A kind of flexible nano-conductive silver paste and preparation method thereof
By using a combination of nano-silver wires and hydroxyethyl methacrylate phosphate and other components in conductive silver paste, the problems of poor conductivity and bending resistance are solved, and the conductive properties and flexible nano-conductive silver paste are achieved. Improved, ensuring efficient conductivity and bending resistance.
Patent Information
- Application Number
- CN202211064825.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-01
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-09-01
AI Technical Summary
The existing conductive silver paste has poor dispersion performance when the silver powder content is high, resulting in poor conductivity and bending resistance. The conductivity is also poor when the silver powder content is low, and the low silver powder accumulation density leads to increased resistance.
Use nano silver wire 60-70%, hydroxyethyl methacrylate phosphate 1-5%, solvent 10-20%, polyurethane prepolymer 5-10%, defoaming agent 1-5%, curing agent 1- 10%, dispersant 0. The combination of 01-0.05% improves the stability and adhesion of nanosilver wires in polyurethane prepolymer through hydrogen bonding, controls the viscosity in the range of 150-300Pa·S, and ensures conductive properties and bending resistance.
It improves the electrical conductivity and bending resistance of the conductive silver paste, enhances the dispersion and bonding properties of nano silver wires, reduces the resistance change rate, and improves the adhesion and flexibility of the flexible nano conductive silver paste.
Smart Images

Figure BDA0003827901150000041 
Figure BDA0003827901150000051 
Figure BDA0003827901150000052
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silver paste, and in particular to a flexible nano conductive silver paste and a preparation method thereof. Background Art
[0002] With the rapid development of the electronic information industry, various novel high-tech electronic products have gradually entered the public's field of vision and are widely favored by people. Flexible screens can meet the needs of the new era by virtue of their bendable form. Their application in mobile phones, the Internet of Things, and wearable devices will bring new consumer experiences.
[0003] There are differences in the use requirements of conductive silver paste and conductive ink. Although both conductive silver paste and conductive ink use conductive silver powder as conductive filler, and are stirred and dispersed with polymer resin, solvent, curing agent, additives, etc. to form a uniform slurry, the conductive ink layer is equivalent to a capacitor when used, and the conductive silver paste is printed around the conductive ink layer, which is equivalent to a conductive circuit. Therefore, when the existing conductive ink is used to replace the conductive silver paste, when the silver powder content is high, the silver powder is not fully dispersed in the resin. After several bends, the silver powder will gradually separate from the resin and affect the conductivity of the silver paste. When the silver powder content is low, the packing density of the silver powder is low, and the conductive performance is relatively poor. After several bends, the gap between the silver powder at the bend increases, resulting in a rapid increase in resistance. Therefore, the silver powder content has an important influence on the conductive performance and bending resistance of the conductive silver paste. Summary of the invention
[0004] In view of the problem in the prior art that when the silver powder content is high, the dispersion performance of the silver powder in the resin is poor, resulting in poor conductivity and bending resistance of the conductive silver paste, the present application provides a flexible nano conductive silver paste, which can achieve good results in the dispersion performance and bending resistance of the conductive silver paste after the silver powder content is increased.
[0005] The first object of the present invention is to provide a flexible nano-conductive silver paste using the following technical solution:
[0006] A flexible nano-conductive silver paste comprises the following components in weight percentage: 60-70% of nano silver wire, 1-5% of hydroxyethyl methacrylate phosphate, 10-20% of solvent, 5-10% of polyurethane prepolymer, 1-5% of defoamer, 1-10% of curing agent and 0.01-0.05% of dispersant.
[0007] Preferably, by weight percentage, the weight percentage content of each component is as follows: 65-70% of nano silver wire, 2-5% of hydroxyethyl methacrylate phosphate, 15-20% of solvent, 5-10% of polyurethane prepolymer, 1-5% of defoamer, 1-10% of curing agent, and 0.01-0.05% of dispersant.
[0008] Preferably, the diameter of the silver nanowire is 30-50 nm and the length is 3-8 μm.
[0009] Preferably, the relative molecular weight of the polyurethane prepolymer is 100-1000.
[0010] Preferably, the viscosity of the flexible nano-conductive silver paste is 150-300 Pa·S.
[0011] Preferably, the solvent is a mixture of ethylene glycol butyl ether and any one of terpineol and diethylene glycol ethyl ether acetate, and the weight ratio of ethylene glycol butyl ether:terpineol or ethylene glycol butyl ether:diethylene glycol ethyl ether acetate is 1:(0.08-0.1).
[0012] Preferably, the curing agent is a polyisocyanate curing agent.
[0013] Preferably, the curing temperature of the nano silver paste is 120-135°C.
[0014] Preferably, the dispersant is cellulose ethers. More preferably, the cellulose ethers can be selected from any one, any two, or any three of methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose.
[0015] The second object of the present invention is to provide a method for preparing a flexible nano-conductive silver paste, which specifically comprises the following preparation steps: (1) firstly stirring and mixing a dispersant and a part of a solvent uniformly;
[0016] (2) Add the remaining solvent and polyurethane prepolymer in parts by weight into the mixture in step (1) and mix them evenly, then add nano silver wire, defoaming agent and curing agent in turn and stir them evenly to obtain nano conductive silver paste.
[0017] By adopting the above technical scheme, when the content of nano silver wires in the present application is selected within the range of 60-70%, not only the conductive performance of the conductive silver paste is effectively improved, but also hydroxyethyl methacrylate phosphate, solvent, polyurethane prepolymer, defoamer, curing agent and dispersant are selected and used in combination with high-content nano silver wires, which solves the dispersion problem of high-concentration nano silver wires in polyurethane prepolymers in the prior art, thereby improving the dispersion performance and stability of the nano silver wires in polyurethane, thereby greatly enhancing the adhesion performance and anti-bending performance of the conductive silver paste. The reason may be that the hydrogen bonding effect between the hydroxyl groups on the hydroxyethyl methacrylate phosphate molecules and the polyurethane prepolymer improves the stability and adhesion of the nano silver wires in the polyurethane prepolymer, thereby greatly enhancing the adhesion and anti-bending performance of the conductive silver paste.
[0018] In addition, the purpose of using polyurethane prepolymer in this application is that the polyurethane prepolymer is not completely cured, so it can solidify the nano-conductive silver paste, and at the same time ensure the bonding effect of the polyurethane prepolymer on the nano-silver wire, effectively ensuring the overlap between the nano-silver wires, while the already cured polyurethane cannot play the role of re-curing, and naturally does not have the bonding effect on the nano-silver wire.
[0019] When the silver powder content is too high, the probability of being coated by the polyurethane prepolymer is reduced, and the adhesion between the nano-silver wires after curing into a film is relatively poor, and there is a risk of the nano-silver wires falling off. Therefore, in this application, the maximum content of the nano-silver wire is limited to 70%, which can not only effectively ensure the conductive properties of the nano-conductive silver paste, but also effectively ensure the adhesion properties between the nano-silver wires.
[0020] In the present application, not only the content of nano silver wire is increased, but also the diameter of the nano silver wire is further limited to 30-50nm and the length is 3-8μm. The first purpose is to ensure that the diameter of the silver wire in the nano conductive silver paste is uniform and reliable, and the nano silver wires can be overlapped together during the curing process of the nano silver paste to ensure the conductive performance of the nano silver paste; the second purpose is to ensure the screen printing effect of the nano silver paste. If the aspect ratio of the nano silver wire is too large, it means that the length of the nano silver wire is longer, and the aperture of the screen is relatively small, resulting in the nano silver wire cannot pass through the screen and be printed on the substrate, resulting in poor screen printing effect, which is not conducive to the conductive performance of the nano silver paste.
[0021] The content of polyurethane prepolymer plays a decisive role in the mechanical properties and bending resistance of conductive silver paste, and also has a great influence on the wetting and dispersibility of nano-silver wires. With the increase of polyurethane prepolymer content, the fluidity, printability and conductivity of conductive silver paste are better. However, when the resin content exceeds a certain value, it is difficult to form a stable conductive path between nano-silver wires, which will reduce the conductivity of conductive silver paste.
[0022] When the polyurethane prepolymer with a relative molecular weight in the range of 100-1000 is selected in the present application, the nano silver paste obtained finally has good adhesion, and the dispersion performance of the nano silver wire in the polyurethane prepolymer can also be guaranteed. With the increase of the relative molecular weight, the flexibility of the polyurethane prepolymer is better. During the curing process, the polyurethane prepolymer is more likely to deform and shrink, so it is easier to form a tightly packed structure. In this denser resin structure, the nano silver wires are more likely to overlap each other, and electron migration is more likely to occur, so the conductivity is better. However, when the relative molecular weight is too large, the interface layer will be too thick to destroy the bridge effect between the nano silver wires, thereby reducing the conductivity of the conductive silver paste. If the relative molecular weight is too small, the interface mechanical properties will be poor.
[0023] After the solvent of the present application is selected as a mixture of ethylene glycol butyl ether and pinene alcohol or a mixture of ethylene glycol butyl ether and diethylene glycol ethyl ether acetate, not only can the nano silver paste obtained in the present application be cured at 120-135°C, but the experiment also found that the mixed solvent has the best matching with the nano silver wire, which helps to fully disperse the nano silver wire in the polyurethane prepolymer and effectively prevent the sedimentation of the nano silver wire due to agglomeration. Therefore, after the solvent of the present application is selected as a mixture of ethylene glycol butyl ether and pinene alcohol or a mixture of ethylene glycol butyl ether and diethylene glycol ethyl ether acetate, it can not only dissolve the polyurethane prepolymer, but also help to evenly disperse the nano silver wire in the polyurethane prepolymer.
[0024] In the present application, hydroxyethyl methacrylate phosphate, solvent, defoamer, curing agent and dispersant are used in combination to control the viscosity of the nano conductive silver paste within the range of 150-300 Pa·S, thereby ensuring the formation of droplets of the nano silver paste during printing and the effective diffusion of the droplets on the substrate.
[0025] If the viscosity is too low, the nano-conductive silver paste will easily disperse after printing, resulting in uneven edges of the printed circuits. At the same time, the printed film thickness is thin, which will reduce the electrical properties of the conductive circuit layer. If the viscosity is too high, the nano-conductive silver paste will have low flowability and will not be easy to level, which may cause gaps between the nano-silver wires, affecting the overlap of the nano-silver wires, and further causing partial defects in the cured circuit layer, which will also affect the conductive properties of the nano-conductive silver paste.
[0026] In addition, the nano-conductive silver paste obtained in the present application can be cured under the condition of 120-135° C., and the curing time is 20-30 minutes, which reduces the use cost of the nano-silver paste. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below with reference to the embodiments.
[0028] The existing flexible touch screen includes a liquid crystal display part and a liquid crystal touch part of the liquid crystal screen, the liquid crystal touch part of the liquid crystal screen includes a polarizer substrate, a liquid crystal protection cover plate bonded to the upper surface of the polarizer substrate by OCA glue, a first PET substrate layer bonded to the liquid crystal protection cover plate by OCA glue, a first bonding layer bonded to the upper surface of the first PET substrate layer, a first circuit layer bonded to the upper surface of the first bonding layer, a second PET substrate layer bonded to the first circuit layer, a second bonding layer bonded to the upper surface of the second PET substrate layer, a second circuit layer bonded to the upper surface of the second bonding layer, and a touch cover plate bonded to the second circuit layer, the first circuit layer and the second circuit layer form two plates of a capacitor, wherein the first circuit layer and the second circuit layer are both made of conductive ink. Since conductive ink is equivalent to the plate of a capacitor, it does not have very high requirements for the content of nano silver wires, which is generally less than 60%. At the same time, the existing conductive ink needs to have good bonding properties with the bonding layer and the PET base layer, so the resin content in the conductive ink needs to be higher to ensure the bonding performance between the conductive ink and other layers. The increase in resin content will not only lead to a decrease in the conductivity of the ink, but also high resin will make the overlapping performance of the nano silver wires poor. As a result, when the conductive ink is used as the circuit layer in the liquid crystal touch part, its conductivity will be relatively poor.
[0029] Therefore, based on the above problems, the inventors further discovered through research that after adjusting the content of nano silver wires, solvents, polyurethane prepolymers, etc. and combining them with hydroxyethyl methacrylate phosphate, the obtained nano silver paste can be screen-printed on the edge of the conductive ink (equivalent to the role of the wire), which can connect the conductive ink into the circuit, and the conductive silver paste has better conductivity.
[0030] The specific embodiments of this application are typical cases in the experimental process, which serve as examples to illustrate the experimental process of the creative work of this application, but do not represent that this is the entire work of this application.
[0031] The preparation method of the nano-conductive silver paste of the present application comprises the following steps:
[0032] (1) First, stir and mix the dispersant and 2g of solvent evenly;
[0033] (2) Add the remaining solvent and polyurethane prepolymer in parts by weight into the mixture in step (1) and mix them evenly, then add nano silver wire, defoaming agent and curing agent in turn and stir them evenly to obtain nano conductive silver paste.
[0034] Embodiment 1.1-1.4: The diameter of the nano silver wire is 30 nm and the length is 3 μm; the relative molecular weight of the polyurethane prepolymer is 100; the specific mass fraction of the nano silver paste is as follows:
[0035]
[0036]
[0037] The viscosity of the nano-conductive silver paste obtained after mixing the raw materials in Example 1.1-1.2 is 150 Pa·S.
[0038] The viscosity of the nano-conductive silver paste obtained after mixing the raw materials in Example 1.3-1.4 is 272 Pa·S.
[0039] Example 2 is different from Example 1 in that the content of each raw material component is changed, and the specific content of the components is shown in the following table:
[0040]
[0041]
[0042] The viscosity of the nano-conductive silver paste obtained after mixing the raw materials in Example 2.1 is 182 Pa·S.
[0043] Example 2.2 The viscosity of the nano-conductive silver paste obtained after mixing the raw materials is 221 Pa·S.
[0044] The viscosity of the nano-conductive silver paste obtained after mixing the raw materials in Example 2.3 is 240 Pa·S.
[0045] The viscosity of the nano-conductive silver paste obtained after mixing the raw materials in Example 2.4 is 300 Pa·S.
[0046] Examples 3.1-3.4 were prepared according to the formula in Example 2, and the diameter of the nano silver wire was 30 nm and the length was 8 μm.
[0047] Examples 4.1-4.4 were prepared according to the formula in Example 2, and the diameter of the nano silver wire was 50 nm and the length was 8 μm.
[0048] Examples 5.1-5.4 were prepared according to the formula in Example 2, and a polyurethane prepolymer with a relative molecular weight of 1000 was selected.
[0049] Comparative Examples 5.1-5.4, prepared according to the formula in Example 2, using a polyurethane prepolymer with a relative molecular weight of 1500
[0050] In Examples 6.1-6.4, other components remain unchanged, and ethylene glycol butyl ether is replaced by a mixture of ethylene glycol butyl ether and pinene alcohol, specifically: ethylene glycol butyl ether: pinene alcohol is 1:0.08.
[0051] In Examples 7.1-7.4, other components remain unchanged, and ethylene glycol butyl ether is replaced by a mixture of ethylene glycol butyl ether and pinene alcohol, specifically: ethylene glycol butyl ether: pinene alcohol is 1:0.1.
[0052] Comparative Example 1
[0053] The scheme of Example 2 in CN105702323A is adopted, specifically a flexible conductive silver paste. Taking the total mass of the flexible conductive silver paste as 100%, the mass percentage of each component is as follows: 60% of silver nanowires, 1% of hydroxyethyl methacrylate phosphate, 18% of butyl acetate, 15% of polyurethane prepolymer, 5% of polyvinyl alcohol butyl ether, 0.5% of defoaming agent, and 0.5% of curing agent.
[0054] Comparative Example 2.1
[0055] The difference from Example 2 is that, calculated by weight, the contents of the components are as follows: 65 g of nanosilver wire, 2 g of hydroxyethyl methacrylate phosphate, 15 g of ethylene glycol butyl ether, 15 g of polyurethane prepolymer, 1 g of defoamer, 1.99 g of curing agent, and 0.01 g of dispersant.
[0056] Comparative Example 2.2
[0057] The difference from Example 2 is that, calculated by weight, the contents of the components are as follows: 75 g of nanosilver wire, 3 g of hydroxyethyl methacrylate phosphate, 12 g of ethylene glycol butyl ether, 6 g of polyurethane prepolymer, 2 g of defoamer, 1.99 g of curing agent, and 0.01 g of dispersant.
[0058] Comparative Examples 3.1-3.4
[0059] The difference from Example 2 is that methylcellulose is replaced by an equal amount of oleic acid.
[0060] Comparative Examples 4.1-4.4
[0061] The difference from Example 2 is that hydroxyethyl methacrylate phosphate is replaced by an equal amount of (2-hydroxyethyl) methacrylate.
[0062] Performance Testing
[0063] The flexible nano silver paste obtained in the above examples and comparative examples was screen printed on a PET substrate, and the following performance tests were performed after curing at 120° C. for 30 minutes. During the test, each group of examples was tested multiple times and the average value was taken.
[0064] (1) Salt spray resistance test. The conditions of the salt spray resistance test are as follows: solution concentration: 5% NaCl, test temperature: (35±2)°C, solution pH value: 6.9, test time: 24h, precipitation amount: 1.42ml / h (80cm 2 ).
[0065] (2) After the salt spray test, the flexibility and conductive properties of the flexible nano-silver paste were tested. The flexibility was characterized by its anti-bending property. The flexible nano-silver paste sample was folded 180° from front to back and then pressed on the fold line with a 2.5 kg weight for 1 min. The film was opened and the resistance of the silver wire was measured. The sample was folded repeatedly and measured multiple times. The number of anti-bending times when ΔR / R (resistance change rate) ≤ 80% was recorded. The more anti-bending times, the better the anti-bending property of the flexible nano-silver paste.
[0066] Adhesion test: The adhesion of the sample is tested according to the standard "Standard method for measuring the adhesion of coatings with tape". The classification table of adhesion test results is shown in the following table
[0067]
[0068] Table 1 Nano-conductive silver paste performance test results
[0069]
[0070]
[0071] The bending resistance of the nano-conductive silver paste is a comprehensive reflection of the adhesion and flexibility of the nano-conductive silver paste. When the flexibility is good and the adhesion is good, the prepared nano-conductive silver paste has the most bending resistance times. It can be seen from Table 1 that the volume resistivity bending resistance times of the nano-conductive silver paste obtained in the embodiment of the present application is much higher than the bending resistance times in Comparative Examples 1 and 2, and the adhesion of the nano-conductive silver paste obtained in the embodiment of the present application is also better than the adhesion in Comparative Examples 1 and 2, and the volume resistivity is lower than the volume resistivity in Comparative Examples 1 and 2, indicating that the components and proportions in the present application can ensure the conductive performance and flexibility of the nano-conductive silver paste when they are within the scope of the present application.
[0072] It can be seen from Comparative Example 5 that when the relative molecular weight of the polyurethane prepolymer is selected to be 1500, the volume resistivity increases, indicating that the conductivity deteriorates. The reason is that the higher the molecular weight of the polyurethane prepolymer, the better the flexibility of the polyurethane prepolymer. However, when the molecular weight exceeds the limit of the present application, its flexibility will not change much, and the rigidity will increase instead. This is because during the curing process, the polyurethane prepolymer with better flexibility is more likely to deform and shrink, and thus it is easier to form a tightly packed structure. In this denser resin structure, the nano silver wires are more likely to overlap with each other, and electron migration is more likely to occur, so the conductivity is better. When the molecular weight of the polyurethane prepolymer is too high, the molecules are already closely connected, and the space left for the polyurethane prepolymer to shrink and deform is reduced. It becomes relatively difficult for the nano silver wires to squeeze into the gaps between the resin molecules, resulting in an increase in the volume resistivity and a deterioration in the conductivity.
[0073] It can be seen from Comparative Example 3 that when oleic acid is used as a dispersant, the volume resistivity of the nano-conductive silver paste increases significantly. The main reason is that the dispersion performance of the nano-silver wires in the polyurethane prepolymer is relatively poor, and the nano-silver wires cannot be effectively overlapped, which leads to relatively poor conductivity of the nano-silver paste.
[0074] It can be seen from Comparative Example 4 that when (2-hydroxyethyl) methacrylate replaces hydroxyethyl methacrylate phosphate, the volume resistivity is significantly increased compared with Example 2, and the number of bending resistance is also reduced, indicating that the matching effect of hydroxyethyl methacrylate phosphate and polyurethane prepolymer is better, which is more helpful to improve the conductive performance and flexibility of nano conductive silver paste.
[0075] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A flexible nano-conductive silver paste, characterized in that: Calculated by weight percentage, the weight percentage content of each component is as follows: 65-70% of nano silver wire, 2-4% of hydroxyethyl methacrylate phosphate, 15-20% of solvent, 5-9% of polyurethane prepolymer, 1-5% of defoamer, 1-10% of curing agent, and 0.01-0.05% of dispersant; the diameter of the nano silver wire is 30-50nm, the length is 3-8μm, and the relative molecular weight of the polyurethane prepolymer is 100-1000.
2. The flexible nano-conductive silver paste according to claim 1, characterized in that: The viscosity of the flexible nano-conductive silver paste is 150-300 Pa·S.
3. The flexible nano-conductive silver paste according to claim 1, characterized in that: The solvent is a mixture of ethylene glycol butyl ether and any one of terpineol and diethylene glycol ethyl ether acetate, and the weight ratio of ethylene glycol butyl ether: terpineol or ethylene glycol butyl ether: diethylene glycol ethyl ether acetate is 1: (0.08-0.1).
4. The flexible nano-conductive silver paste according to claim 1, characterized in that: The curing agent is a polyisocyanate curing agent.
5. The flexible nano-conductive silver paste according to claim 1, characterized in that: The curing temperature of the flexible nano-conductive silver paste is 120-135°C.
6. The flexible nano-conductive silver paste according to claim 1, characterized in that: The dispersant is cellulose ether.
7. A method for preparing the flexible nano-conductive silver paste according to any one of claims 1 to 6, characterized in that: The method comprises the following preparation steps: (1) First, stir and mix the dispersant and part of the solvent evenly; (2) The remaining solvent and polyurethane prepolymer are added to the mixture in step (1) in parts by weight and mixed evenly, and then nano silver wires, defoaming agent, curing agent, and hydroxyethyl methacrylate phosphate are added in turn and stirred evenly to obtain nano conductive silver paste.
Citation Information
Patent Citations
Flexible conductive silver paste and manufacturing method
CN105702323A
Low-temperature conductive silver paste and preparation method and application thereof
CN106024100A
Conductive ink composition for printing of radio frequency identification system
CN106147385A
Preparation method of ultraviolet light cured conductive silver paste
CN108257708A
Low-temperature conductive silver paste and heterojunction battery
CN114023490A