Application and electroplating solution of 3,3′-disulfanediylbis(pyridin-2-amine)

By using 3,3'-disulfanediylbis(pyridine-2-amine) as leveling agent in acidic copper sulfate plating solution, the problem of unevenness of through-hole electroplating is solved and better electroplating uniformity is achieved and electronic product reliability.

CN115404524BActive Publication Date: 2024-11-12JIHUA LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110592994.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-28
Publication Date
2024-11-12
Estimated Expiration
2041-05-28

AI Technical Summary

Technical Problem

The existing acidic copper sulfate plating solution system has unevenness problems in through-hole electroplating, resulting in a decrease in reliability of electronic products. The effect of 2,2'-dithiodipyridine as a leveling agent is still insufficient to improve the through-hole electroplating effect.

Method used

3,3'-disulfanediylbis(pyridine-2-amine) is introduced as the electroplating copper leveling agent, and the surface copper deposition is inhibited by its amino groups, reducing copper deposition in the pores, thereby achieving through-hole uniform electroplating.

Benefits of technology

By using 3,3'-disulfanediylbis(pyridin-2-amine) leveling agent, copper deposition in high current density areas is effectively suppressed, and the uniformity and reliability of through-hole electroplating are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115404524B_ABST
    Figure CN115404524B_ABST
Patent Text Reader

Abstract

The present invention discloses the application of 3,3'-disulfanediylbis(pyridine-2-amine) and an electroplating solution, and uses 3,3'-disulfanediylbis(pyridine-2-amine) as an electroplating copper leveler. The present invention proposes to use 3,3'-disulfanediylbis(pyridine-2-amine) as a leveler, introduce amino groups, inhibit the deposition of surface copper, and affect the deposition of copper in the hole to a lesser extent, thereby achieving the purpose of uniform electroplating of through holes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electroplating solution, and mainly to the application of 3,3'-disulfanediylbis(pyridine-2-amine) and electroplating solution. Background Art

[0002] The rapid development of electronic products has put forward higher requirements for the production of printed circuit boards. The light and short product characteristics have prompted PCB boards to develop from single-sided boards to double-sided boards and multi-layer boards, and finally to high-density interconnection boards. The acid copper sulfate plating solution system is the mainstream of copper electroplating technology. The copper deposition can be regulated by compounding additives and uniform electroplating of electrical interconnection structures can be achieved.

[0003] The geometric shape of the through-hole causes the uneven distribution of current, and the difference in convection intensity brings greater challenges to through-hole electroplating, especially the uniformity of through-hole electroplating with a large aperture ratio. Uneven through-holes will greatly reduce the reliability of electronic products. In order to solve the problem of through-hole electroplating uniformity, it is necessary to introduce additives to redistribute the current and use the disadvantage of convection difference to convert it into an advantage: inhibit the deposition of surface copper and affect the deposition of copper in the hole to a lesser extent, so as to achieve the purpose of through-hole uniformity electroplating.

[0004] In the acid copper sulfate plating system, the basic plating solution consists only of copper sulfate pentahydrate (CuSO 4∙ 5H2O) and sulfuric acid, CuSO4∙5H2O as the copper source, sulfuric acid is used to improve the conductivity of the plating solution. In the acidic copper sulfate plating solution system, the quality of the copper layer plated by the basic components alone is far from the required target, so different additives need to be added to achieve a higher dispersibility of the plating solution and form a uniform and fine copper plating layer. In the prior art, it is mentioned that 2,2'-dithiodipyridine is used. It is added to the copper sulfate plating solution as a leveling agent, but its through-hole electroplating effect still needs to be improved. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide an application of 3,3'-disulfanediylbis(pyridin-2-amine) and an electroplating solution, aiming to provide a new leveler suitable for through-hole electroplating.

[0006] The technical solution of the present invention is as follows:

[0007] Application of 3,3'-disulfanediylbis(pyridine-2-amine), wherein 3,3'-disulfanediylbis(pyridine-2-amine) is used as a copper electroplating leveler, and the chemical structure of 3,3'-disulfanediylbis(pyridine-2-amine) is .

[0008] A plating solution, wherein the plating solution is used for through-hole electroplating, the plating solution contains a leveler, and the leveler is 3,3'-disulfanediylbis(pyridine-2-amine), and the chemical structural formula is .

[0009] The electroplating solution, wherein the concentration of the leveler in the electroplating solution is 0.5-30 ppm.

[0010] The electroplating solution further comprises an accelerator and an inhibitor.

[0011] In the electroplating solution, the accelerator is one of SPS or MPS.

[0012] The electroplating solution, wherein the inhibitor is one or more of 3-aminobenzaldehyde polymer, PEG, polymer of divinylbenzene and sodium vinylbenzene sulfonate, PPG, L-glutamic acid polymer, 4-aminobenzaldehyde polymer, and EPE.

[0013] The electroplating solution, wherein the concentration range of the inhibitor is 200-600 ppm, and the concentration range of the accelerator is 0.5-20 ppm.

[0014] In the electroplating solution, the accelerator is one of SPS or MPS, and the inhibitor is one or two of PEG, L-glutamic acid polymer or 3-aminobenzaldehyde polymer.

[0015] The electroplating solution further comprises the following components:

[0016] Copper sulfate pentahydrate 90-110 g / L, sulfuric acid 140-160 g / L, chloride ion concentration 60-80 mg / L.

[0017] The electroplating solution comprises the following components:

[0018] 3,3'-disulfanediylbis(pyridin-2-amine) 0.5-30 ppm, accelerator SPS 0.5-20 ppm, inhibitor PEG6000 200-300 ppm, inhibitor L-glutamic acid polymer or 3-aminobenzaldehyde polymer 100-200 ppm, copper sulfate pentahydrate 100 g / L, sulfuric acid 150 g / L, chloride ion concentration 70 ppm.

[0019] Beneficial effect: The present invention provides a new application of 3,3'-disulfanediylbis(pyridine-2-amine), which is used as a copper electroplating leveler. By introducing amino groups, the deposition of copper on the surface is inhibited while the deposition of copper in the hole is affected to a lesser extent, thereby achieving the purpose of uniform through-hole electroplating. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the electroplating effect of Example 1 of the present invention.

[0021] Figure 2 This is the electroplating effect of Example 2 of the present invention.

[0022] Figure 3 This is the electroplating effect of Example 3 of the present invention.

[0023] Figure 4 This is the electroplating effect of the comparative example. DETAILED DESCRIPTION

[0024] The present invention provides the application of 3,3'-disulfanediylbis(pyridin-2-amine) and electroplating solution. To make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0025] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.

[0026] In order to complete the through-hole in the HDI printed circuit board, the present invention proposes an application of 3,3'-disulfanediylbis(pyridine-2-amine), and uses 3,3'-disulfanediylbis(pyridine-2-amine) as a copper electroplating leveler. The chemical structure of 3,3'-disulfanediylbis(pyridine-2-amine) is shown in formula (1).

[0027] Formula (1).

[0028] The present invention overcomes the poor through-hole electroplating effect, proposes to use 3,3'-disulfanediylbis(pyridine-2-amine) as a leveler, and introduces amino groups to inhibit the deposition of surface copper while affecting the deposition of copper in the hole to a lesser extent, thereby achieving the purpose of uniform through-hole electroplating. The amino group can enhance the adsorption of the leveler on the copper surface and effectively inhibit copper deposition in high current density areas. Therefore, 3,3'-disulfanediylbis(pyridine-2-amine) is particularly suitable for use as a copper electroplating leveler for through-hole electroplating.

[0029] The present invention also provides an electroplating solution, which is used for through-hole electroplating, and contains a leveler, which is 3,3'-disulfanediylbis(pyridine-2-amine). The present invention also provides a preferred concentration range of the leveler in the electroplating solution, and the concentration of the leveler in the electroplating solution is preferably 0.5-30 ppm.

[0030] Preferably, the leveler is preferably used in combination with an accelerator and an inhibitor. Therefore, the electroplating solution also includes an accelerator and an inhibitor. Combined with the accelerator and the inhibitor used in conjunction, the electroplating solution additive formula can meet the requirements of the through hole. In order to improve the through-hole electroplating effect, the present invention also provides a specific accelerator and inhibitor combination used in conjunction therewith, wherein the accelerator can be one of SPS or MPS, and the accelerator is preferably used in a concentration range of 0.5-20ppm. The inhibitor can be one or more of 3-aminobenzaldehyde polymer, PEG, a polymer of divinylbenzene and sodium vinylbenzene sulfonate, PPG, L-glutamic acid polymer, 4-aminobenzaldehyde polymer, and EPE. The concentration range of the inhibitor is preferably 200-600 ppm, and more preferably 200-500 ppm.

[0031] Preferably, the accelerator is one of SPS or MPS, and the inhibitor is one or two of PEG, L-glutamic acid polymer or 3-aminobenzaldehyde polymer. This combination can achieve better through-hole electroplating effect. The leveler interacts with the accelerator and the inhibitor. The leveler and the accelerator have an antagonistic effect, which can hinder the adsorption of the accelerator at the orifice and reduce the copper deposition rate at the orifice. The leveler and the inhibitor synergistically adsorb on the copper surface in the high current density area to isolate the copper ions from being reduced here.

[0032] Furthermore, the electroplating solution also includes the following components:

[0033] Copper sulfate pentahydrate 90-110 g / L, sulfuric acid 140-160 g / L, chloride ion concentration 60-80 mg / L.

[0034] Using a high-acid, low-copper system in the electroplating solution with the above concentration can effectively improve the conductivity of the electroplating solution, which is beneficial to the uniform deposition of copper ions on the copper surface.

[0035] The present invention also provides a most preferred electroplating solution, comprising the following components:

[0036] 3,3'-disulfanediylbis(pyridin-2-amine) 0.5-30 ppm, accelerator SPS 0.5-20 ppm, inhibitor PEG6000 200-300 ppm, inhibitor L-glutamic acid polymer or 3-aminobenzaldehyde polymer 100-200 ppm, copper sulfate pentahydrate 100 g / L, sulfuric acid 150 g / L, chloride ion concentration 70 ppm.

[0037] The present invention is further described below by means of specific examples.

[0038] Example 1

[0039] A plating solution is provided, comprising: 100 g / L copper sulfate pentahydrate, 150 g / L sulfuric acid, 70 ppm chloride ion concentration, and additives: 2 ppm of leveling agent 3,3'-disulfanediylbis(pyridine-2-amine), 4 ppm of accelerator SPS, 300 ppm of inhibitor PEG6000, and 100 ppm of L-glutamic acid polymer.

[0040] The hole diameter in the through-hole test board is 15μm and the hole depth is 90μm. The through-hole can be completely filled by electroplating with a current density of 10 ASD for 50 min. The electroplating effect is as follows: Figure 1 shown.

[0041] Example 2

[0042] A plating solution is provided, comprising: 100 g / L copper sulfate pentahydrate, 150 g / L sulfuric acid, 70 ppm chloride ion concentration, and additives: 6 ppm of leveling agent 3,3'-disulfanediylbis(pyridine-2-amine), 5 ppm of accelerator SPS, 300 ppm of inhibitor PEG6000, and 200 ppm of 3-aminobenzaldehyde polymer.

[0043] The hole diameter in the through-hole test board is 15μm and the hole depth is 90μm. The through-hole can be completely filled by electroplating with a current density of 10 ASD for 50 min. The electroplating effect is as follows: Figure 2 shown.

[0044] Example 3

[0045] A plating solution is provided, wherein the plating solution is prepared as follows: 100 g / L copper sulfate pentahydrate, 150 g / L sulfuric acid, 70 ppm chloride ion concentration, and additives are added: 4 ppm of leveling agent 3,3'-disulfanediylbis(pyridine-2-amine), 5 ppm of accelerator SPS, and 300 ppm of inhibitor PEG6000.

[0046] The hole diameter in the through-hole test board is 15μm and the hole depth is 90μm. The through-hole can be completely filled by electroplating with a current density of 10 ASD for 50 min. The electroplating effect is as follows: Figure 3 shown.

[0047] Comparative Example

[0048] A plating solution is prepared by mixing: 100 g / L copper sulfate pentahydrate, 150 g / L sulfuric acid, 70 ppm chloride ion concentration, and adding: 5 ppm leveler JGB, 4 ppm accelerator SPS, 300 ppm inhibitor PEG6000, and 100 ppm L-glutamic acid polymer.

[0049] The hole diameter in the through-hole test board is 15μm and the hole depth is 90μm. The through-hole is not completely filled when electroplated with a current density of 10 ASD for 50 min. The electroplating effect is as follows: Figure 4 shown.

[0050] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. The use of 3,3'-disulfanediylbis(pyridin-2-amine), characterized in that: 3,3'-disulfanediylbis(pyridine-2-amine) is used as a copper electroplating leveler. The chemical structure of 3,3'-disulfanediylbis(pyridine-2-amine) is: .

2. An electroplating solution, characterized in that: The electroplating solution is used for through-hole electroplating. The electroplating solution contains a leveler. The leveler is 3,3'-disulfanediylbis(pyridine-2-amine) having a chemical structural formula of .

3. The electroplating solution according to claim 2, characterized in that The concentration of the leveler in the electroplating solution is 0.5-30 ppm.

4. The electroplating solution according to claim 2, characterized in that: The electroplating solution also includes an accelerator and a suppressor.

5. The electroplating solution according to claim 4, characterized in that: The accelerator is one of SPS or MPS.

6. The electroplating solution according to claim 4, characterized in that The inhibitor is one or more of 3-aminobenzaldehyde polymer, PEG, polymer of divinylbenzene and sodium vinylbenzene sulfonate, PPG, L-glutamic acid polymer, 4-aminobenzaldehyde polymer and EPE.

7. The electroplating solution according to claim 4, characterized in that The concentration range of the inhibitor is 200-600 ppm, and the concentration range of the accelerator is 0.5-20 ppm.

8. The electroplating solution according to claim 4, characterized in that The accelerator is one of SPS or MPS, and the inhibitor is one or two of PEG, L-glutamic acid polymer or 3-aminobenzaldehyde polymer.

9. The electroplating solution according to claim 2, characterized in that: The electroplating solution also includes the following components: Copper sulfate pentahydrate 90-110 g / L, sulfuric acid 140-160 g / L, chloride ion concentration 60-80 mg / L.

10. The electroplating solution according to claim 2, characterized in that: The electroplating solution includes the following components: 3,3'-disulfanediylbis(pyridin-2-amine) 0.5-30 ppm, accelerator SPS 0.5-20 ppm, inhibitor PEG6000 200-300 ppm, inhibitor L-glutamic acid polymer or 3-aminobenzaldehyde polymer 100-200 ppm, copper sulfate pentahydrate 100 g / L, sulfuric acid 150 g / L, chloride ion concentration 70 ppm.