Knife and method for manufacturing knife

By alternately arranging branch layers with different hardness along the length direction of kitchen knives, a layered composite structure and a micro-serrated edge are formed, which solves the problem of bending and sharpness loss of the knife edge, and achieves longer-lasting sharpness.

CN115416053BActive Publication Date: 2024-10-18WUHAN SUPOR COOKWARE
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202211194291.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-28
Publication Date
2024-10-18
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

The cutting edges of existing kitchen knives are prone to bending and loss of sharpness during use, and the existing hard coating cannot meet the demand for lasting sharpness after wear.

Method used

Multiple branch layers with alternating high and low hardness are formed along the length of the tool to form a layered composite structure. During polishing, each branch layer has different amounts of wear due to different hardnesses, forming a micro-serrated structure to improve the sharpness and durability of the edge. .

Benefits of technology

It effectively avoids the bending of the cutting edge, improves the sharpness and long-lasting sharpness of the tool, and ensures that the cutting edge can still regain its sharpness after each polishing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115416053B_ABST
    Figure CN115416053B_ABST
Patent Text Reader

Abstract

The present application provides a tool and a method for manufacturing the tool. The tool has a layered composite structure along the length direction, the layered composite structure is formed by a plurality of branch layers with different hardnesses alternately stacked along the length direction, the hardness of the plurality of branch layers is arranged alternately in high and low positions along the length direction of the tool, and the layered composite structure at least constitutes the cutting edge of the tool, wherein the cutting edge has a micro-serrated structure. The tool manufactured according to the present application can be kept sharp for a long time and is not prone to edge curling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of kitchen knives, and in particular to a knife and a method for manufacturing the knife. Background Art

[0002] Knives are one of the essential tools in kitchen equipment. The sharpness of knives is an important factor that characterizes the performance of knives. The materials used to make knives are usually stainless steel. During daily use, the cutting edge of knives made of this material will inevitably hit hard materials (such as cutting boards, bones), and after using them for a period of time, obvious bending (i.e., curling) will occur at the cutting edge. In addition, the sharpness of the cutting edge will significantly decrease after a short period of use, which cannot meet the needs of consumers.

[0003] Therefore, in the prior art, a hard alloy is placed on the surface of the tool to form a hard coating, and the hard coating is used to improve the long-term sharpness of the tool. However, after the hard coating is worn, the long-term sharpness of the tool will drop sharply, so this method still cannot meet the use needs of consumers. Summary of the invention

[0004] Therefore, the purpose of the present application is to provide a tool and a method for manufacturing a tool to solve the problem of poor long-term sharpness of tools in the prior art. A plurality of branch layers with alternating hardness are formed along the length direction of the tool. The tool is formed by the plurality of branch layers. When the tool is grinded along the thickness direction, under the same grinding conditions, each branch layer has different wear amounts in the length direction due to different hardnesses, which is conducive to forming a cutting edge portion with a micro-serrated structure along the length direction to improve the sharpness. Since the cutting edge portion of the tool is in the form of a layered composite structure along the thickness direction, it can regain sharpness after each grinding, thereby improving the long-term sharpness performance.

[0005] According to the first aspect of the present application, a tool is provided, which has a layered composite structure along the length direction, and the layered composite structure is formed by a plurality of branch layers alternately stacked along the length direction, and the hardness of the plurality of branch layers is arranged alternately in high and low patterns along the length direction, and the layered composite structure at least constitutes the cutting edge portion of the tool, and the cutting edge portion of the tool has a micro-serrated structure.

[0006] In an embodiment, the plurality of branch layers have the same thickness, and the plurality of branch layers are formed by stacking a plurality of identical layered units, wherein each layered unit includes an even number of layers.

[0007] In an embodiment, the plurality of branch layers are formed of a plurality of iron alloy materials with a hardness difference of 1-10 HRC; and the thickness of each branch layer is 500 μm-700 μm.

[0008] According to a second aspect of the present application, a method for manufacturing a tool is provided, the method for manufacturing a tool comprising:

[0009] A raw material block having a layered composite structure along a width direction is formed, wherein the layered composite structure is formed by a plurality of branch layers alternately stacked along the width direction, and the hardness of the plurality of branch layers is alternately arranged in high and low positions along the length direction; the raw material block is molded along the width direction to obtain a tool blank having the layered composite structure in the length direction; the tool blank is polished to obtain a tool having a cutting edge portion with a micro-serrated structure formed by the layered composite structure in the length direction.

[0010] In an embodiment, the step of forming a raw material block includes: providing a plurality of ferroalloy materials, and arranging the plurality of ferroalloy materials alternately according to hardness; sequentially using the plurality of ferroalloy materials to perform 1st, 2nd, ..., Nth spraying respectively to form 1st, 2nd, ..., Nth branch layers respectively, thereby obtaining a raw material block having a layered composite structure, wherein N is a positive integer not less than 100.

[0011] In an embodiment, a pre-pressing treatment step is performed after each 1st, 2nd, ..., N-1th spraying; after the Nth spraying, a hot isostatic pressing sintering process is performed on the formed raw material block with a layered composite structure, so that adjacent layers are embedded with each other and adjacent particles of each branch layer have predetermined pores.

[0012] In an embodiment, the multiple branch layers are formed by stacking a plurality of identical layered units, each layered unit includes a first sublayer and a second sublayer, and the steps of forming each layered unit include: providing a first ferroalloy material, and spraying the first ferroalloy material to form a first sublayer; providing a second ferroalloy material, and spraying the second ferroalloy material on the first sublayer to form a second sublayer, wherein the hardness of the first ferroalloy material and the second ferroalloy material are different.

[0013] In an embodiment, the thickness of the first sublayer is the same as the thickness of the second sublayer, wherein the hardness of the first ferroalloy material is greater than the hardness of the second ferroalloy material and the particle size of the first ferroalloy material is smaller than the particle size of the second ferroalloy material; or, the hardness of the first ferroalloy material is less than the hardness of the second ferroalloy material and the particle size of the first ferroalloy material is greater than the particle size of the second ferroalloy material.

[0014] In an embodiment, the difference between the particle size of the first ferroalloy material and the particle size of the second ferroalloy material is 10μm-60μm, the particle size of one of the first ferroalloy material and the second ferroalloy material is 70μm-100μm, and the particle size of the other of the first ferroalloy material and the second ferroalloy material is 40μm-60μm.

[0015] In an embodiment, before the step of grinding the tool blank, the method for manufacturing a tool further comprises: roll forging the tool blank at a predetermined temperature along the length direction of the tool blank so that the various branch layers of the tool blank are interlocked with each other.

[0016] In an embodiment, the ferroalloy material includes at least two martensitic stainless steel materials selected from 3Cr13, 4Cr13, 5Cr15MoV, 6Cr13MoV, 7Cr17MoV and 102Cr17MoV.

[0017] According to the tool of the present application, by forming multiple branch layers with alternating hardness along the length direction of the tool, when the tool is ground along the thickness direction, under the same grinding conditions, each branch layer has different grinding amounts due to different hardness along the length direction, so that a tool with a micro-serrated structure on the cutting edge can be formed. On the one hand, since the cutting edge of the micro-serrated structure is subjected to dispersed force, the "curling blade" phenomenon can be avoided. On the other hand, when the cutting edge of the micro-serrated structure hits the hard material, the force is point-forced. Compared with the continuous arc-shaped cutting edge structure with linear force, under the same force, the tip of the cutting edge of the micro-serrated structure exerts a greater pressure on the food, making it easier for the cutting edge to cut into the food, so it can have better sharpness. In addition, since the cutting edge of the tool is in the form of a layered composite structure along the thickness direction, it can regain sharpness after each grinding, thereby improving the long-lasting sharpness performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The above and other objects and features of the present application will become more apparent through the following description of the embodiments in conjunction with the accompanying drawings, in which:

[0019] Figure 1 is a schematic diagram of a top view of a raw material block according to an embodiment of the present application;

[0020] Figure 2 is a schematic structural diagram of a tool according to a first embodiment of the present application;

[0021] Figure 3 According to this application Figure 2 A schematic diagram of the enlarged structure at I in the middle;

[0022] Figure 4 is a schematic structural diagram of a tool according to a second embodiment of the present application;

[0023] Figure 5 It is a schematic structural diagram of a cutting tool according to the third embodiment of the present application. DETAILED DESCRIPTION

[0024] The inventive concepts of the present application will be more fully described hereinafter.

[0025] Iron alloy materials, such as stainless steel materials, have excellent properties such as being not easily corroded, having good hardness and being inexpensive, etc. Therefore, iron alloy materials can be used as materials for forming durable and sharp knives.

[0026] The inventor has found through research that by forming multiple branches with alternating hardness along the length direction of the tool, when the tool is ground along the thickness direction, under the same grinding conditions, the grinding amount of each branch layer will be different due to the different hardness along the length direction, so that a tool with a micro-serrated structure on the cutting edge can be formed. Since the cutting edge of the micro-serrated structure is subjected to dispersed force, the "curling blade" phenomenon can be avoided; on the other hand, when the cutting edge of the micro-serrated structure hits the hard material, the force is point-forced. Compared with the continuous arc-shaped cutting edge structure with linear force, under the same force, the tip of the cutting edge of the micro-serrated structure exerts a greater pressure on the food, making it easier for the cutting edge to cut into the food, so it can be sharp for a long time. In addition, since the cutting edge of the tool is in the form of a layered composite structure along the thickness direction, it can regain sharpness after each grinding, thereby improving the long-lasting sharpness performance.

[0027] The inventive concept of the present application will be described in detail below in conjunction with exemplary embodiments.

[0028] According to the first aspect of the present application, a tool is provided. According to the present application, the tool has a layered composite structure along the length direction, wherein the layered composite structure is formed by a plurality of branch layers stacked along the length direction of the tool, and the hardness of the plurality of branch layers is arranged alternately in high and low positions along the length direction of the tool. The layered composite structure at least constitutes the cutting edge of the tool, and the cutting edge of the tool has a micro-serrated structure.

[0029] In the embodiment of the present application, the micro-serrated structure is formed by grinding the layered composite structure.

[0030] According to the present application, the thickness of the plurality of layers is the same or similar. In an exemplary embodiment, the thickness difference between adjacent branch layers is 0-100 μm. Specifically, the thickness of each branch layer is in the range of 500 μm-700 μm.

[0031] According to the present application, the layered composite structure can be formed by any number of layers. According to one embodiment of the present application, a plurality of different iron alloy materials can be selected and arranged alternately according to the hardness to form the layered composite structure of the tool according to the present application. In these embodiments, the number of layers of the layered composite structure may not be limited. Figure 5 In the example shown, the number of layers of the layered composite structure is an odd number of layers. According to another embodiment of the present application, an even number of ferroalloy materials may be sprayed sequentially and alternately for multiple times to form the layered composite structure of the tool according to the present application.

[0032] In an exemplary embodiment, a plurality of branch layers are formed by stacking a plurality of identical layered units, wherein each layered unit is composed of an even number of layers. According to an exemplary embodiment of the present application, the number of layers included in the layered unit may be an even number not less than 50. According to an exemplary embodiment, each layered unit may include two sublayers stacked in sequence, or each layered unit may include four sublayers stacked in sequence.

[0033] Figure 2 It is a schematic structural diagram of a cutting tool according to the first embodiment of the present application. Figure 3 According to this application Figure 2 The enlarged structural diagram of I in FIG. Figure 2 As shown, the tool 20 comprises a plurality of layered units 21 stacked along the length direction, wherein each layered unit 21 comprises a first sublayer 211 and a second sublayer 212 having different hardnesses, so that the plurality of layered units 21 constitute a plurality of layers whose hardnesses are alternately arranged in high and low order along the length direction of the tool. Figure 3 As shown, the cutting edge of the tool 20 has a micro-serration structure.

[0034] Figure 4 Schematic diagram of the structure of the tool according to the second embodiment of the present application. Figure 4 As shown, each layer unit 21 includes a first sub-layer 211, a second sub-layer 212, a third sub-layer 213 and a fourth sub-layer 214 having different hardnesses.

[0035] According to the present application, the first sublayer 211 in the first layered unit 21 is disposed near the end of the knife away from the handle along the length direction. The hardness of the first sublayer 211 may be less than the hardness of the second sublayer 212, or the hardness of the first sublayer 211 may be greater than the hardness of the second sublayer 212. The present application does not impose too many restrictions on the order of the hardness of the two sublayers.

[0036] According to the present application, the branch layer has a suitable thickness and can form a regularly arranged micro-serrated structure. In an exemplary embodiment, the first sub-layer 211 and the second sub-layer 212 have the same thickness, and the two sub-layers constitute a layered unit 21. The multiple branch layers formed by stacking and connecting multiple layered units 21 have a regular alternating hardness arrangement, thereby facilitating the formation of a regular micro-serrated structure.

[0037] In order to make it easier for adjacent branch layers to form a suitable micro-serration structure during the subsequent grinding process, it is necessary to set the adjacent branch layers to have a suitable hardness difference. In an exemplary embodiment, the hardness difference of the iron alloy material used to make the adjacent branch layers can be in the range of 1-10HRC. In the actual manufacturing process, the formed branch layers have a suitable hardness difference by selecting iron alloy materials of different hardness.

[0038] In an embodiment, the height of each sawtooth of the micro-sawtooth structure is in the range of 100 μm-200 μm, and the width is in the range of 500 μm-700 μm.

[0039] As is known to all, among the materials used to make cutting tools, stainless steel is relatively easy to obtain, corrosion-resistant, and inexpensive. In the embodiment, the ferroalloy material is a stainless steel material, and each branch layer is a stainless steel layer. This will be described in detail later.

[0040] According to a second aspect of the present application, a method for manufacturing a tool is provided, the method comprising:

[0041] Step S101 , forming a raw material block having a layered composite structure along a width direction, wherein the layered composite structure is formed by a plurality of branch layers alternately stacked along the width direction, and the hardness of the plurality of branch layers is alternately arranged in high and low positions along the width direction.

[0042] Step S102 , forming the raw material block along the width direction to obtain a tool blank having a layered composite structure in the length direction.

[0043] Step S103 , grinding the tool blank to obtain a tool having a cutting edge portion with a micro-serrated structure formed by a layered composite structure in the length direction.

[0044] Hereinafter, a method for manufacturing a cutting tool according to the present application will be described in detail.

[0045] Provide ferroalloy materials

[0046] Prepare different ferroalloy materials, which can be in powder or strip form. The ferroalloy material can be a stainless steel material, specifically, a martensitic stainless steel. Martensitic stainless steel can include 3Cr13, 4Cr13, 5Cr15MoV, 6Cr13MoV, 7Cr17MoV and 102Cr17MoV. According to the present application, the higher the carbon content of the stainless steel material, the higher the hardness of the branch layer formed by it. The order of carbon content from small to large is: 3Cr13, 4Cr13, 5Cr15MoV, 6Cr13MoV, 7Cr17MoV, 102Cr17MoV.

[0047] Preparation of raw material blocks

[0048] According to the present application, the raw material block can be formed by stacking a plurality of mutually different branch layers in the width direction. Specifically, the plurality of branch layers can be formed by stacking and connecting a plurality of identical layered units in the width direction. The following first introduces an example of forming a raw material block by stacking and connecting a plurality of mutually different branch layers in the width direction.

[0049] According to the present application, the ferroalloy material may be in a granular form, and a raw material block having a layered composite structure is formed by stacking and connecting a plurality of branch layers in the width direction, and the steps of making the raw material block include: providing a plurality of ferroalloy materials and arranging the plurality of ferroalloy materials alternately according to the hardness; sequentially using a plurality of ferroalloy materials for the 1st, 2nd, ..., Nth spraying to form the 1st, 2nd, ..., Nth branch layers respectively, thereby forming a raw material block having a layered composite structure, wherein N is a positive integer not less than 100. It should be noted here that the number of layers in the accompanying drawings of the present invention is only exemplary and is not shown in reality. It should be noted that, in the case where the layered composite structure does not include the same layered units, the composite coating may be composed of an odd number of layers or an even number of layers. When preparing a layered composite structure, it is only necessary to arrange a plurality of ferroalloy materials alternately according to the hardness and spray them sequentially to form a layered composite structure with alternating hardness distribution. In the case where the layered composite structure includes the same layered units, the layered composite structure is composed of an even number of layers. In the attached Figure 4 In the example shown, the layered composite structure consists of an even number of layers. Figure 5 In the example shown, the layered composite structure consists of an odd number of layers.

[0050] Figure 1 Schematic diagram of the top view of the raw material block according to the embodiment of the present application. Figure 1As shown, the first, second, ..., and sixth sprayings are performed in sequence to form the first, second, ..., and sixth branch layers, respectively, thereby forming a raw material block 10 having a layered composite structure. It should be noted that any substrate can be used as a carrier in the first spraying, and after the last spraying, the carrier substrate is first cut, and the layered composite structure portion is retained as the raw material block 10.

[0051] Figure 5 Schematic diagram of the structure of a tool according to the third embodiment of the present application. Figure 5 As shown, the tool 20 includes the first, second, ..., Nth branch layers alternately arranged along the length direction. The particle sizes of the branch layers are alternately distributed in high and low order, and the hardness of the branch layers are alternately arranged in high and low order along the length direction.

[0052] Most kitchen knives have structures with uneven thickness. Excessive stress on the knives will lead to a low pass rate for the knives, and there will also be defects such as collapse of the cutting edge of the knives. Therefore, during the manufacturing process, it is necessary to reduce the stress in the knives. According to the present application, the ferroalloy material is in granular form, and a pre-pressing step is performed after each 1st, 2nd, ..., N-1th spraying; after the Nth spraying, the formed raw material block with a layered composite structure is processed by a hot isostatic pressing sintering process, so that adjacent branch layers are embedded with each other and adjacent particles of each branch layer have predetermined pores.

[0053] In these embodiments, a granular ferroalloy material is used to sinter and form a raw material block 10. During the sintering process, the internal stress of the raw material block 10 is relatively low. At the same time, after the hot isostatic pressing sintering is completed, it can be cooled with the furnace. Due to the low cooling rate, the internal stress of the raw material block 10 can be further reduced, thereby obtaining a raw material block 10 with low internal stress and a layered composite structure, which can be suitable for manufacturing cutting tools with uneven thickness.

[0054] Hereinafter, the raw material block of the present application will be described in detail by taking an example in which a raw material block is formed by stacking and connecting a plurality of identical layered units in the width direction.

[0055] According to the present application, a plurality of branch layers are formed by stacking a plurality of identical layered units 21. Each layered unit 21 is two sub-layers with different hardnesses. When the ferroalloy material is in powder form, the step of forming each layered unit includes: pre-spraying a first ferroalloy material to form a first sub-layer 211, and then spraying a second ferroalloy material on the surface of the first sub-layer 211 to form a second sub-layer 212, thereby forming a layered unit 21. When the ferroalloy material is in strip form, the step of forming a layered unit includes: pre-spraying a first ferroalloy material to form a first sub-layer 211, and then spraying a second ferroalloy material to form a second sub-layer 212, and compounding the first sub-layer 211 and the second sub-layer 212 to form a layered unit 21. In an exemplary embodiment, the step of forming the layered unit 21 includes: using a stainless steel particle to spray for the first time to form a first sub-layer 211, and pre-pressing the first sub-layer by hydraulic pressure; then using another stainless steel particle to spray for the second time on the first sub-layer 211 to form a second sub-layer 212, and pre-forming the second sub-layer by hydraulic pressure, thereby forming a layered unit 21. In these embodiments, after each sub-layer is formed, it is pre-pressed (pre-formed) by hydraulic pressure, so that adjacent sub-layers can be tightly combined, thereby making each sub-layer tightly combined.

[0056] According to the present application, after forming a layered unit 21, the formation operation of the previous layered unit 21 is repeated, and the next layered unit 21 is formed on the previous layered unit 21, and multiple branch layers composed of multiple layered units 21 are alternately formed in this way, thereby forming a raw material block 10 with a layered composite structure.

[0057] According to the present application, when the raw material block 10 reaches a specified thickness (wherein the specified thickness of the raw material block 10 here is used as the length of the tool, and can be set according to the actual length of the tool), the raw material block 10 with a layered composite structure can be sintered so that adjacent branch layers in the layered composite structure are embedded with each other and adjacent particles of each branch layer have a predetermined pore size. In an exemplary embodiment, the size of the predetermined pore is in the range of 40μm-150μm. Figure 3 As shown, the predetermined pores between adjacent particles can add more teeth to the micro-serrated structure, so that the micro-serrated structure has more teeth, which can improve the long-lasting sharpness performance. It should be noted that during the sintering process, the layered composite structure is in a solid state, and is in a solid-phase sintering state. Specifically, by controlling the temperature and pressure during the hot isostatic pressing operation, the predetermined pore structure can be retained between adjacent particles. In an exemplary embodiment, the sintering time using hot isostatic pressing technology is 3h-4h, the sintering temperature is 1050℃-1200℃, and the pressure is 120Mpa-150Mpa.

[0058] In order to prevent the granular ferroalloy material from being oxidized during the manufacturing process, the step of making the raw material block can be performed in a vacuum environment. In an exemplary embodiment, in a vacuum environment of a vacuum furnace, the vacuum degree is controlled at 0.1-20 Pa, and the mold of the vacuum furnace is sprayed and pre-pressed, and the layered composite structure is formed repeatedly.

[0059] In an embodiment, the first sub-layer 211 and the second sub-layer 212 have the same thickness, and the thickness of each sub-layer is 500 μm-700 μm.

[0060] According to the present application, the particle size difference of the ferroalloy material forming adjacent branch layers may be 10 μm-60 μm. By setting a predetermined particle size difference of the ferroalloy material forming adjacent branch layers, the bonding force between adjacent branch layers can be enhanced.

[0061] In some embodiments, the hardness of the first ferroalloy material is less than the hardness of the second ferroalloy material and the particle size of the first ferroalloy material is greater than the particle size of the second ferroalloy material. In other embodiments, the hardness of the first ferroalloy material is less than the hardness of the second ferroalloy material and the particle size of the first ferroalloy material is greater than the particle size of the second ferroalloy material.

[0062] In these embodiments, the particle size of the material with greater hardness is set to be relatively small. Due to the small particle size, the grains after sintering are small, and there are more grain boundaries, which can hinder the expansion of dislocations. The material strength is greater, thereby improving the strength of the formed micro-serrated structure, thereby making the tool more durable and sharper.

[0063] like Figure 2 and Figure 3 As shown, a layered unit 21 formed of two ferroalloy materials includes a first sublayer 211 and a second sublayer 212 alternately arranged in a length direction. Two ferroalloy materials need to be prepared to form such a tool. Wherein, in the case where the hardness of the first ferroalloy material is less than the hardness of the second ferroalloy material, exemplarily, the hardness of the first ferroalloy material may be in the range of 50-55HRC, the hardness of the second ferroalloy material may be in the range of 56-60HRC, the particle size of the first ferroalloy material is 70μm-100μm, and the particle size of the second ferroalloy material is 40μm-60μm. In the case where the hardness of the first ferroalloy material is greater than the hardness of the second ferroalloy material, exemplarily, the hardness of the first ferroalloy material may be in the range of 56-60HRC, the hardness of the second ferroalloy material may be in the range of 50-55HRC, the particle size of the first ferroalloy material is 40μm-60μm, and the particle size of the second ferroalloy material is 70μm-100μm. In the attached Figure 2In the example shown, the hardness of the first sub-layer 211 is greater than the hardness of the second sub-layer 212 .

[0064] Forming the tool blank

[0065] Figure 1 It is a schematic diagram of the top view structure of a raw material block according to an embodiment of the present application. Figure 2 Schematic diagram of the structure of a tool according to an embodiment of the present application. Figure 1 and Figure 2 As shown, the obtained raw material block 10 is formed along the width direction to obtain a tool blank having a layered composite structure in the length direction. By forming the raw material block 10 along the width direction, each sublayer in the length direction of the cutting edge has different hardness, thereby facilitating the formation of a micro-serrated structure.

[0066] According to the present application, before the step of grinding the tool blank, the method for manufacturing the tool further includes: performing roll forging on the tool blank at a predetermined temperature along the length direction so that the various branch layers of the tool blank are interlocked with each other. In addition, by performing roll forging at a preset temperature, the thickness of the tool blank can be gradually reduced in the width direction to form a kitchen knife structure with uneven thickness. The specific parameters of the roll pressing process are a roll pressing pressure of 80MPa-120MPa and a roll pressing temperature of 500℃-700℃. In these embodiments, the roll forging process can make the various branch layers of the tool blank interlock with each other, and the layers of the layered composite structure are tightly combined, which can form processing strengthening to a certain extent and enhance the strength of the tool blank.

[0067] According to the present application, a grinder is used to grind along the thickness direction of the tool, and under the condition of consistent grinding conditions, a micro-serrated structure is formed on the cutting edge of the tool along the length direction.

[0068] like Figure 3 As shown, the cutting edge of the tool of the present application has a micro-serrated structure. Specifically, the above-mentioned tool blank is ground by a grinder. When the travel speed of the grinder is consistent, the multiple branch layers with alternating hardness along the length direction will have different grinding amounts during the grinding process due to different hardness (different hardness leads to different grinding amounts). Most of the branch layers with relatively large hardness are retained in the cutting edge, and most of the branch layers with relatively small hardness are ground away, so that a fine micro-serrated structure can be formed at the cutting edge of the cutting edge during grinding. Among them, the height of the micro-serrated structure is 100μm-200μm, and the width is 500μm-700μm.

[0069] According to the present application, the shape of the micro-serration structure can be set according to actual needs, and the present application does not limit it to be formed as a rack-like structure in the extension direction of the tool edge. The micro-serration structure according to the present application, for example but not limited to, forms a continuous wavy structure along the extension direction of the tool edge (see Figure 3 ). According to the micro-serrated structure of the present application, in the thickness direction of the tool, the teeth of each micro-serrated structure can be an inverted cone structure. It should be noted that the tip of the micro-serrated structure of the present application can be selected according to actual needs, for example but not limited to, determined according to the application of the tool and the cutting requirements of the tool (hardness of the object to be cut, etc.). The extension direction of the extension direction of the tool edge can be strip-shaped or arc-shaped. When the extension direction of the extension direction of the tool edge is strip-shaped, it is consistent with the length direction of the tool.

[0070] The manufacturing method and tool of the tool of the present invention are described in detail above in combination with exemplary embodiments. In the following, the beneficial effects of the present invention will be described in more detail in combination with specific embodiments, but the protection scope of the present invention is not limited to the embodiments.

[0071] Example 1

[0072] The cutting tool according to Example 1 was prepared by the following method.

[0073] Step S10, manufacturing a raw material block having a layered composite structure.

[0074] Step S11, providing 3Cr13 stainless steel powder with an average particle size of 70 μm-100 μm as a ferroalloy material, spraying the 3Cr13 stainless steel powder for the first time, and using hydraulic pressure to preform the first sub-layer, thereby forming a first sub-layer with a thickness of 600 μm.

[0075] Step S12, providing 5Cr15MoV stainless steel powder with an average particle size of 40μm-60μm as another ferroalloy material, spraying the 5Cr15MoV stainless steel powder on the first sublayer for a second time, and preforming the second sublayer by hydraulic pressure, thereby forming a second sublayer with a thickness of 600μm.

[0076] Step S13, repeating steps S11 to S12 alternately 50 times on the second sub-layer (i.e., performing the 3rd, 4th, ..., 100th spraying to form the 3rd, 4th, ..., 100th branch layers respectively), thereby forming a raw material block with a width of 6 cm and a layered composite structure.

[0077] Step S20, after the 100th spraying, the raw material block with a layered composite structure is processed by hot isostatic pressing sintering process, wherein the sintering time is 3 hours, the sintering temperature is 1100° C., and the pressure is 130 MPa.

[0078] Step S30, forming the raw material block along the width direction to obtain a tool blank having a layered composite structure in the length direction, wherein the length direction of the tool blank is the width direction of the raw material block, that is, 6 cm.

[0079] Step S40, heating the formed tool blank and then performing roll forging along the length direction to form a tool blank with an average thickness of 1 mm at the cutting edge, wherein the specific parameters of the roll forging process are a roll pressure of 90 MPa and a roll temperature of 600°C.

[0080] Step S50, when the parameters of the grinder are consistent, the tool blank is ground in the thickness direction by a grinder to form a fine micro-serration structure at the cutting edge, wherein the height of the micro-serration structure is 200 μm and the width is 500 μm, thereby obtaining the tool of Example 1.

[0081] Example 2

[0082] The cutting tool of Example 2 is manufactured by the same method as Example 1, except that the step of manufacturing the raw material block having a layered composite structure is performed under a vacuum environment.

[0083] Example 3

[0084] The tool of Example 3 is manufactured by the same method as Example 1, except that step S20 is not performed (ie, the hot isostatic pressing sintering process is not used).

[0085] Example 4

[0086] The tool of Example 4 is manufactured by the same method as Example 1, except that 4Cr13 stainless steel powder is used instead of 3Cr13 stainless steel powder for the first spraying to form the first sublayer (and the same is true for the subsequent formation of each layered unit).

[0087] Example 5

[0088] The tool of Example 5 is manufactured by the same method as Example 1, except that 102Cr17MoV stainless steel powder is used instead of 5Cr15MoV stainless steel powder to spray form the second sublayer (and the same applies to the subsequent formation of each layered unit).

[0089] Example 6

[0090] The tool of Example 6 is manufactured by the same method as Example 1, except that 4Cr13 stainless steel powder is used instead of 5Cr15MoV stainless steel powder to spray form the second sublayer (and the same applies to the subsequent formation of each layered unit).

[0091] Example 7

[0092] The tool of Example 7 is manufactured by the same method as in Example 1, except that 5Cr15MoV stainless steel powder is used instead of 3Cr13 stainless steel powder for the first spraying to form the first sublayer, and 3Cr13 stainless steel powder is used instead of 5Cr15MoV stainless steel powder for the second spraying to form the second sublayer (and the same applies to the subsequent formation of each layered unit).

[0093] Example 8

[0094] In addition to spraying 3Cr13, 7Cr17MoV, 4Cr13, 5Cr15MoV, 3Cr13, 6Cr13MoV, 4Cr13, 102Cr17MoV, 3Cr13, 7Cr17MoV, 5Cr15MoV, 102Cr17MoV, 6Cr13MoV, 7Cr17MoV, 3Cr13, 102Cr17MoV, 3Cr13, 7Cr17MoV, 4Cr13, 5Cr15MoV, 3Cr13, 7Cr17MoV, 4Cr13, 5Cr15MoV, 3Cr13, 6Cr13MoV, 4Cr13 , 102Cr17MoV, 3Cr13, 7Cr17MoV, 5Cr15MoV, 102Cr17MoV, 4Cr13, 6Cr13MoV, 4Cr13, 102Cr17MoV, 3Cr13, 7Cr17MoV, 5Cr15MoV, 102Cr1 7MoV, 5Cr15MoV, 102Cr17MoV, 6Cr13MoV, 7Cr17MoV, 3Cr13, 102Cr17MoV, 3Cr13, 7Cr17MoV, 4Cr13, 5Cr15MoV, 3Cr13, 102Cr17MoV, 3Cr 13. 7Cr17MoV, 4Cr13, 5Cr15MoV, 3Cr13, 7Cr17MoV, 4Cr13, 5Cr15MoV, 3Cr13, 6Cr13MoV, 4Cr13, 102Cr17MoV, 5Cr15MoV, 102Cr17MoV, 6Cr13MoV, 7Cr17MoV, 3Cr13, 102Cr17MoV, 3Cr13, 7Cr17MoV, 4Cr13, 5Cr15MoV, 4Cr13, 102Cr17MoV, 3Cr13, 7Cr17MoV, 5Cr15MoV, 102 Cr17MoV, 5Cr15MoV, 102Cr17MoV, 6Cr13MoV, 7Cr17MoV, 3Cr13, 102Cr17MoV, 3Cr13, 7Cr17MoV, 4Cr13, 5Cr15MoV, 7Cr17MoV, 102Cr17MoV, 6Cr13MoV, 7Cr17MoV, 3Cr13, 102Cr17MoV, 4Cr13, 5Cr15MoV, 7Cr17MoV, 102Cr17MoV to form a raw material block, and the same method as in Example 1 is used to manufacture the cutting tool of Example 8.

[0095] Example 9

[0096] The raw material block prepared in Example 1 is used to form a cutting edge portion having a multilayer structure along the length direction. The cutting edge portion having the same thickness as that in the example is connected to a blade body having a thickness of 2 mm by welding and forging, thereby manufacturing the tool of Example 9.

[0097] Comparative Example 1

[0098] The average thickness of the cutting edge is 1mm. 5Cr15MoV stainless steel knife.

[0099] Comparative Example 2

[0100] The average thickness of the cutting edge is 1mm.

[0101] Comparative Example 3

[0102] The average thickness of the cutting edge is 1mm. 102Cr17MoV stainless steel knife.

[0103] Performance index test

[0104] The thickness of the cutting edge of the tool in Examples 1-9 and Comparative Examples 1-3 is the same, and performance index tests are performed on them respectively, and the test results are recorded in the following Table 1. The performance test method is as follows:

[0105] (1) Initial sharpness: Refer to the sharpness test method in GBT 40356-2021 Kitchen Knives. The larger the sharpness value, the better the initial sharpness, and the smaller the sharpness value, the opposite.

[0106] (2) Test method for long-lasting sharpness:

[0107] The lasting sharpness adopts the simulated tool life test method. The specific method is described below. The larger the value of the lasting sharpness, the longer the initial sharpness and lasting sharpness life. The smaller the value of the lasting sharpness, the opposite is true.

[0108] The specific method of simulating tool life test is as follows: fix the tested tool edge horizontally downward on the tool fixture, and after adding weights, press it on the simulation with a pressure of 16N. The cutting simulation (3mm kraft paper) remains stationary, and the tool fixture is driven by a motor and air pressure to drive the tool to cut in the X-axis direction, with a reciprocating speed of 50mm / s. At the same time, it rises in the Z-axis direction and moves 1mm in the Y-axis direction to shape the simulation. The cutting stroke is 100mm, and it ends after cutting the simulation 5 times. The evaluation object (ham sausage) is used to determine the tool's long-term sharpness. The test ends when the evaluation object cannot be cut. The total number of cuts from the start to the end of the test is recorded, which is the tool's long-term sharpness. The more total cuts, the higher the long-term sharpness.

[0109] Table 1 Performance test data of the embodiments of the present application and the comparative examples

[0110]

[0111] As is known to all, the long-lasting sharpness of knives made of 102Cr17MoV martensitic stainless steel is the best level among knives currently made of stainless steel. However, the cost of manufacturing knives therefrom is too high. According to the above comparison, the comparative examples of the embodiments and their corresponding materials have been improved. This improvement can reach the best level of knives made of 102Cr17MoV martensitic stainless steel, and is even far superior to 102Cr17MoV martensitic stainless steel knives. In summary, the present application ensures the service life by using a sub-layer with relatively good toughness, and ensures the sharpness by using a sub-layer with relatively high hardness, and combines a variety of materials to obtain a long-lasting sharp knives suitable for people to use. The knives made according to the present application can be long-lasting and sharp, and are not prone to edge curling.

[0112] Although the embodiments of the present application have been described in detail above, those skilled in the art may make various modifications and variations to the embodiments of the present application without departing from the spirit and scope of the present application. However, it should be understood that, in the opinion of those skilled in the art, these modifications and variations will still fall within the spirit and scope of the embodiments of the present application defined by the claims.

Claims

1. A method for manufacturing a cutting tool, characterized in that: The method for manufacturing a tool comprises: A raw material block having a layered composite structure along a width direction is formed, wherein the layered composite structure is formed by a plurality of branch layers alternately stacked along the width direction, and the hardness of the plurality of branch layers is arranged alternately in high and low positions along the width direction; wherein the plurality of branch layers are formed by stacking a plurality of identical layered units, and each layered unit includes a first sublayer and a second sublayer, and the steps of forming each layered unit include: providing a first ferroalloy material, and spraying the first ferroalloy material to form a first sublayer; providing a second ferroalloy material, and spraying the second ferroalloy material on the first sublayer to form a second sublayer, wherein the hardness of the first ferroalloy material is greater than the hardness of the second ferroalloy material and the particle size of the first ferroalloy material is smaller than the particle size of the second ferroalloy material; or, the hardness of the first ferroalloy material is less than the hardness of the second ferroalloy material and the particle size of the first ferroalloy material is greater than the particle size of the second ferroalloy material; Forming the raw material block along the width direction to obtain a tool blank having the layered composite structure in the length direction; The tool blank is subjected to grinding treatment to obtain a tool having a cutting edge portion with a micro-serrated structure formed by the layered composite structure in the length direction.

2. The method for manufacturing a tool according to claim 1, characterized in that: The method for manufacturing a cutting tool further comprises: performing a pre-pressing step after spraying.

3. The method for manufacturing a tool according to claim 1, characterized in that: After spraying, a hot isostatic pressing sintering process is performed on the raw material block having a layered composite structure, so that adjacent layers are interlocked with each other and adjacent particles of each branch layer have predetermined pores.

4. The method for manufacturing a cutting tool according to claim 1, characterized in that: The thickness of the first sub-layer is the same as the thickness of the second sub-layer.

5. The method for manufacturing a cutting tool according to claim 1, characterized in that: The difference between the particle size of the first ferroalloy material and the particle size of the second ferroalloy material is 10μm-60μm, the particle size of one of the first ferroalloy material and the second ferroalloy material is 70μm-100μm, and the particle size of the other of the first ferroalloy material and the second ferroalloy material is 40μm-60μm.

6. The method for manufacturing a cutting tool according to claim 1, characterized in that: Before the step of grinding the tool blank, the method for manufacturing a tool further comprises: performing roll forging on the tool blank at a predetermined temperature along the length direction of the tool blank so that the various support layers of the tool blank are embedded with each other.

7. The method for manufacturing a cutting tool according to claim 1, characterized in that: The ferroalloy material includes at least two martensitic stainless steel materials selected from 3Cr13, 4Cr13, 5Cr15MoV, 6Cr13MoV, 7Cr17MoV and 102Cr17MoV.

8. The method for manufacturing a cutting tool according to claim 1, characterized in that: Each layered unit includes an even number of layers.

9. The method for manufacturing a cutting tool according to claim 1, characterized in that: The plurality of branch layers are formed of a plurality of iron alloy materials with a hardness difference of 1HRC-10HRC.

10. The method for manufacturing a cutting tool according to claim 1, characterized in that: The thickness of each branch layer is 500 μm-700 μm.

Citation Information

Patent Citations

  • Magnet and forming method thereof

    CN104575895A

  • TiCrN&MoS2 / Cr / Ti laminated coated tool and preparation process thereof

    CN105887024A

  • Sandwich-structured compound zirconia-alumina-zirconia ceramic and preparation method thereof

    CN106986630A

  • Formula and process of cemented carbide circle blade, circle blade with positioning hole, and process

    CN108098281A

  • Cutter manufacturing method and cutter

    CN115055685A