Method for growing vertical tungsten disulfide on flexible carbon substrate, tungsten disulfide-carbon composite material and application thereof

By forming a carbon coating and growing tungsten trioxide on the carbon nanotube film, the problem of unstable vertical growth of tungsten disulfide nanosheets is solved, efficient vertical growth and active edge exposure are achieved, improving its application in the field of electrochemistry. potential.

CN115483041BActive Publication Date: 2024-10-22SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211124043.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2024-10-22
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

In the existing technology, tungsten disulfide nanosheets tend to slip when growing on carbon nanotube films, resulting in unstable vertical growth and shielding of active edges, limiting their application potential in the field of electrochemistry.

Method used

A carbon coating is formed on the carbon nanotube film, tungsten trioxide is grown by chemical vapor deposition, and then sulfide is performed to make the tungsten disulfide nanosheets grow vertically on the carbon coating to form a stable tungsten disulfide-carbon composite material.

Benefits of technology

The efficient vertical growth of tungsten disulfide nanosheets is achieved, ensuring more active edge exposure and improving its application prospects in the field of electrochemistry, especially its performance in supercapacitors and electrochemical drivers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115483041B_ABST
    Figure CN115483041B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for growing vertical tungsten disulfide on a flexible carbon substrate, a tungsten disulfide-carbon composite material and an application thereof. The method comprises: growing a carbon coating on a carbon nanotube film to obtain a carbon coating / carbon nanotube composite film; growing tungsten trioxide on its surface to obtain a tungsten trioxide / carbon coating / carbon nanotube composite film; and then performing a sulfurization treatment to make the formed tungsten disulfide nanosheets grow vertically on the carbon coating / carbon nanotube composite film to obtain a tungsten disulfide-carbon composite material. The present invention deposits a carbon coating on the surface of a CNT film that is prone to slip deformation by a chemical vapor deposition method, which can prevent the slippage of CNTs, improve the stability of the substrate, and then effectively realize the vertical growth of tungsten disulfide nanosheets, and the preparation process is simple and easy to control; and the prepared tungsten disulfide nanosheet has a high vertical rate, which largely ensures that more active edges are exposed, and has broad application prospects in the field of electrochemistry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for growing tungsten disulfide on a flexible carbon substrate, and in particular to a method for growing vertical tungsten disulfide nanosheets on a flexible carbon nanotube film substrate, and the obtained tungsten disulfide-carbon composite material and application thereof, belonging to the technical field of transition metal tungsten sulfide-nanocarbon composite materials. Background Art

[0002] Carbon nanotube (CNT) film is a complex conductive network formed by overlapping many CNTs. It has the characteristics of high strength, high modulus, high conductivity, etc. and is widely used in the field of smart materials. Tungsten disulfide (WS2) is a typical transition metal chalcogenide. It belongs to the hexagonal system. It has strong SWS covalent bonds within the layer and weak van der Waals forces between the layers. The thickness of the single layer is about 0.65nm. The preparation methods of tungsten disulfide nanosheets include tape stripping, hydrothermal method and chemical vapor deposition (CVD). Since the preparation method of CVD is simple to operate and can be finely controlled, it has become the main means of preparing WS2 nanosheets in recent years. For WS2, its exposed active edge has greater electrochemical activity and can be used in batteries, electrochemical hydrogen evolution and electrochemical drives. However, since WS2 is easy to agglomerate and spread out, it is very easy to stack, which further inhibits the exposure of the active edge. Coupled with its poor conductivity, its excellent performance cannot be fully utilized.

[0003] For example, the existing patent CN105280900A discloses a tungsten disulfide / graphene nanoribbon composite material and a preparation method thereof, and CN110911544A discloses a lightweight, flexible paper-based 1T phase tungsten disulfide / carbon nanotube composite thermoelectric material and a preparation method thereof. However, at present, the preparation of some CNT films and WS2 composite structures is simple, mostly by simple adsorption of dispersion liquid, and it is impossible to form an effective and stable composite structure; and, the CNT film and WS2 composite structure prepared by chemical vapor deposition method, because the CNTs inside the CNT film are easy to slip, the secondary grown WS2 thereon tends to stack in the horizontal direction, resulting in most of the WS2 edge active sites being shielded. Summary of the invention

[0004] The main purpose of the present invention is to provide a method for growing vertical tungsten disulfide on a flexible carbon substrate to overcome the shortcomings of the prior art.

[0005] Another object of the present invention is to provide a tungsten disulfide-carbon composite material and its application.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] An embodiment of the present invention provides a method for growing vertical tungsten disulfide on a flexible carbon substrate, which includes:

[0008] Providing carbon nanotube films;

[0009] Growing a carbon coating on the carbon nanotube film to obtain a carbon coating / carbon nanotube composite film;

[0010] Growing tungsten trioxide on the carbon coating / carbon nanotube composite film to obtain a tungsten trioxide / carbon coating / carbon nanotube composite film;

[0011] The tungsten trioxide / carbon coating / carbon nanotube composite film is subjected to a sulfurization treatment so that the formed tungsten disulfide nanosheets grow vertically on the carbon coating / carbon nanotube composite film to obtain a tungsten disulfide / carbon coating / carbon nanotube composite film, namely a tungsten disulfide-carbon composite material.

[0012] The embodiment of the present invention also provides a tungsten disulfide-carbon composite material prepared by the aforementioned method, which includes a carbon coating / carbon nanotube composite film as a flexible carbon substrate, and tungsten disulfide nanosheets vertically grown on the flexible carbon substrate.

[0013] The embodiment of the present invention also provides application of the tungsten disulfide-carbon composite material in the field of supercapacitors.

[0014] Compared with the prior art, the significant advantages and beneficial effects of the present invention are at least:

[0015] The present invention deposits a carbon coating on the surface of a CNT film that is prone to slip and deformation by a simple chemical vapor deposition method, thereby preventing the slip of CNTs and improving the stability of the substrate, thereby effectively realizing the vertical growth of tungsten disulfide nanosheets. The preparation process is simple and easy to control; moreover, the prepared tungsten disulfide nanosheets have a high vertical rate, and most of the nanosheets are in a vertical shape, which largely ensures that more active edges are exposed, and is conducive to further expanding its application prospects in the field of electrochemistry. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 is a flow chart of the preparation of WS2 / DG / CNT composite film in a typical implementation case of the present invention;

[0018] Figure 2This is a microscopic morphology of vertically grown WS2 nanosheets in a typical implementation case of the present invention.

[0019] Figure 3 This is a schematic diagram showing that WS2 in comparative example 1 tends to grow horizontally on a pure CNT film substrate.

[0020] Figure 4 It is a schematic diagram showing that WS2 tends to grow vertically on a composite DG / CNT film substrate in a typical implementation case of the present invention.

[0021] Figure 5 It is a comparison diagram of cyclic voltammetry curves of capacitance performance of WS2 / amorphous carbon / CNT composite film, amorphous carbon / CNT composite film, and CNT film in a typical implementation case of the present invention.

[0022] Figure 6 It is a comparison diagram of cyclic voltammetry curves of capacitance performance of WS2-horizontally grown and WS2-vertically grown in a typical implementation case of the present invention. DETAILED DESCRIPTION

[0023] In view of the many deficiencies in the prior art and the limitations of the materials, the inventors of this case, after long-term research and extensive practice, proposed the technical solution of the present invention, which mainly effectively combines the carbon nanotube film with WS2, and realizes the vertical growth of WS2 through technical means, which largely ensures that more active edges are exposed, and helps to further expand its application prospects in the field of electrochemistry. Specifically, it can be possible to add a carbon coating by chemical vapor deposition to prevent the slippage of CNTs and improve the stability of the substrate, which can improve the efficiency of the vertical growth of WS2 nanosheets and effectively realize the vertical growth of WS2 nanosheets.

[0024] The technical solution, its implementation process and principle will be further explained as follows.

[0025] An aspect of an embodiment of the present invention provides a method for growing vertical tungsten disulfide on a flexible carbon substrate, comprising:

[0026] Providing carbon nanotube (CNT) films;

[0027] Growing a carbon coating on the carbon nanotube film to obtain a carbon coating / carbon nanotube composite film;

[0028] Growing tungsten trioxide on the carbon coating / carbon nanotube composite film to obtain a tungsten trioxide / carbon coating / carbon nanotube composite film;

[0029] The tungsten trioxide / carbon coating / carbon nanotube composite film is subjected to a sulfurization treatment so that the formed tungsten disulfide (WS2) nanosheets grow vertically on the carbon coating / carbon nanotube composite film to obtain a tungsten disulfide / carbon coating / carbon nanotube composite film, that is, a tungsten disulfide-carbon composite material.

[0030] In some embodiments, the carbon coating may be amorphous graphene (DG), but is not limited thereto. The present invention increases the carbon coating by chemical vapor deposition, effectively achieving the vertical growth of WS2 nanosheets, preferably by a simple chemical vapor deposition (CVD) method, depositing a layer of amorphous graphene DG on the surface of a CNT film that is prone to slip deformation, and limiting and preventing the slip of CNTs, thereby improving the stability of the substrate, and effectively achieving the vertical growth of WS2 nanosheets. In addition, in addition to amorphous graphene, from the growth mechanism of the present invention, most other hard carbon layers can achieve the role of assisting vertical growth, such as glassy carbon layers, diamond-like carbon layers, etc., but are not limited thereto.

[0031] In some embodiments, the method includes: growing an amorphous graphene layer on a carbon nanotube film using a chemical vapor deposition method to obtain an amorphous graphene / carbon nanotube composite film.

[0032] Furthermore, the thickness of the amorphous graphene layer is 50nm-5μm. The thickness of the carbon nanotube film used in the present invention is not limited, and the deposition of amorphous carbon will not affect the internal structure of the carbon nanotube film, but only densifies the surface carbon nanotubes.

[0033] In some preferred embodiments of the present invention, the method may specifically include: placing a carbon nanotube film in a reaction chamber of a chemical vapor deposition device, introducing an inert protective gas, then raising the temperature of the reaction chamber to a growth temperature of 900 to 1300°C, while introducing a carbon source and a reducing gas, reacting for 10 to 60 minutes, and obtaining an amorphous graphene / carbon nanotube composite film.

[0034] Furthermore, the flow rate of the inert protective gas is 80-110 sccm.

[0035] Furthermore, the flow rate of the carbon source is 10 to 70 sccm.

[0036] In some embodiments, the preparation of the carbon coating in the present invention is mainly achieved by high-temperature cracking and recombination of the carbon source. The carbon source selected in the present invention is preferably methane. In addition to methane, it can also be replaced by other carbon sources, such as ethylene, ethanol, methanol, toluene, acetonitrile and other organic gases or organic liquids.

[0037] Furthermore, the flow rate of the reducing gas is 20-50 sccm.

[0038] Further, the reducing gas includes hydrogen, but is not limited thereto.

[0039] In some embodiments, the method includes: raising the temperature of the reaction chamber to a growth temperature of 900-1300° C. by using any one of a high-temperature tube furnace, transient Joule heat, a high-temperature spray gun, and the like.

[0040] In some embodiments, the method includes: using magnetron sputtering technology and tungsten as a target to prepare a tungsten trioxide / carbon coating / carbon nanotube composite film, wherein the process conditions used in the magnetron sputtering technology are: power of 20 to 400 W, gas pressure of 20 to 100 Pa, time of 20 to 60 min, and the thickness of the tungsten trioxide is above 50 nm.

[0041] In some embodiments, the method includes: placing the tungsten trioxide / carbon coating / carbon nanotube composite film in a high-temperature tube furnace, placing sulfur powder at the air inlet end of the furnace tube, introducing an inert protective gas, and then raising the temperature of the high-temperature tube furnace to a growth temperature of 500 to 900°C, reacting for 10 to 240 minutes, and forming tungsten disulfide nanosheets that grow vertically on the carbon coating / carbon nanotube composite film to obtain a tungsten disulfide / carbon coating / carbon nanotube composite film.

[0042] Furthermore, the flow rate of the inert protective gas is 100-500 sccm.

[0043] Another aspect of an embodiment of the present invention further provides a tungsten disulfide-carbon composite material prepared by the aforementioned method, which includes a carbon coating / carbon nanotube composite film as a flexible carbon substrate, and tungsten disulfide nanosheets vertically grown on the flexible carbon substrate.

[0044] Furthermore, the content of tungsten disulfide nanosheets in the tungsten disulfide-carbon composite material is 5 to 40 wt%.

[0045] Furthermore, the verticality rate of the tungsten disulfide nanosheets in the tungsten disulfide-carbon composite material is 10-60%.

[0046] Furthermore, the thickness of the tungsten disulfide nanosheet is 50-200 nm, and the vertical height is 20-170 nm.

[0047] Another aspect of the embodiments of the present invention further provides application of the tungsten disulfide-carbon composite material in the field of electrochemistry.

[0048] Furthermore, the improvement in the capacity of the tungsten disulfide-carbon composite material is conducive to its application in supercapacitors, exposing more active edges, forming fast electron and ion insertion and extraction, and can be applied to electrochemical driving.

[0049] In some specific embodiments, the method for growing vertical tungsten disulfide on a flexible carbon substrate proposed in the present invention is mainly prepared by multiple steps, specifically including the following steps:

[0050] S01: Deposit a layer of amorphous graphene (DG) on a pure CNT film substrate by chemical vapor deposition. The main operation method is to place the pure CNT film in a closed tube furnace, introduce inert protective gas Ar (flow rate of 80-110sccm), then heat the tube furnace to a growth temperature of 900-1300°C, then introduce carbon source methane (flow rate of 10-70sccm) and reducing gas hydrogen (flow rate of 20-50sccm), keep the growth temperature unchanged, keep the constant temperature time for 10-60min, and then cool naturally to obtain a DG / CNT composite film.

[0051] S02: The obtained DG / CNT composite film is processed through a magnetron sputtering device, the target material is tungsten (purity 99.99%), the coating conditions are: power of 30-500W, gas pressure of 0.5-100Pa, to prepare a WO3 / DG / CNT composite film.

[0052] S03: The prepared WO3 / DG / CNT composite film is placed in a high-temperature tubular furnace, high-purity sulfur powder (99%) is placed at the air inlet end of the furnace tube, and inert protective gas Ar (flow rate is 100-500sccm) is introduced, and then the tubular furnace is heated to the growth temperature of 500-900°C, the constant temperature time is 10-240min, and then naturally cooled to obtain the WS2 / DG / CNT composite film, that is, the aforementioned "tungsten disulfide-carbon composite material".

[0053] The technical scheme, implementation process and principle of the embodiment of the present invention will be further explained in combination with the embodiments and drawings as follows. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present invention and do not have any limiting effect on it. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.

[0054] Example 1

[0055] See also Figure 1 As shown, the method for growing vertical tungsten disulfide on a flexible carbon substrate in this embodiment specifically includes the following steps:

[0056] S01: Deposit a layer of amorphous graphene (DG) on a pure CNT film substrate by chemical vapor deposition. The main operation method is to place the pure CNT film in a closed tube furnace, introduce inert protective gas Ar (flow rate of 100sccm), and then heat the tube furnace to a growth temperature of 1050°C. At this time, carbon source methane (flow rate of 10sccm) and reducing gas hydrogen (flow rate of 20-40sccm) are introduced. At this time, the growth temperature is kept unchanged, the constant temperature time is 10-60min, and then the temperature is naturally lowered to obtain a DG / CNT composite film with a DG layer thickness of 50nm.

[0057] S02: The obtained DG / CNT composite film is processed through magnetron sputtering equipment, the target material is tungsten (purity 99.99%), the coating conditions are: power 20W, gas pressure 100Pa, time 60min, and WO3 / DG / CNT composite film is prepared, and the WO3 thickness is 55nm.

[0058] S03: The prepared WO3 / DG / CNT composite film is placed in a high-temperature tubular furnace, high-purity sulfur powder (99%) is placed at the air inlet end of the furnace tube, and inert protective gas Ar (flow rate is 200sccm) is introduced. Then the tubular furnace is heated to the growth temperature of 650°C, the constant temperature time is 60min, and then the temperature is naturally lowered to obtain the WS2 / DG / CNT composite film, that is, the aforementioned "tungsten disulfide-carbon composite material".

[0059] The WS2 nanosheets prepared in this embodiment have a high vertical rate, and most of the WS2 nanosheets are in a vertical shape, such as Figure 2 As shown. The thickness of the tungsten disulfide nanosheet is 50-200nm, and the vertical height is 20-170nm. Since this embodiment deposits a layer of amorphous graphene on the surface of the CNT film that is easy to slip and deform, the vertical growth of the WS2 nanosheet is effectively achieved by limiting the slip, as shown in FIG. Figure 4 shown.

[0060] Example 2

[0061] The method for growing vertical tungsten disulfide on a flexible carbon substrate in this embodiment specifically includes the following steps:

[0062] S01: Deposit a layer of amorphous graphene (DG) on a pure CNT film substrate by chemical vapor deposition. The main operation method is to place the pure CNT film in a closed tube furnace, introduce inert protective gas Ar (flow rate of 80sccm), then heat the tube furnace to the growth temperature of 900℃, then introduce carbon source methane (flow rate of 30sccm) and reducing gas hydrogen (flow rate of 20-40sccm), keep the growth temperature unchanged, keep the constant temperature time for 10-60min, and then cool naturally to obtain a DG / CNT composite film with a DG layer thickness of 1μm.

[0063] S02: The obtained DG / CNT composite film is processed through magnetron sputtering equipment, the target material is tungsten (purity 99.99%), the coating conditions are: power 200W, gas pressure 60Pa, time 40min, to prepare WO3 / DG / CNT composite film, WO3 thickness is 60nm.

[0064] S03: The prepared WO3 / DG / CNT composite film is placed in a high-temperature tubular furnace, high-purity sulfur powder (99%) is placed at the air inlet end of the furnace tube, and inert protective gas Ar (flow rate is 100sccm) is introduced, and then the tubular furnace is heated to the growth temperature of 500°C, the constant temperature time is 240min, and then naturally cooled to obtain the WS2 / DG / CNT composite film, that is, the aforementioned "tungsten disulfide-carbon composite material".

[0065] Example 3

[0066] The method for growing vertical tungsten disulfide on a flexible carbon substrate in this embodiment specifically includes the following steps:

[0067] S01: Deposit a layer of amorphous graphene (DG) on a pure CNT film substrate by chemical vapor deposition. The main operation method is to place the pure CNT film in a closed tube furnace, introduce inert protective gas Ar (flow rate of 110sccm), and then heat the tube furnace to the growth temperature of 1300℃, then introduce carbon source methane (flow rate of 20-70sccm) and reducing gas hydrogen (flow rate of 30-50sccm), keep the growth temperature unchanged, keep the constant temperature time for 60min, and then cool naturally to obtain a DG / CNT composite film with a DG layer thickness of 5μm.

[0068] S02: The obtained DG / CNT composite film is processed through magnetron sputtering equipment, the target material is tungsten (purity 99.99%), the coating conditions are: power 400W, gas pressure 20Pa, time 20min, and WO3 / DG / CNT composite film is prepared, and the WO3 thickness is 63nm.

[0069] S03: The prepared WO3 / DG / CNT composite film is placed in a high-temperature tubular furnace, high-purity sulfur powder (99%) is placed at the air inlet end of the furnace tube, and inert protective gas Ar (flow rate is 500sccm) is introduced. Then the tubular furnace is heated to the growth temperature of 900°C, the constant temperature time is 10 minutes, and then the temperature is naturally lowered to obtain the WS2 / DG / CNT composite film, that is, the aforementioned "tungsten disulfide-carbon composite material".

[0070] In the above examples 1-3, the carbon source selected for amorphous graphene (DG) is methane, and the heating method is a high-temperature tube furnace. The methane in this process can be replaced by other carbon sources, such as ethylene, ethanol, methanol, toluene, acetonitrile and other organic gases or organic liquids. The heating method in this process can also be replaced by transient Joule heat, high-temperature spray gun, etc.

[0071] The amorphous graphene (DG) in the above embodiments 1-3 may also be replaced by a glassy carbon layer, a diamond-like carbon layer, or the like.

[0072] Comparative Example 1

[0073] The difference between this comparative example and Example 1 is that WO3 is directly magnetron sputtered on the surface of the pure CNT film, and then WS2 is grown.

[0074] The results are as follows Figure 3 It shows that the WS2 in this comparative example tends to grow horizontally on the surface of the pure CNT film substrate. For tungsten disulfide, compared with the horizontal structure, the vertical structure will expose more chemically active sites and facilitate the insertion and extraction of electrons and ions in electrochemical behavior, which is very helpful for improving its overall capacitance performance. This result is from Figure 5 and Figure 6 It can be seen that the capacitance (usually reflected by the area of ​​the cyclic voltammetry curve) of tungsten sulfide with a vertical structure is larger than that of tungsten sulfide with a horizontal structure.

[0075] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other process operations and process conditions described in this specification, and obtained relatively ideal results.

[0076] In summary, the present invention deposits a carbon coating on the surface of a CNT film that is prone to slip and deformation by a chemical vapor deposition method, which can prevent the slip of CNTs and improve the stability of the substrate, thereby effectively realizing the vertical growth of tungsten disulfide nanosheets. The preparation process is simple and easy to control; and the prepared tungsten disulfide nanosheets have a high vertical rate, which to a large extent ensures that more active edges are exposed, and have broad application prospects in the field of electrochemistry.

[0077] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in every sense, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all New Year greetings falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered to limit the claim to which it relates.

Claims

1. A method for growing vertical tungsten disulfide on a flexible carbon substrate, characterized in that: include: Providing carbon nanotube films; Placing the carbon nanotube film in a reaction chamber of a chemical vapor deposition device, introducing an inert protective gas, then raising the temperature of the reaction chamber to a growth temperature of 900-1300°C, introducing a carbon source and a reducing gas at the same time, reacting for 10-60 minutes, growing an amorphous graphene layer on the carbon nanotube film, and preparing an amorphous graphene / carbon nanotube composite film, wherein the thickness of the amorphous graphene layer is 50 nm-5 μm; Adopting magnetron sputtering technology, taking tungsten as a target, growing tungsten trioxide on the amorphous graphene / carbon nanotube composite film to obtain a tungsten trioxide / amorphous graphene / carbon nanotube composite film, wherein the process conditions adopted by the magnetron sputtering technology are: power of 20-400 W, gas pressure of 20-100 Pa, time of 20-60 min, and the thickness of tungsten trioxide is above 50 nm; The tungsten trioxide / amorphous graphene / carbon nanotube composite film is placed in a high-temperature tube furnace, sulfur powder is placed at the air inlet end of the furnace tube, and an inert protective gas is introduced, and then the temperature of the high-temperature tube furnace is raised to a growth temperature of 500-900°C, and the reaction is carried out for 10-240 minutes, and the formed tungsten disulfide nanosheets are vertically grown on the carbon coating / carbon nanotube composite film to obtain a tungsten disulfide / amorphous graphene / carbon nanotube composite film, that is, a tungsten disulfide-carbon composite material; The tungsten disulfide-carbon composite material includes an amorphous graphene / carbon nanotube composite film as a flexible carbon substrate, and a tungsten disulfide nanosheet vertically grown on the flexible carbon substrate. The content of the tungsten disulfide nanosheet in the tungsten disulfide-carbon composite material is 5-40 wt %, the vertical rate of the tungsten disulfide nanosheet in the tungsten disulfide-carbon composite material is 10-60%, the thickness of the tungsten disulfide nanosheet is 50-200 nm, and the vertical height is 20-170 nm.

2. The method according to claim 1, characterized in that: The flow rate of the inert protective gas introduced into the reaction chamber of the chemical vapor deposition equipment is 80-110 sccm.

3. The method according to claim 1, characterized in that: The flow rate of the carbon source is 10-70 sccm.

4. The method according to claim 1, characterized in that: The carbon source is selected from any one of methane, ethylene, ethanol, methanol, toluene and acetonitrile, or a combination of two or more thereof.

5. The method according to claim 1, characterized in that: The flow rate of the reducing gas is 20-50 sccm.

6. The method according to claim 1, characterized in that: The reducing gas is hydrogen.

7. The method according to claim 1, characterized in that include: The temperature of the reaction chamber is raised to a growth temperature of 900-1300°C by using any one of a high temperature tube furnace, transient Joule heat, and a high temperature spray gun.

8. The method according to claim 1, characterized in that: The flow rate of the inert protective gas introduced into the high temperature tube furnace is 100~500 sccm.

9. A tungsten disulfide-carbon composite material prepared by the method according to any one of claims 1 to 8, comprising an amorphous graphene / carbon nanotube composite film as a flexible carbon substrate, and tungsten disulfide nanosheets vertically grown on the flexible carbon substrate, wherein the content of the tungsten disulfide nanosheets in the tungsten disulfide-carbon composite material is 5-40 wt %, the vertical rate of the tungsten disulfide nanosheets in the tungsten disulfide-carbon composite material is 10-60%, the thickness of the tungsten disulfide nanosheets is 50-200 nm, and the vertical height is 20-170 nm.

10. Use of the tungsten disulfide-carbon composite material according to claim 9 in the field of supercapacitors.