A method for preparing and coating end face of semiconductor laser device

Through inductively coupled plasma-reactive ion etching and wet polishing technology, combined with vacuum electron beam evaporation, the problems of low yield and surface roughness in the end surface preparation of semiconductor laser devices are solved, and the coating quality and device reliability are improved. A more efficient end face preparation and coating process is achieved.

CN115418615BActive Publication Date: 2024-11-05SHANGHAI SANFEI ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210075850.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-23
Publication Date
2024-11-05
Estimated Expiration
2042-01-23

AI Technical Summary

Technical Problem

The existing end surface preparation methods of semiconductor laser devices have problems such as low yield, complex process, high surface roughness and easy optical catastrophic damage during coating, which affects the long-term reliability of the device.

Method used

Inductively coupled plasma-reactive ion etching is used to form the end surface, and combined with wet chemical polishing and vacuum electron beam evaporation technology, a high-quality cavity surface coating is formed through photolithography development and inorganic solution treatment.

Benefits of technology

Simplify the process flow, improve the quality of end surface coating and long-term device reliability, reduce surface roughness, enhance the uniformity and density of coating, and improve the performance of laser devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115418615B_ABST
    Figure CN115418615B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing and coating the end face of a semiconductor laser device, which belongs to the technical field of preparing semiconductor laser devices, and comprises the following steps: step 1, forming the front end face and the rear end face of the laser device by an inductively coupled plasma-reactive ion etching method; step 2, exposing the area to be coated on the front end face or the area to be coated on the rear end face by photolithography, and then developing the wafer; step 3, performing wet chemical polishing on the area to be coated on the front end face or the area to be coated on the rear end face by an inorganic solution; step 4, coating by vacuum electron beam evaporation, bombarding the area to be coated on the front end face or the area to be coated on the rear end face with an ion beam during the coating process; step 5, performing rapid stripping and organic solution cleaning on the coated wafer. The present invention can simplify the process flow, greatly improve the quality of the cavity surface coating, and improve the long-term reliability of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation technology of a semiconductor laser device, and in particular to an end face preparation and film coating method of a semiconductor laser device. Background Art

[0002] In recent years, the development of semiconductor lasers has been extremely rapid. With the popularization of artificial intelligence, the Internet of Things and 5G networks, the demand for high-speed laser devices and communication modules is extremely urgent; the development of autonomous driving technology also places extremely high demands on the power, line width and long-term reliability of optical radars; in industrial environments, high-power, high-energy laser devices are also widely used. For the above scenarios, edge-emitting laser devices (EEL) have unique advantages over vertical-emitting lasers (VCSEL) and still dominate. For EEL, major domestic and foreign manufacturers still use the cleave method to form facets and finally separate the devices. This method has a low yield and a complex process. Some foreign companies also form end faces through Chemically Assisted Ion Beam Etching (CAIBE). This process can simplify the process and moderately improve the yield. However, there are problems with surface roughness and high loss when forming end faces through etching. In addition, due to oxidation and adhesion problems in the coating process, it is easy to cause catastrophic optical damage (COD) and cause long-term reliability problems. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing and coating the end face of a semiconductor laser device, which can simplify the process flow, greatly improve the quality of the cavity surface coating, and improve the long-term reliability of the device. As a processing paradigm, the present invention can be applied to any edge-emitting laser with a ridge waveguide and an end face.

[0004] The present invention is achieved through the following technical solutions:

[0005] A method for preparing and coating an end face of a semiconductor laser device comprises the following steps:

[0006] Step 1, forming the front end face and the rear end face of the laser device by using an inductively coupled plasma-reactive ion etching method;

[0007] Step 2, exposing the area to be coated on the front face or the area to be coated on the rear face by photolithography, and then developing the wafer;

[0008] Step 3, using an inorganic solution to perform wet chemical polishing on the area to be coated on the front face or the area to be coated on the rear face;

[0009] Step 4, coating is performed by vacuum electron beam evaporation, and during the coating process, an ion beam is used to bombard the area to be coated on the front face or the area to be coated on the rear face;

[0010] Step 5: Rapidly strip the coated wafer and clean it with an organic solution.

[0011] In step 1, the wafer has a ridge waveguide formed and has SiO 2 Wafer as hard mask pattern.

[0012] The step 1 is specifically as follows: placing the wafer into an inductively coupled plasma-reactive ion etching device. During the wafer etching process, the temperature is 45-55°C, the chlorine gas flow rate is 18-22sccm, the argon gas flow rate is 4-6sccm, the power of the inductively coupled plasma is 200-250W, the power of the bias voltage RF source is 100-120W, the chamber pressure is 200-250mTorr, and the etching time is at least 4 minutes.

[0013] The specific steps of exposing the area to be coated on the front face or the area to be coated on the rear face by photolithography in step 2 are:

[0014] Step 21, coating a layer of non-photosensitive polymer adhesive layer on the surface of the wafer by a coating machine, the rotation speed of the coating machine is 3000-3500 rpm, and the time is at least 1 minute.

[0015] Step 22, coating a photosensitive photoresist layer on the non-photosensitive polymer layer by means of a coating machine, the rotation speed of the coating machine is 3000-3500 rpm, and the time is at least 1 minute.

[0016] Step 23, exposing the mask pattern of the area to be coated on the front face or the area to be coated on the rear face by using a contact exposure machine or a stepper lithography machine.

[0017] The specific steps of developing the wafer in step 2 are: placing the wafer on a developer for development, using MIF3000 as the developer, and the developing time is at least 2 minutes and 30 seconds.

[0018] The specific steps of step 3 are:

[0019] Step 31, plasma cleaning the developed wafer;

[0020] Step 32, immersing the wafer after plasma cleaning in a diluted hydrochloric acid solution for at least 1 minute, then rinsing with deionized water, and then drying with nitrogen gas;

[0021] Step 33, immersing the wafer after being blown dry with nitrogen in a diluted ammonia solution for at least 30 seconds, then rinsing it with deionized water again, and then blowing it dry with nitrogen again.

[0022] In step 31, the process parameters of plasma cleaning are: temperature of 20-25°C, oxygen flow rate of 180-200sccm, pressure of 200-250mTorr, plasma power of 100-120W, and cleaning time of at least 1 minute.

[0023] In the hydrochloric acid dilution solution, the mass ratio of hydrochloric acid to the hydrochloric acid dilution solution is 1:15 to 1:20.

[0024] In the ammonia water dilution solution, the mass ratio of ammonia water to the ammonia water dilution solution is 1:20 to 1:25.

[0025] The specific steps of step 4 are:

[0026] Step 41, placing the wafer to be coated and the test sample into an electron beam evaporation device for evaporation of the transparent film, wherein the material of the test sample is the same as that of the wafer;

[0027] Step 42, measuring the reflectivity of the test sample.

[0028] In step 42, when detecting the reflectivity of the sample, the sample is placed on a desktop spectrophotometer, and the reflectivity of the sample in the wavelength range of 200nm to 2000nm is measured to be qualified. The reflectivity of the transparent film on the front end surface of the wafer is verified by comparing the reflectivity curve in the wavelength range of 200nm to 2000nm.

[0029] During the evaporation process of step 4, the wafer and the test sample are respectively fastened to the base of the fixture, and the fixture includes a vertical central axis; before starting the evaporation, the wafer is in an initial position, and the plane where the wafer is located and the vapor cloud sphere formed by the evaporation of the dielectric material are at a 45-degree angle to the normal plane of the wafer position; during the evaporation process, the wafer moves in a circular motion around the vertical central axis of the fixture, and at the same time, the wafer swings back and forth within the range of 30° to 60° between the plane where the wafer is located and the aforementioned normal plane.

[0030] In step 4, a first film layer is evaporated on the to-be-coated area of ​​the front end surface, and then a second film layer is evaporated on the first film layer. The dielectric material used for evaporating the first film layer is titanium dioxide, and the dielectric material used for evaporating the second film layer is silicon dioxide.

[0031] In step 4, before starting the evaporation, nitrogen is introduced and the ion beam is turned on to bombard the wafer surface. The power of the ion beam is 150W, and the ion beam is turned on during the entire evaporation process. The specific steps of the step 5 for quickly stripping the coated wafer are as follows:

[0032] Step 51, applying pressure with a sponge roller to roll the blue film evenly onto the surface of the wafer;

[0033] Step 52, peeling off the blue film, and the dielectric material attached to the surface of the photosensitive photoresist layer will be peeled off together;

[0034] Step 53, putting the wafer after the blue film is peeled off into a stripping solution at 50-60°C, soaking for at least 20 minutes and then taking it out.

[0035] In the step 4, the third film layer, the fourth film layer, the fifth film layer, the sixth film layer, the seventh film layer, the eighth film layer, the ninth film layer and the tenth film layer are sequentially evaporated in the area to be coated on the rear end face, the dielectric material used for evaporating the third film layer, the fifth film layer, the seventh film layer and the ninth film layer is aluminum oxide, and the dielectric material used for evaporating the fourth film layer, the sixth film layer, the eighth film layer and the tenth film layer is silicon, so as to form a high reflective film.

[0036] Compared with the prior art, the present invention has the following beneficial technical effects:

[0037] The present invention uses an inductively coupled plasma-reactive ion etching method to form the front and rear facets of the laser device, which has the advantage of maintaining the integrity of the wafer from beginning to end, and can be mass-produced by automated equipment with extremely high efficiency. In addition, unlike the end face (cleavefacet) formed by the cleavage method, the present invention is completely independent of the crystal direction of the wafer, and will not cause the cleavage facet to be scratched into the device due to the angle deviation of the crystal direction, resulting in a reduction in yield.

[0038] In order to solve the problem of rough end faces formed by etching methods, the present invention adopts wet chemical etching to assist in compensating for it. Chemical polishing (Cavity Chemical Polishing, CCP) is performed by treating the above-mentioned chemical reagents, which can effectively reduce the surface roughness and improve the vertical fine stripes. At the same time, the natural oxide generated on the surface of the etched end face is removed, greatly improving the substrate quality of the end face.

[0039] For coating technology, the present invention adopts a method in which the wafer moves in a circle around the vertical central axis of the fixture, which can greatly improve the overall uniformity of the high-reflection film and the overall uniformity of the transparent film and improve the process conditions. At the same time, the reciprocating swing of the wafer during the evaporation process can make the high-reflection film and the transparent film better adhere to the front face, the rear face, the upper edge of the front face, the lower edge of the front face, the upper edge of the rear face, and the lower edge of the rear face, which can play a sealing role, thereby isolating air and water vapor, which is beneficial to the long-term reliability of the device. Nitrogen is introduced before electron beam evaporation, and an ion beam such as a nitrogen ion beam is used to assist in the evaporation process, which can make the coating dense and further improve the quality of the coating on the end face and the rear face. After coating, the process stability is verified by detecting the reflectivity of the sample.

[0040] For the stripping technology after coating, the present invention adopts a combination of blue film and stripping solution. First, most of the useless dielectric materials on the wafer surface are removed by blue film to expose the photoresist substrate, and then the remaining useless dielectric materials can be quickly stripped and removed by immersion in a medium-temperature stripping solution. The process is extremely simple and can save 80% of time compared to traditional immersion stripping.

[0041] In summary, the present invention forms a good end face substrate by combining dry etching with wet surface treatment, and forms high-quality high-reflective film and transparent film by optimizing the coating method, thereby improving the reliability of laser devices; with the present invention, the wafer can be tested without being cleaved into bars, and test data can be obtained for each chip on the wafer. By analyzing the data, the main information of the epitaxial design and process flow of this wafer can be fed back to the design and development team without waiting for all the back-end processes, which can greatly accelerate design iterations and improve research and development efficiency. And combined with the subsequent costs, it can be decided whether to push the wafers processed by the present invention into the back-end process, thereby reducing the factory operating costs. The above advantages are not currently possessed by mainstream manufacturers. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is the appearance image formed on the wafer surface by combining dry etching with wet surface treatment in this patent.

[0043] Figure 2 This is an end face cross-section diagram obtained by photolithography based on a double layer of LOR5A and photoresist material.

[0044] Figure 3 Jigs and platforms used for electron beam vacuum evaporation.

[0045] Figure 4 Schematic diagram of the angle and position of electron beam vacuum evaporation.

[0046] Figure 5 This is the thickness uniformity distribution diagram of electron beam evaporated high-reflective film and transparent film obtained by software simulation. DETAILED DESCRIPTION

[0047] All features disclosed in this specification, or all steps in the disclosed methods or processes, except mutually exclusive features and / or steps, may be combined in any manner and, unless otherwise stated, may be replaced by other equivalent or alternative features having similar purposes, that is, unless otherwise stated, each feature is merely an embodiment of a series of equivalent or similar features.

[0048] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0049] In order to explain the present invention more clearly, the method of forming laser devices by the splitting method is first introduced. This method requires thinning and splitting the wafer before coating the cavity surface, and then the cavity surface coating and testing at the bar level can be carried out, and finally cleavage. However, the method of forming laser devices by the splitting method has the following disadvantages: First, the test results of the wafer are unknown before thinning; if the device operation problems are caused by epitaxial technology, front-end process flow, etc., the factory cannot predict, and the back-end process may become a sunk cost and cannot create any value; second, the process arrangement of the back-end process itself will affect the yield. The cavity surface coating needs to be arranged manually or automatically, which is time-consuming and increases uncertainty; testing can only be performed at the bar level, which is extremely inconvenient.

[0050] The present invention is further described in detail below with reference to the embodiments.

[0051] The present invention is a method for preparing and coating the end face of a semiconductor laser device. The surface morphology of the wafer obtained by the present invention can be referred to Figure 1 The front face 1 and the rear face 2 are obtained by dry etching and wet surface treatment, and the wafer is still intact, and wafer-level optical chip testing can be performed. The end face preparation and coating method mentioned in the present invention includes the following steps:

[0052] Step 1: using an inductively coupled plasma-reactive ion etching method to form the front end face and the rear end face of the laser device; specifically, the ridge waveguide having been formed and having SiO 2The wafer with hard mask pattern is placed in the inductively coupled plasma-reactive ion etching equipment. During the wafer etching process, the temperature is 45-55°C, the chlorine flow rate is 18-22sccm, the argon flow rate is 4-6sccm, the power of the inductively coupled plasma is 200-250W, the power of the bias voltage RF source is 100-120W, the chamber pressure is 200-250mTorr, and the etching time is at least 4 minutes; after etching, the wafer is cleaned with an organic solvent to remove water-soluble byproducts. Through this step, the etching depth of the front and rear faces can reach about 3.5 microns, the etching is uniform, the side wall morphology is highly vertical, and there are certain vertical lines along the vertical ion etching direction.

[0053] Step 2, expose the area to be coated on the front face by photolithography, and then develop the wafer; specifically, place the wafer on a coater, and coat a layer of non-photosensitive polymer adhesive layer (such as LOR5A) on the surface of the wafer by the coater, the speed of the coater is 3000-3500rpm, and the time is at least 1 minute; then coat a layer of photosensitive photoresist layer (such as SPR220-3.0) on the non-photosensitive polymer adhesive layer by the coater, the speed of the coater is 3000-3500rpm, and the time is at least 1 minute; then expose the mask pattern of the area to be coated on the front face by a contact exposure machine or a stepper lithography machine. The double-layer adhesive system composed of the non-photosensitive polymer adhesive layer and the photosensitive photoresist layer will form a morphology that is very conducive to the stripping process, such as Figure 2 shown. Figure 2 In the figure, 8 is an active area, 9 is a wafer substrate, 5 is a photosensitive photoresist layer, 6 is a non-photosensitive polymer adhesive layer, and 7 is a coating layer deposited on the end surface. After the non-photosensitive polymer adhesive layer 6 and the photosensitive photoresist layer 5 are exposed and developed, the exposed area of ​​the photosensitive photoresist layer 5 is dissolved by the developer, and the non-photosensitive polymer adhesive layer 6 can be dissolved in the developer regardless of whether it is exposed or not, so the two together form a structure with a unique concave morphology, which is conducive to the penetration and stripping of the stripping solution.

[0054] Step 3, using an inorganic solution to perform wet chemical polishing on the area to be coated on the front face. Specifically, first, the developed wafer is plasma cleaned, and the process parameters of the plasma cleaning are: temperature of 20-25°C, oxygen flow rate of 180-200sccm, pressure of 200-250mTorr, plasma power of 100-120W, and cleaning time of at least 1 minute; the wafer after plasma cleaning is immersed in a diluted hydrochloric acid solution for at least 1 minute, then rinsed with deionized water, and then dried with nitrogen. In the diluted hydrochloric acid solution, the mass ratio of hydrochloric acid to the diluted hydrochloric acid solution is 1:15 to 1:20; the wafer after nitrogen drying is immersed in a diluted ammonia solution for at least 30 seconds, then rinsed with deionized water again, and then dried with nitrogen again. In the diluted ammonia solution, the mass ratio of ammonia to the diluted ammonia solution is 1:20 to 1:25. After the wafer is processed in step 3, the dry etching end face will be smoothed, and the natural oxide on the end face will be completely removed. This is of great help in improving the coating quality.

[0055] Step 4, coating is performed by vacuum electron beam evaporation, and the area to be coated on the front face is bombarded with an ion beam during the coating process. Specifically, the wafer to be coated and the test sample are first placed in an electron beam evaporation device for evaporation of a transparent film, wherein, Figure 3 , Figure 4 As shown, the wafer 20 and the test sample are respectively fastened to the base of the fixture, and the fixture 10 includes a vertical center axis. Before the start of evaporation, the wafer is in the initial position, and the plane where the wafer is located (i.e., the second dotted plane 21) and the normal plane of the vapor cloud sphere 17 formed by the evaporation of the dielectric material at the position of the wafer 10 (i.e., the first dotted plane 19) are at a 45-degree angle; during the evaporation process, the wafer 20 moves in a circle around the vertical center axis of the fixture 10, and at the same time, the wafer 20 swings back and forth within the range of 30° to 60° between its plane and the aforementioned normal plane; then the reflectivity of the test sample is measured to ensure the quality of the coating. For example, Figure 4 In the embodiment, the electron beam 15 is deflected by the magnetic field and driven into the crucible 16 to heat the dielectric material in the crucible 16, and the dielectric material evaporates to form a vapor cloud sphere 17; the first dotted line plane 19 is the normal plane of the vapor cloud sphere 17 at the wafer 20, and the second dotted line plane 21 is the plane where the wafer 20 is located, and the normal plane of the vapor cloud sphere 17 at the wafer 20 is at an angle of 45 degrees to the plane where the wafer 20 is located. For example, Figure 3As shown, the motor 12 is installed vertically, and the output shaft of the motor 12 is connected to the reduction box 13. The output shaft of the reduction box 13 drives the fixture 10 to rotate with its own vertical central axis as the axis. The fixture 10 includes four support platforms 11, which are centrally symmetrically arranged with the vertical central axis of the fixture 10 as the center. The wafer to be coated and the test sample are placed on the support platform 11 of the fixture 10 and tightened. During the evaporation process, the fixture 10 is rotated with its own vertical central axis as the axis through the pulley mechanism in the motor 12 and the reduction box 13, and the wafer 20 moves in a circle around the vertical central axis of the fixture 10. The plane where the wafer 20 is located is at a 45-degree angle to the normal plane of the vapor cloud sphere 17 formed by the evaporation of the dielectric material at the wafer position. At the same time, driven by the motor 12 and the mechanical transmission mechanism in the reduction box 13, the wafer 20 swings back and forth within the range of 30° to 60° between the plane where the wafer 20 is located and the aforementioned normal plane. The test sample is 2cmx4cm in length and made of the same material as the wafer, which is used to check the evaporation results. The transparent film includes a first film layer and a second film layer. Specifically, the first film layer is evaporated in the area to be coated on the front face, and then the second film layer is evaporated on the first film layer. The dielectric material used for evaporating the first film layer is titanium dioxide, and the dielectric material used for evaporating the second film layer is silicon dioxide. The thickness of the first film layer is 5nm, and the thickness of the second film layer is 70nm. Before starting evaporation, nitrogen is introduced and the ion beam is turned on to bombard the wafer surface. The power of the ion beam is 150W, and the ion beam 22 is turned on during the entire evaporation process. The auxiliary treatment of the ion beam 22 will increase the density of the dielectric material on the end face and further enhance the reliability of the device. After the evaporation is completed, when testing the reflectivity of the sample, the test sample with the same material as the wafer is placed on a desktop spectrophotometer, and its reflectivity in the wavelength range of 200nm to 2000nm is measured to be qualified, thereby verifying the reflectivity of the transparent film on the front face of the wafer. This fixture and coating process can make the thickness of the transparent film more uniform, and the thickness deviation does not exceed ±1.5% of the total thickness. Figure 5 .

[0056] Step 5, quickly strip the coated wafer and clean it with an organic solution; specifically, place the wafer on a special base and tighten it, use a sponge roller to apply pressure and roll the blue film evenly on the wafer surface; then peel off the blue film, and the dielectric material attached to the surface of the photosensitive photoresist layer will be peeled off together; then put the wafer with the blue film peeled off into a stripping solution at 50-60°C, soak it for at least 20 minutes, take it out, and then clean it with an organic solvent.

[0057] The area to be coated on the rear face can be processed in the manner of steps 2 to 5. However, it should be noted that the third film layer, the fourth film layer, the fifth film layer, the sixth film layer, the seventh film layer, the eighth film layer, the ninth film layer, and the tenth film layer are sequentially deposited on the area to be coated on the rear face, that is, the third film layer is firstly deposited on the area to be coated on the rear face, and then the fourth film layer is deposited on the third film layer, and so on, until the tenth film layer is deposited; wherein, the dielectric material used for the deposition of the third film layer, the fifth film layer, the seventh film layer, and the ninth film layer is aluminum oxide, and the dielectric material used for the deposition of the fourth film layer, the sixth film layer, the eighth film layer, and the tenth film layer is silicon; the thickness of the third film layer, the fifth film layer, the seventh film layer, and the ninth film layer can be 139nm, and the thickness of the fourth film layer, the sixth film layer, the eighth film layer, and the tenth film layer can be 68nm, so as to form a high-reflection film. In addition, the other processing methods of the rear face are the same as the processing methods of the front face in steps 2 to 5.

[0058] It is understandable that the area to be coated on the rear end face can be processed first according to the above content, and then the area to be coated on the front end face can be processed. The order of processing the area to be coated on the front end face and the area to be coated on the rear end face does not constitute a limitation on the protection scope of the present invention.

Claims

1. A method for preparing and coating an end face of a semiconductor laser device, characterized in that: The following steps are involved: Step 1, forming the front end face and the rear end face of the laser device by using an inductively coupled plasma-reactive ion etching method; Step 2, exposing the area to be coated on the front face or the area to be coated on the rear face by photolithography, and then developing the wafer; Step 3, using an inorganic solution to perform wet chemical polishing on the area to be coated on the front face or the area to be coated on the rear face; Step 4, coating is performed by vacuum electron beam evaporation, and during the coating process, an ion beam is used to bombard the area to be coated on the front face or the area to be coated on the rear face; Step 5, quickly stripping the coated wafer and cleaning it with an organic solution; In the step 4, a first film layer is evaporated on the to-be-coated area of ​​the front end surface, and then a second film layer is evaporated on the first film layer, wherein the dielectric material used for evaporating the first film layer is titanium dioxide, and the dielectric material used for evaporating the second film layer is silicon dioxide; In the step 4, a third film layer, a fourth film layer, a fifth film layer, a sixth film layer, a seventh film layer, an eighth film layer, a ninth film layer, and a tenth film layer are sequentially evaporated on the to-be-coated area of ​​the rear end face, the dielectric material used for evaporating the third film layer, the fifth film layer, the seventh film layer, and the ninth film layer is aluminum oxide, and the dielectric material used for evaporating the fourth film layer, the sixth film layer, the eighth film layer, and the tenth film layer is silicon, to form a high-reflective film; The step 1 is specifically as follows: placing the wafer into an inductively coupled plasma-reactive ion etching device, during the wafer etching process, the temperature is 45-55° C., the chlorine gas flow rate is 18-22 sccm, the argon gas flow rate is 4-6 sccm, the power of the inductively coupled plasma is 200-250 W, the power of the bias voltage RF source is 100-120 W, the chamber pressure is 200-250 mTorr, and the etching time is at least 4 minutes; The specific steps of step 4 are: Step 41, placing the wafer to be coated and the test sample into an electron beam evaporation device for evaporation of the transparent film, wherein the material of the test sample is the same as that of the wafer; Step 42, measuring the reflectivity of the test sample; During the evaporation process of step 4, the wafer and the test sample are respectively fastened to the support table of the fixture, and the fixture includes a vertical central axis; before the start of evaporation, the wafer is in an initial position, and the plane where the wafer is located and the vapor cloud sphere formed by the evaporation of the dielectric material are at a 45-degree angle at the normal plane of the wafer position; during the evaporation process, the wafer moves in a circle around the vertical central axis of the fixture, and at the same time, the wafer swings back and forth within the range of 30° to 60° between the plane where the wafer is located and the aforementioned normal plane; The specific steps of the step 5 for quickly peeling the coated wafer are as follows: Step 51, applying pressure with a sponge roller to roll the blue film evenly onto the surface of the wafer; Step 52, peeling off the blue film, and the dielectric material attached to the surface of the photosensitive photoresist layer will be peeled off together; Step 53, putting the wafer after the blue film is peeled off into a stripping solution at 50-60°C, soaking for at least 20 minutes and then taking it out.

2. The preparation and coating method according to claim 1, characterized in that: In step 1, the wafer is a wafer on which a ridge waveguide has been formed and SiO2 is used as a hard mask pattern.

3. The preparation and coating method according to claim 1, characterized in that: The specific steps of exposing the area to be coated on the front face or the area to be coated on the rear face by photolithography in step 2 are: Step 21, coating a layer of non-photosensitive polymer adhesive layer on the surface of the wafer by a coating machine, the rotation speed of the coating machine is 3000-3500 rpm, and the time is at least 1 minute; Step 22, coating a photosensitive photoresist layer on the non-photosensitive polymer layer by a coating machine, the rotation speed of the coating machine is 3000-3500 rpm, and the time is at least 1 minute; Step 23, exposing the mask pattern of the area to be coated on the front face or the area to be coated on the rear face by using a contact exposure machine or a stepper lithography machine.

4. The preparation and coating method according to claim 1, characterized in that: The specific steps of step 3 are: Step 31, plasma cleaning the developed wafer; Step 32, immersing the wafer after plasma cleaning in a diluted hydrochloric acid solution for at least 1 minute, then rinsing with deionized water, and then drying with nitrogen gas; Step 33, immersing the wafer after being blown dry with nitrogen in a diluted ammonia solution for at least 30 seconds, then rinsing it with deionized water again, and then blowing it dry with nitrogen again.

5. The preparation and coating method according to claim 4, characterized in that: In step 31, the process parameters of plasma cleaning are: temperature of 20-25°C, oxygen flow rate of 180-200sccm, pressure of 200-250mTorr, plasma power of 100-120W, and cleaning time of at least 1 minute.

6. The preparation and coating method according to claim 4, characterized in that: In the hydrochloric acid dilution solution, the mass ratio of hydrochloric acid to the hydrochloric acid dilution solution is 1:15 to 1:

20.

7. The preparation and coating method according to claim 4, characterized in that: In the ammonia water dilution solution, the mass ratio of ammonia water to the ammonia water dilution solution is 1:20 to 1:

25.

8. The preparation and coating method according to claim 1, characterized in that: In step 42, when detecting the reflectivity of the sample, the sample is placed on a desktop spectrophotometer, and the reflectivity of the sample in the wavelength range of 200nm to 2000nm is measured to be qualified. The reflectivity of the transparent film on the front end surface of the wafer is verified by comparing the reflectivity curve in the wavelength range of 200nm to 2000nm.

9. The preparation and coating method according to claim 1, characterized in that: In the step 4, before starting the evaporation, nitrogen gas is introduced and an ion beam is turned on to bombard the wafer surface. The power of the ion beam is 150 W, and the ion beam is turned on during the entire evaporation process.