resin used in this comparative example is the solvent-based acrylic resin prepared in comparative example 3, and the rest is the same as that in comparative example 7.

[0116] Comparative Example 10

[0117] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this comparative example is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, Figure 1 .

[0118] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this comparative example is the same as that in comparative example 7, wherein the solvent-based acrylic resin used in this comparative example is the solvent-based acrylic resin prepared in comparative example 4, and the rest is the same as that in comparative example 7.

[0119] Comparative Example 11

[0120] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this comparative example is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, Figure 1 .

[0121] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this comparative example is the same as that in comparative example 7, wherein the solvent-based acrylic resin used in this comparative example is the solvent-based acrylic resin prepared in comparative example 5, and the rest is the same as that in comparative example 7.

[0122] Comparative Example 12

[0123] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this comparative example is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, Figure 1 .

[0124] The method for preparing the high temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this comparative example is the same as that in comparative example 7, wherein the solvent-based acrylic resin used in this comparative example is the solvent-based acrylic resin prepared in comparative example 6, and the rest is the same as that in comparative example 7.

[0125] Comparative Example 13

[0126] The high temperature and electrolyte resistant pressure sensitive adhesive tape in this comparative example is composed of a base film layer 1, a pressure sensitive adhesive layer 2, and a release film layer 3, Figure 1 .

[0127] The method for preparing the high-temperature resistant and electrolyte resistant pressure sensitive adhesive tape in this comparative example is consistent with that in comparative example 7, wherein the solvent-based acrylic resin used in this comparative example is a commercially available solvent-based acrylic resin having a viscosity of about 10,000 to 12,000 mPa·s and a solid content of 40%, and the rest is consistent with comparative example 7.

[0128] Test Case

[0129] 1. Experimental Construction Method

[0130] (1) The solvent-based acrylic resins in Examples 1 to 5 and Comparative Examples 1 to 6 were characterized by solid content, monomer conversion rate, and viscosity.

[0131] (2) The pressure-sensitive adhesives in Examples 6 to 10 and Comparative Examples 7 to 13 were subjected to high temperature resistance and electrolyte resistance performance tests.

[0132] 2. Experimental results

[0133] (1) Characterization of solvent-based acrylic resin parameters

[0134] Table 1 below shows the characterization results of relevant parameters of the solvent-based acrylic resins in Examples 1 to 5 and Comparative Examples 1 to 6.

[0135] Table 1 Characterization of parameters of solvent-based acrylic resins in Examples 1 to 5 and Comparative Examples 1 to 6

[0136] parameter Solid content (%) Monomer conversion rate (%) Viscosity (mPa·s) Example 1 39.8 99.5 12225 Example 2 39.84 99.6 11569 Example 3 39.86 99.7 12014 Example 4 39.78 99.5 11687 Example 5 39.81 99.6 11902 Comparative Example 1 39.6 99 11399 Comparative Example 2 39.92 99.8 3922 Comparative Example 3 39.8 99.5 11228 Comparative Example 4 39.6 99.4 11016 Comparative Example 5 39.7 99.6 12011 Comparative Example 6 39.5 99.1 4502

[0137] (2) Test and characterization of high temperature and electrolyte resistance of pressure-sensitive adhesive tape

[0138] Table 2 below shows the results of characterization of the high temperature resistance and electrolyte resistance of the pressure-sensitive adhesive tapes in Examples 6 to 10 and Comparative Examples 7 to 13.

[0139] Table 2 Characterization results of high temperature resistance and electrolyte resistance of pressure-sensitive adhesive tapes in Examples 6 to 10 and Comparative Examples 7 to 13

[0140]

[0141]

[0142] As shown in Table 1 and Table 2, the solvent-based acrylic resins in Examples 1 to 5 all have high solid content and high monomer conversion rate, and moderate viscosity, between 11000 and 13000 Pa·s, and the pressure-sensitive adhesive tapes prepared using the solvent-based acrylic resins in Examples 1 to 5 all have good high temperature resistance and electrolyte resistance, refer to the performance data of the pressure-sensitive adhesive tapes in Examples 6 to 10. The initiators used in the reaction process in Comparative Examples 1 and 2 are all the same initiators, the monomer conversion rate in the acrylic resin prepared in Comparative Example 1 is low, and the resin contains the smell of the monomer; while the acrylic resin prepared in Comparative Example 2 has a low viscosity, so the pressure-sensitive adhesive tape prepared using it has residual adhesive after tearing the adhesive at high temperature, refer to the performance data of the pressure-sensitive adhesive tape in Comparative Example 9. The acrylic monomers in Comparative Examples 3 and 4 contain a small amount of epoxy monomers or no epoxy monomers, so the obtained acrylic resins are not tightly cross-linked, and the high temperature resistance and electrolyte resistance of the pressure-sensitive adhesive tapes prepared using them are reduced, and residual adhesive appears at high temperatures. After soaking in the electrolyte, the peeling force on the aluminum foil is significantly smaller, refer to the performance data of the pressure-sensitive adhesive tapes in Comparative Examples 9-10. The acrylic monomers in Comparative Example 5 do not contain functional monomers, so the obtained acrylic resin cannot undergo a cross-linking reaction, has poor cohesion, and is easily swollen and dissolved, and has poor adhesion and peeling properties. Therefore, the pressure-sensitive adhesive tape prepared using it has residual adhesive at high temperatures, refer to the performance data of the pressure-sensitive adhesive tape in Example 11. The use order of the low-activity initiator and the high-activity initiator in Comparative Example 6 is changed, resulting in a lower viscosity of the acrylic resin and a lower monomer conversion rate, so the pressure-sensitive adhesive tape prepared using it has lower high temperature resistance and electrolyte resistance, refer to the performance data of the pressure-sensitive adhesive tape in Example 12. The pressure-sensitive adhesive tape in Comparative Example 13 was prepared by using a commercially available solvent-based acrylic resin, and residual adhesive appeared after being soaked in electrolyte.

[0143] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. A solvent-based acrylic resin, characterized in that: Calculated by weight, it is composed of the following components: 220-280 parts of acrylic monomer, 0.2-0.4 parts of initiator, and 360-380 parts of organic solvent; The acrylic monomers include soft monomers, hard monomers, epoxy monomers and functional monomers; wherein the mass ratio of the soft monomers to the hard monomers is 150-170:40-60; The epoxy monomer is 3,4-epoxycyclohexyl methacrylate, and the mass percentage of the epoxy monomer in the acrylic monomer is not less than 5.36%; The functional monomer contains at least one of a hydroxyl functional group and a carboxyl functional group, and the mass percentage of the functional monomer in the acrylic monomer is not less than 5.36%; The solvent-based acrylate is prepared according to the method: S1. Mixing the first part of the initiator A with the first part of the organic solvent to form a mixed solution A, uniformly mixing the acrylate monomer with the second part of the organic solvent to form a mixed solution B, heating the mixed solution B to 75-80° C., keeping the temperature, adding the mixed solution A to the mixed solution B, and continuing to heat to 85-90° C., keeping the temperature for 8-13 minutes to obtain an acrylate prepolymer A; S2. Cooling the acrylate prepolymer to 65-70° C., mixing the second part of the initiator A with the third part of the organic solvent to form a mixed solution C, adding the mixed solution C to the acrylate prepolymer A, and continuing to keep warm for 2-3 hours to obtain an acrylate prepolymer B; S3. The initiator B is mixed with the fourth part of the organic solvent to form a mixed solution D, the mixed solution D is added to the acrylate prepolymer B, and then the temperature is raised to 75 to 78 ° C, kept warm for 2.5 to 3.5 hours, and then cooled to 45 to 55 ° C, and the fifth part of the organic solvent is added thereto to obtain a solvent-based acrylic resin; Among them, the reaction activity of initiator A is lower than that of initiator B; the total amount of initiator A is equal to the sum of the masses of the first part of initiator A and the second part of initiator A; the total amount of the organic solvent is equal to the sum of the masses of the first part of organic solvent, the second part of organic solvent, the third part of organic solvent, the fourth part of organic solvent, and the fifth part of organic solvent.

2. The solvent-based acrylic resin according to claim 1, characterized in that: The mass ratio of the first part initiator A, the second part initiator A and the initiator B is 1-2:5-7:1; the mass ratio of the first part solvent, the second part solvent, the third part solvent, the fourth part solvent and the fifth part solvent is 255-270:5-10:20-30:15-30:50-70.

3. The solvent-based acrylic resin according to claim 2, characterized in that: The initiator A includes at least one of lauroyl peroxide and azobisisobutyronitrile, and the initiator B includes at least one of azobisisoheptanenitrile and tert-butyl peroxy-2-ethylhexanoate; The organic solvent includes at least one of ethyl acetate, butanone and toluene.

4. A high temperature resistant and electrolytic resistant pressure sensitive adhesive, characterized in that: The method is prepared by using the solvent-based acrylic resin as described in any one of claims 1 to 3.

5. The high temperature and electrolyte resistant pressure sensitive adhesive as claimed in claim 4, characterized in that: Calculated by weight, the invention is prepared by mixing 90-98 parts of solvent-based acrylic resin, 1-4 parts of amino resin, 0.01-1 part of catalyst and 0.1-1 part of epoxy curing agent.

6. The high temperature and electrolyte resistant pressure sensitive adhesive as claimed in claim 5, characterized in that: The amino resin includes at least one of butylated melamine formaldehyde resin, isobutylated melamine formaldehyde resin and methylated melamine formaldehyde resin.

7. A high temperature resistant and electrolytically resistant pressure sensitive adhesive tape, characterized in that: The release film layer, the pressure-sensitive adhesive layer and the base film layer are compounded in sequence, and the pressure-sensitive adhesive layer is obtained by coating the high temperature resistant and electrolytic resistant pressure-sensitive adhesive as claimed in claim 4 on the base film layer and then heat curing it.