A kind of iron-carbon filler based on gasified fine slag and its preparation method and application
By using iron-carbon fillers based on gasified fine slag, the problems of easy passivation of fillers and poor acidic wastewater treatment effects in micro-electrolysis technology are solved, achieving efficient and low-cost treatment of high-salt and strong-acid wastewater, extending the life of the fillers and Reduces the difficulty of replacement.
Patent Information
- Application Number
- CN202210463179.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-04-28
AI Technical Summary
When existing micro-electrolysis technology is used to treat printing and dyeing wastewater, the fillers are prone to passivation and hardening, and the cost of pH adjustment is high. The treatment effect of acidic wastewater is not good, resulting in a short life of the fillers and difficulty in replacement.
Iron-carbon filler based on gasified fine slag is used, which is made of gasified fine slag, reduced iron powder, binder and porogen. It is formed into spherical particles through a granulator and roasted at high temperature to form a product with high compressive strength and acid resistance. High-performance filler for treating high-salt and strong-acid wastewater.
It extends the service life of the filler, reduces the difficulty of filler replacement and processing costs, significantly improves the treatment effect, and is in line with the concept of treating waste with waste.
Smart Images

Figure CN115477369B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of sewage treatment, and specifically relates to an iron-carbon filler based on gasified fine slag and a preparation method and application thereof. Background Art
[0002] In recent years, the printing and dyeing industry has developed rapidly, and the annual discharge of printing and dyeing wastewater is huge, accounting for about one-tenth of industrial wastewater. Printing and dyeing wastewater has the characteristics of large chromaticity, complex composition, high content of organic pollutants, large water quality changes, non-degradability and high biological toxicity. Direct discharge will threaten the ecology.
[0003] Micro-electrolysis technology has the advantages of wide material sources, low investment, small footprint, easy industrialization, stable treatment effect, etc. It is highly compatible with high-salt wastewater and is widely used in the treatment of various organic wastewaters, and has achieved remarkable results. Micro-electrolysis technology is mainly based on iron and carbon. Wastewater, zero-valent iron, and granular activated carbon constitute a primary cell microsystem, which removes pollutants in wastewater through electrochemical processes.
[0004] However, in actual industrial applications, it is found that the use of micro-electrolysis technology to treat wastewater has the following defects: the filler will become passivated and hardened after long-term operation, the water quality has a significant impact on the treatment effect, and the pH requirements for the wastewater to be treated are relatively high. Generally, the effect is best when the pH is 2-3. In order to maintain the optimal pH range, alkaline reagents are usually used to adjust the pH value, but the use of chemical reagents to control the pH is costly. The use of limestone or lime milk to increase the pH of wastewater will produce a large amount of solid waste and bring new pollution problems. In addition, when the pH is above 4, iron oxides or iron hydroxides will be generated on the surface of iron, hindering the reaction. When the pH is too low, that is, in strongly acidic wastewater, the iron-carbon filler will be severely corroded and have a short service life. After a large amount of iron is dissolved in the strongly acidic wastewater, the iron-carbon filler becomes loose and easy to collapse, and a large amount of residue blocks the drain, making it difficult to replace the filler. Summary of the invention
[0005] In view of the above analysis, the present invention aims to provide an iron-carbon filler based on gasified fine slag and a preparation method and application thereof, so as to solve the above problems existing in the prior art.
[0006] The object of the present invention is achieved in that:
[0007] In a first aspect, an iron-carbon filler based on gasified fine slag is provided, which is made of gasified fine slag, reduced iron powder, a binder and a porogen; the mass ratio of gasified fine slag to iron powder is 1:1, the content of the binder is 10-30% of the total mass of the gasified fine slag and the reduced iron powder, and the content of the porogen is 1-5% of the total mass of the gasified fine slag and the reduced iron powder.
[0008] Furthermore, the binder is kaolin and the porogen is basic copper carbonate.
[0009] In a second aspect, a method for preparing an iron-carbon filler based on gasified fine slag is provided, comprising: fully mixing the gasified fine slag, reduced iron powder, a binder and a porogen according to a designed proportion, placing the mixed particles into a granulator to form spherical particles, calcining the spherical particles at a high temperature in an airtight environment, and obtaining an iron-carbon filler based on gasified fine slag after cooling.
[0010] Furthermore, the particle sizes of the gasified fine slag and the reduced iron powder are both less than 0.15 mm.
[0011] Furthermore, the mixed material is made into spherical particles of 20-50 mm by using a granulator; and the spherical particles are vacuum dried at a temperature of 60-90° C. before high-temperature roasting.
[0012] Further, the spherical particles are calcined at high temperature in a calcining furnace, including the following four stages:
[0013] The first stage: heating from room temperature to 150°C at 15°C / min and maintaining the temperature for 30 min;
[0014] The second stage: heating to 200°C at 15°C / min and maintaining the temperature for 30 min;
[0015] The third stage: after heating to 800°C at 25°C / min, adjust the heating rate to 10°C / min, heat to 1000°C, and keep the temperature constant for 30 min;
[0016] Stage 4: Stop heating and cool to room temperature.
[0017] In a third aspect, an application of an iron-carbon filler based on gasified fine slag is provided, which is applied to a micro-electrolysis reaction tower for treating acidic wastewater, wherein the micro-electrolysis reaction tower comprises:
[0018] A tower body, wherein the tower body has a reaction space for treating wastewater;
[0019] The packing column is arranged in the tower body, and the packing column is filled with iron-carbon packing based on gasified fine slag.
[0020] Furthermore, the packing column is arranged on the inner wall of the tower body, and the outer wall of the tower body is provided with a packing filling port connected to the reaction space in the tower body. The packing filling port is located above the packing column and connected to the charging port of the packing column.
[0021] Furthermore, there are multiple packing columns, which are symmetrically arranged on the inner wall of the tower body.
[0022] Furthermore, the micro-electrolysis reaction tower also includes a stirring assembly and an aeration device. The stirring assembly includes a motor, a transmission rod and a stirring paddle arranged on the transmission rod. The motor is arranged on the top of the tower body, and the transmission rod is coaxially arranged in the tower body; the aeration device is arranged on the transmission rod.
[0023] Furthermore, there are multiple aeration devices and stirring paddles, which are alternately arranged on the transmission rod.
[0024] Furthermore, a wastewater inlet is provided at the bottom of the tower body, a wastewater outlet and an exhaust port are provided at the top of the tower body, and a filter screen is also provided in the tower body. The filter screen is located below the wastewater outlet, and a spray head for spraying pickling liquid onto the filter screen is provided above the filter screen.
[0025] Furthermore, a solid waste outlet is provided at the bottom of the tower body, and a submersible pump is also provided in the tower body to discharge the solid residue or flocculants at the bottom of the tower body through the solid waste outlet.
[0026] Furthermore, a plurality of pH detectors are dispersedly arranged from top to bottom in the tower body.
[0027] Furthermore, the packing column comprises a shell, the top opening of the shell is a loading port of the packing column, and the side wall and the bottom wall of the shell are evenly provided with through holes.
[0028] Furthermore, a plurality of inclined baffles are arranged from top to bottom in the shell, the odd-numbered baffles are located above the even-numbered baffles, and the shell has a first side inner wall and a second side inner wall relative to each other; the first end of the odd-numbered baffle is connected to the first side inner wall, the second end of the odd-numbered baffle extends downwardly at an angle, and a first gap is provided between the first end of the odd-numbered baffle and the second side inner wall for the iron-carbon filler to pass through; the first end of the even-numbered baffle is connected to the second side inner wall, the second end of the even-numbered baffle extends downwardly at an angle, and a second gap is provided between the first side inner wall and the first side inner wall for the iron-carbon filler to pass through.
[0029] Furthermore, the first end of the baffle is fixed to the inner wall of the shell through an elastic member.
[0030] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0031] a) The iron-carbon filler based on gasified fine slag provided by the present invention adopts gasified fine slag and reduced iron powder, and iron and carbon are fully mixed and exist in the form of an iron-carbon inclusion structure. In the process of treating high-salt and strong acid wastewater, the iron source and the carbon source are consumed at the same time, and there is no need to replace or supplement the filler with the iron source, thereby reducing the operational difficulties caused by replacing the filler; because the gasified fine slag contains aluminum oxide and calcium oxide, the consumption rate of the iron source can be slowed down, and the service life of the iron-carbon filler in high-acid wastewater is increased.
[0032] b) The method for preparing the iron-carbon filler based on gasified fine slag provided by the present invention utilizes the gasified fine slag as a carbon source, thereby solving the problem of environmental pollution caused by industrial waste slag; and the preparation process is simple, easy to operate, and low in cost, and the prepared iron-carbon filler has high compressive strength.
[0033] c) The iron-carbon filler based on gasified fine slag provided by the present invention can be used to treat high-salt and strong-acid printing and dyeing wastewater. Compared with other types of iron-carbon fillers, it not only has a good treatment effect, but also greatly improves the acid resistance, conforms to the idea of treating waste with waste, and significantly reduces the cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of this specification or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the embodiments of this specification. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.
[0035] Figure 1 A schematic diagram of the structure of a micro-electrolysis reaction tower provided by the present invention;
[0036] Figure 2 A schematic diagram of the arrangement of packing columns in a micro-electrolysis reaction tower provided by the present invention.
[0037] Figure 3 This is a schematic structural diagram of the packing column provided by the present invention.
[0038] Reference numerals:
[0039] 1. Tower body; 2. Packing column; 2-1. Shell; 2-2. Baffle; 2-3 Elastic part; 2-4. Unfilled space; 3. Packing filling port; 4. Aeration device; 5. Agitator; 6. Drive rod; 7. Submersible pump; 8. Wastewater inlet; 9. Wastewater outlet; 10. Solid waste outlet; 11. Exhaust port; 12. pH tester; 13. Filter; 14. Sprinkler head. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0041] To facilitate understanding of the embodiments of the present application, further explanation will be given below with reference to specific embodiments in conjunction with the accompanying drawings. The embodiments do not constitute a limitation on the embodiments of the present application.
[0042] In the description of the embodiments of the present invention, it should be noted that, unless otherwise clearly specified and limited, the term "connected" should be understood in a broad sense, for example, it can be a fixed connection, or a detachable connection, or an integral connection, which can be a mechanical connection, or an electrical connection, which can be a direct connection, or can be indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0043] The terms "top", "bottom", "above", "lower", and "on" used throughout the description are relative to the relative positions of components of a device, such as the relative positions of the top and bottom substrates within a device. It is understood that devices are multifunctional regardless of their orientation in space.
[0044] Example 1
[0045] A specific embodiment of the present invention discloses an iron-carbon filler based on gasified fine slag, which is made of gasified fine slag, reduced iron powder, a binder and a porogen; wherein the mass ratio of gasified fine slag to iron powder is 1:1, the content of the binder is 10-30% of the total mass of the gasified fine slag and the reduced iron powder, and the content of the porogen is 1-5% of the total mass of the gasified fine slag and the reduced iron powder.
[0046] In one optional embodiment, the binder is kaolin and the porogen is basic copper carbonate.
[0047] The present embodiment also discloses a preparation method of an iron-carbon filler based on gasified fine slag, comprising the following steps: fully mixing the gasified fine slag, reduced iron powder, a binder and a porogen according to a designed ratio, placing the mixed particles into a granulator to form spherical particles, calcining the spherical particles at a high temperature in an airtight environment, and obtaining the iron-carbon filler based on gasified fine slag after cooling.
[0048] Before mixing, dry the gasified fine slag and grind the reduced iron powder, and screen out the dried gasified fine slag and reduced iron powder with a particle size of less than 0.15 mm. Since the gasified fine slag has a fine particle size and does not need to be ground, it only needs to be fully dried and screened to screen out fine slag particles with a particle size of less than 0.15 mm; grind the reduced iron powder, screen out the reduced iron powder with a particle size of less than 0.15 mm, and mix it with the dried and screened gasified fine slag, kaolin and basic copper carbonate through mechanical stirring. Fully stirring allows the iron source and the carbon source to be fully mixed, and the iron-carbon particles are evenly dispersed, which can increase the number of primary cells during micro-electrolysis, increase the reaction rate of wastewater treatment, and the iron particles are not easy to rust and reduce compaction; on the other hand, the iron and carbon in the iron-carbon filler exist in the form of an iron-carbon inclusion framework through a binder, and the iron skeleton and the carbon structure intersect with each other, with high compressive strength.
[0049] After the reduced iron powder, gasified fine slag, kaolin and basic copper carbonate are fully mixed by mechanical stirring, an appropriate amount of water is added to fully mix them to obtain a mixed material. The mixed material is placed in a granulator to form spherical particles with a particle size of 20-50 mm. Before high-temperature roasting, the spherical particles are vacuum dried at a temperature of 60-90°C. The vacuum-dried spherical particles are roasted under vacuum and high-temperature conditions. The spherical particles have high compressive resistance and a large surface area, and can fully contact with wastewater to increase the reaction rate; the added basic copper carbonate can help incorporate copper components into the iron-carbon material on the one hand, catalyzing the reaction efficiency of micro-electrolysis, and on the other hand, it decomposes during the subsequent high-temperature roasting process, so that the iron-carbon filler has more developed voids; compared with the simple mixing of traditional iron and carbon, the iron-carbon filler after granulation can be repeatedly recycled and reused to reduce pipeline blockage.
[0050] After the spherical particles are vacuum dried, they are placed in a roasting furnace at room temperature and isolated from air for high-temperature roasting. The high-temperature roasting is carried out in the roasting furnace in the following four stages:
[0051] The first stage: the calcining furnace is first heated to 150°C at 15°C / min and kept at this temperature for 30 min to dry out moisture and prevent polymerization.
[0052] The second stage: continue to increase the temperature to 200℃ at a rate of 15℃ / min and keep the temperature constant for 30 min to induce the porogen to slowly decompose and form pores and form a copper catalyst to prevent the decomposition rate from being too fast and causing the collapse of the internal structure of the filler;
[0053] The third stage: After rapidly heating to 800°C at 25°C / min, the heating rate was adjusted to 10°C / min, the temperature was raised to 1000°C, and the temperature was kept constant for 30 min to optimize the physical and chemical properties of the filler by high-temperature calcination;
[0054] The fourth stage: stop heating, take out after naturally cooling to room temperature, and the obtained black solid particles are the gasified fine slag iron-carbon filler to be prepared.
[0055] In the process of firing iron-carbon filler based on gasified fine slag, the firing process of spherical particles in a calcining furnace is designed into multiple stages. Different firing stages are set differently in terms of heating rate and firing time, so that the prepared iron-carbon filler has better physical and chemical properties.
[0056] Compared with the prior art, the iron-carbon filler based on gasified fine slag provided in this embodiment selects gasified fine slag as the carbon source because the gasified fine slag is rich in components, rich in silicon, aluminum, and carbon resources, and the carbon content is generally about 20%. It forms countless micro-batteries with iron, and treats printing and dyeing wastewater through electrochemical action; silicon oxide can increase the compressive strength of the iron-carbon filler after high-temperature roasting; aluminum oxide, calcium oxide, etc. in the gasified fine slag can replace iron in the reaction process to react with hydrogen in high-acid wastewater, reduce the consumption rate of iron, and play an excellent buffering role; after the aluminum ions and iron ions are dissolved, they can be used as good flocculants in subsequent stages to further treat wastewater according to the situation; trace amounts of titanium oxide, manganese oxide and other components can play a good catalytic role in the high-temperature roasting process. Secondly, the gasified fine slag has a fine particle size and can be fully mixed with the iron source. It has a large specific surface area and developed pores, and has a good adsorption effect on organic wastewater. As one of the industrial solid wastes, gasification fine slag has a huge annual discharge volume. It can be efficiently recycled and used to treat printing and dyeing wastewater, with low wastewater treatment costs, which is in line with the idea of treating waste with waste and the newly developed environmental protection concept. The iron-carbon filler prepared based on gasification fine slag in this embodiment is suitable for high-salt strong acid wastewater. High salt can increase the conductivity of wastewater and promote the reaction rate. The acidic environment is conducive to the best effect of iron-carbon micro-electrolysis technology. The iron-carbon filler prepared based on gasification fine slag has higher acid resistance than other fillers in the prior art.
[0057] Example 2
[0058] Another specific embodiment of the present invention discloses an application of an iron-carbon filler based on gasified fine slag, which is applied to a micro-electrolysis reaction tower for treating acidic wastewater, such as applying the prepared iron-carbon filler based on gasified fine slag to treat high-salt and strong-acid printing and dyeing wastewater.
[0059] In order to improve the treatment effect of high-salt and strong-acid printing and dyeing wastewater, this embodiment improves the structure of the micro-electrolysis reaction tower. Figure 1 As shown, the micro-electrolysis reaction tower includes a tower body 1, which has a reaction space for treating wastewater. The tower body 1 is made of a strong acid-resistant material. A filling column 2 is provided in the tower body 1, and the filling column 2 is filled with the iron-carbon filler based on gasified fine slag in Example 1.
[0060] Specifically, the packing column 2 is arranged on the inner wall of the tower body 1, and the outer wall of the tower body 1 is provided with a packing filling port 3 connected to the reaction space in the tower body 1. The packing filling port 3 is located above the packing column 2 and is connected to the charging port of the packing column 2. The packing is filled or supplemented into the packing column through the packing filling port. The loss of the packing and the hardening and passivation of the packing can also be observed through the packing filling port. The packing filling port 3 is provided with a sealing door, which is detachably arranged at the packing filling port 3 and can open and close the packing filling port 3.
[0061] In order to improve the reaction effect, the number of the packing columns 2 is multiple, such as Figure 2 As shown, they are symmetrically arranged on the inner wall of the tower body 1. Optionally, the number of the packing columns 2 is 4-6.
[0062] In order to prevent the occurrence of concentration polarization during the micro-electrolysis reaction and affect the reaction effect, and to prevent the bottom floccules from adhering to the tower body 1 and being unable to be discharged, the micro-electrolysis reaction tower also includes a stirring assembly to stir the wastewater and the bottom floccules. Specifically, the stirring assembly includes a motor, a transmission rod 6, and a stirring paddle 5 arranged on the transmission rod 6. The motor is arranged at the top of the tower body 1, and the transmission rod 6 is coaxially arranged in the space surrounded by multiple packing columns 2 in the tower body 1.
[0063] In order to enhance the reaction rate of micro-electrolysis, the micro-electrolysis reaction tower based on iron-carbon filler of gasified fine slag also includes an aeration device 4. During the reaction between wastewater and filler, air is blown into the tower body 1 by the aeration device to increase the oxygen content in the wastewater and improve the treatment effect. The surface of the iron-carbon filler is repeatedly flushed by aeration to reduce compaction.
[0064] Exemplarily, a plurality of aeration devices are arranged in the middle space surrounded by the packing columns to aerate the surrounding areas, thereby increasing the oxygen content in the wastewater and also flushing the packing to reduce the occurrence of compaction and passivation.
[0065] Furthermore, the aeration device 4 is arranged on the transmission rod 6, and the number of the aeration device 4 and the stirring paddle 5 are both multiple, and they are alternately arranged on the transmission rod 6. With the stirring of the stirring paddle 5, the aeration of the aeration device 4, and the aeration of the aeration device 4 is also driven by the transmission rod 6 to rotate, the aeration process of the aeration device 4 is carried out during the rotation process, and combined with the stirring of the stirring paddle 5, a better stirring effect can be achieved.
[0066] In this embodiment, a wastewater inlet 8 is provided at the bottom of the tower body 1, and a wastewater outlet 9 and an exhaust port 11 are provided at the top of the tower body 1; a solid waste outlet 10 is provided at the bottom of the tower body 1, and a submersible pump 7 is also provided in the tower body 1 to discharge the solid residue or flocculants at the bottom of the tower body 1 through the solid waste outlet 10.
[0067] In order to prevent a large amount of solid wastewater from blocking the drain outlet and pipeline when the wastewater is discharged, a filter screen is set before the drain outlet. Specifically, a filter screen 13 is also provided in the tower body 1, and the filter screen 13 is located below the wastewater outlet 9.
[0068] Considering that the surface of the micro-electrolytic filler may become hardened and passivated after long-term operation, a spray head 14 for spraying pickling liquid on the filter 13 is provided above the filter 13 to rinse its surface by spraying a small amount of pickling liquid so that it continues to maintain its reaction activity.
[0069] In one of the optional embodiments, a plurality of pH detectors 12 are dispersedly arranged from top to bottom in the tower body 1. By setting a plurality of pH detection devices in the micro-electrolysis reaction tower, the pH change of the reaction solution in the reaction tower can be detected in real time, so as to adjust the pH value of the wastewater and keep the micro-electrolysis reaction in the optimal reaction condition.
[0070] In this embodiment, the packing column 2 includes a shell 2-1, the top opening of the shell 2-1 is a charging port of the packing column 2, and the side wall and bottom wall of the shell 2-1 are evenly provided with through holes; the aperture of the through hole of the shell 2-1 is smaller than the particle size of the iron-carbon filler based on gasification fine slag, and optionally, the aperture of the through hole is 1-3 mm. The wastewater enters the shell 2-1 through the through hole and contacts with the iron-carbon filler, and the solid residue or flocculant produced by the reaction flows out through the through hole and settles to the bottom of the tower body 1.
[0071] In one optional embodiment, Figure 3 As shown, a plurality of inclined baffles 2-2 are arranged from top to bottom in the shell 2-1, and the odd-numbered baffles 2-2 are located above the even-numbered baffles 2-2, and the shell 2-1 has a first side inner wall and a second side inner wall relative to each other; the first end of the odd-numbered baffle 2-2 is connected to the first side inner wall, and the second end of the odd-numbered baffle 2-2 extends obliquely downward, and has a first gap between the second side inner wall and the second side inner wall for the iron-carbon filler to pass through; the first end of the even-numbered baffle 2-2 is connected to the second side inner wall, and the second end of the even-numbered baffle 2-2 extends obliquely downward, and has a second gap between the first side inner wall and the first side inner wall for the iron-carbon filler to pass through. This structural setting allows the carbon-iron filler to be rolled along the baffle 2-2 for multiple times and filled into the shell 2-1, thereby avoiding local accumulation of the carbon-iron filler in the shell 2-1. In addition, the inclined baffle 2-2 allows the shell 2-1 to have an unfilled space 2-4 after filling. The unfilled space 2-4 is located inside the shell 2-1, which increases the contact reaction area between the acid liquid and the filler, thereby improving the treatment effect.
[0072] Further, the first end of the baffle 2-2 is fixed to the inner wall of the shell 2-1 through the elastic member 2-3. Except for the first end, the rest of the baffle 2-2 does not contact the inner wall of the shell 2-1, and can swing up and down within a certain range in the shell 2-1. The shell 2-1, the baffle 2-2 and the elastic member 2-3 are all made of strong acid-resistant materials. Exemplarily, the elastic member 2-3 is a spring or an elastic plate, so that the baffle 2-2 can swing downward to a certain extent under the gravity of the iron-carbon filler. As the iron-carbon filler is consumed, the baffle 2-2 can be reset to the initial position, and due to the structure of the inclined baffle 2-2, there is always a space under each baffle 2-2 that is not filled with the iron-carbon filler. This space is filled with wastewater, which not only increases the reaction contact area between the wastewater and the iron-carbon filler, but also with the stirring of the stirring paddle 5 and the aeration of the aeration device 4, the baffle 2-2 will also vibrate to a certain extent when the wastewater flows, and the iron-carbon filler in the shell 2-1 is stirred to a certain extent, thereby improving the reaction effect.
[0073] Furthermore, there is a gap between the outer wall of the shell 2-1 of the packing column 2 and the inner wall of the tower body 1, such as a gap of 1-5 cm. A certain gap is reserved between the packing column 2 and the inner wall of the tower body 1, which helps the wastewater to fully contact with the packing column 2 and is beneficial to the circulation of the wastewater in the tower body 1.
[0074] When using a micro-electrolysis reaction tower to treat high-salt and strong-acid printing and dyeing wastewater, first use alkaline substances such as lime milk to adjust the pH value of the high-salt and strong-acid printing and dyeing wastewater to about 1, and the adjusted wastewater is injected into the micro-electrolysis reaction tower. The wastewater is supplied to the reaction space of the tower body 1 from the wastewater inlet 8 at the bottom of the micro-electrolysis reaction tower, and discharged from the wastewater outlet 9 at the top of the micro-electrolysis reaction tower. The residence contact time of the wastewater in the reaction tower is 3-8h. In the process of treating high-salt and strong-acid printing and dyeing wastewater, the carbon-iron filler is gradually consumed, and the part of the carbon-iron filler that cannot be dissolved in acid, such as residual carbon, will settle to the bottom of the tower body 1 through the through hole on the shell 2-1; as the micro-electrolysis proceeds, the pH of the wastewater increases, and the iron and aluminum ions dissolved in the carbon-iron filler in the wastewater will produce floccules with the hydroxide ions, and settle to the bottom of the tower body 1 together with the above-mentioned residual carbon, and be pumped from the solid waste outlet 10 to the flocculation section by the submersible pump 7 as a flocculant to continue to degrade the wastewater. The printing and dyeing wastewater treated by the iron-carbon filler process can achieve the goals of complete decolorization and significant reduction of COD. The wastewater can be sent to subsequent processes for further treatment or efficient utilization of its high salt and strong acid resources.
[0075] After pretreatment in the micro-electrolysis section, the high-salt and strong-acid printing and dyeing wastewater enters the flocculation section. As the iron source is consumed, iron becomes ions and dissolves into the wastewater, and other oxides also become ions and dissolve into the wastewater. A small amount of carbon-silicon residues enter the next flocculation section along with the wastewater, and finally flocculate and separate with the flocculant in the flocculation section or deposit at the bottom of the micro-electrolysis cell to be discharged in a centralized manner. This also solves the problem of the difficulty in replacing iron-carbon fillers, and only needs to be replenished regularly; while consuming hydrogen ions, the gasified fine slag increases the pH of the wastewater, and the iron oxide and aluminum oxide in the gasified fine slag components dissolve into the wastewater, which is a good flocculant. This can reduce the dosage of acid-base reagents and flocculants in the flocculation section, reduce treatment costs, and avoid color problems caused by excessive iron ions dissolved in the micro-electrolysis section.
[0076] The specific implementation methods described above further illustrate the purpose, technical solutions and beneficial effects of the present application in detail. It should be understood that the above description is only the specific implementation method of the present application and is not intended to limit the scope of protection of the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application.
Claims
1. A micro-electrolysis reaction tower based on iron-carbon filler of gasified fine slag, characterized in that: Applied to treating acidic wastewater, the micro-electrolysis reaction tower comprises: A tower body (1), wherein the tower body (1) has a reaction space for treating wastewater; A packing column (2) is arranged in a tower body (1), and is filled with an iron-carbon packing based on gasified fine slag, wherein the iron-carbon packing based on gasified fine slag is made of gasified fine slag, reduced iron powder, a binder and a porogen; the packing column (2) comprises a shell (2-1), and the shell (2-1) has a first side inner wall and a second side inner wall opposite to each other; a plurality of inclined baffles (2-2) are arranged in the shell (2-1) from top to bottom, wherein the odd-numbered baffles (2-2) are located above the even-numbered baffles (2-2), the first ends of the odd-numbered baffles (2-2) are connected to the first side inner wall, the second ends of the odd-numbered baffles (2-2) extend downwardly at an angle, and have a first gap between the first end and the second side inner wall for the iron-carbon packing to pass through; the first ends of the even-numbered baffles (2-2) are connected to the second side inner wall, the second ends of the even-numbered baffles (2-2) extend downwardly at an angle, and have a second gap between the first end and the first side inner wall for the iron-carbon packing to pass through; The packing column (2) is arranged on the inner wall of the tower body (1); the outer wall of the tower body (1) is provided with a packing loading port (3) connected to the reaction space in the tower body (1); the packing loading port (3) is located above the packing column (2) and is connected to the loading port of the packing column (2); the top opening of the shell (2-1) is the loading port of the packing column (2); the side wall and the bottom wall of the shell (2-1) are both provided with through holes; the aperture of the through hole of the shell (2-1) is smaller than the particle size of the gasified fine slag iron-carbon filler; There are multiple packing columns (2), which are symmetrically arranged on the inner wall of the tower body (1); The micro-electrolysis reaction tower further comprises a stirring assembly and an aeration device (4); the stirring assembly comprises a motor, a transmission rod (6), and a stirring paddle (5) arranged on the transmission rod (6); the motor is arranged at the top of the tower body (1), and the transmission rod (6) is coaxially arranged inside the tower body (1); the aeration device (4) is arranged on the transmission rod (6); The first end of the baffle (2-2) is fixed to the inner wall of the shell (2-1) via an elastic member (2-3); except for the first end, the rest of the baffle (2-2) does not contact the inner wall of the shell (2-1) and can swing up and down within a certain range in the shell (2-1).
Citation Information
Patent Citations
Micro-electrolysis flocculation method for treating acid waste water containing heavy metals in mine
CN101948200A
Method for producing iron carbon micro-electrolysis filler from nonferrous metal waste ore slag
CN103332767A
Packed catalytic reaction column
CN104085977A
Efficient heterogeneous catalytic oxidation ferric-carbon micro-electrolysis packing and preparation method thereof
CN104761024A
Aeration cylinder
CN106732052A