A catalyst for electrochemical nitrate conversion into ammonia and a preparation method thereof

By anchoring Cu/M-TiO2 electrocatalyst at the Cu/M heterogeneous phase interface on the TiO2 surface, the problem of low efficiency and selectivity in the conversion of electrochemical nitrates into ammonia is solved, and the efficient ammonia generation and industrial applicability are achieved. The effectiveness of the adaptive site switching mechanism is achieved.

CN115505963BActive Publication Date: 2024-11-29ZHEJIANG ZHENENG TECHN RES INST CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211294519.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-21
Publication Date
2024-11-29
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

The conversion efficiency and ammonia production selectivity of electrochemical nitrate conversion and synthesis of ammonia are low, mainly due to the lack of understanding of the mechanism of action of reaction intermediates at the catalyst surface interface, resulting in a single active site and a blurred synergistic effect of hydrogenation.

Method used

Using Cu/M-TiO2 electrocatalyst, the catalyst is prepared by anchoring the Cu/M heterophase interface on the surface of TiO2, and ion exchange and high-temperature calcination methods to achieve the adaptive site switching mechanism of NO3-, reduce the reaction barrier and accelerate the Ammonia production.

Benefits of technology

It significantly improves the efficiency and ammonia production selectivity of electrochemical nitrate conversion and synthesis of ammonia, is suitable for industrial applications, and the effectiveness of the adaptive site switching mechanism is verified through density functional theory.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115505963B_ABST
    Figure CN115505963B_ABST
Patent Text Reader

Abstract

The present invention relates to an electrochemical nitrate conversion ammonia synthesis catalyst and a preparation method thereof, and belongs to the technical field of ammonia synthesis catalyst application. The present invention discloses an electrochemical nitrate conversion ammonia synthesis catalyst, which is a Cu / M-TiO2 electrocatalyst (M is any one of Fe, Ni, Co, Pt, Ru or Ir), wherein the Cu / M heterogeneous phase interface is anchored on the TiO2 surface. The catalyst of the present invention has a good catalytic effect and can greatly improve the efficiency of electrochemical nitrate conversion ammonia synthesis. In addition, the present invention also discloses a preparation method of an electrochemical nitrate conversion ammonia synthesis catalyst, which is mainly prepared by ion exchange and high-temperature calcination. The preparation method is simple and convenient, suitable for mass preparation, and is conducive to the industrial application of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of synthetic ammonia catalysts and relates to an electrochemical nitrate conversion synthetic ammonia catalyst and a preparation method thereof. Background Art

[0002] The electrochemical nitrate conversion method for synthesizing ammonia can not only realize the resource utilization of waste, but also serve as an alternative to the traditional Haber-Bosch method for synthesizing ammonia. However, the low conversion efficiency and ammonia production selectivity have limited the development of this technology to a certain extent. The key lies in the lack of understanding of the mechanism of reaction intermediates at the catalyst surface interface. The existing interpretation mainly involves two aspects: first, the single active site, that is, the reaction is carried out at one active site; second, the hydrogenation synergistic effect (a vague concept).

[0003] Therefore, a new electrochemical nitrate conversion catalyst for ammonia synthesis can be provided based on the above principle. Summary of the invention

[0004] In view of this, one of the objects of the present invention is to provide a catalyst for electrochemical nitrate conversion to ammonia synthesis; a second object of the present invention is to provide a method for preparing the catalyst for electrochemical nitrate conversion to ammonia synthesis.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] 1. An electrochemical nitrate conversion ammonia synthesis catalyst, the catalyst is a Cu / M-TiO2 electrocatalyst, in which the Cu / M heterogeneous phase interface is anchored on the TiO2 surface;

[0007] Wherein M is any one of Fe, Ni, Co, Pt, Ru or Ir.

[0008] Preferably, the molar ratio of Cu to M is 1:9 to 9:1.

[0009] Preferably, the molar ratio of Cu to TiO2 is 1:5 to 1:50.

[0010] 2. The preparation method of the electrochemical nitrate conversion ammonia synthesis catalyst is as follows:

[0011] (1) Preparation of Na2Ti3O7 nanorods: titanium dioxide is added to a sodium hydroxide solution, ultrasonically dispersed to make it uniform, treated in a high pressure hydrothermal reactor at 150-180°C for more than 10 hours, centrifuged, washed, and dried to obtain Na2Ti3O7 nanorods for use;

[0012] (2) Preparation of catalyst (Cu / M-TiO2 electrocatalyst): The Na2Ti3O7 nanorods prepared in step (1) are added to a solution containing M halide and CuCl2, and are evenly dispersed by ultrasonication. The nanorods are then transferred to an oscillating reactor for ion exchange treatment for more than 24 hours. The nanorods are centrifuged, washed, and dried, and then calcined at 750-850°C for 200-300 minutes in a mixed atmosphere of argon and hydrogen to obtain a catalyst (Cu / M-TiO2 electrocatalyst).

[0013] Preferably, the mass molar ratio of titanium dioxide to sodium hydroxide is 2:0.3-3, g:mol.

[0014] Preferably, the mass molar ratio of Ti to CuCl2 in the Na2Ti3O7 nanorods is 5 to 50:1;

[0015] The molar ratio of M to CuCl2 in the M halide is 1:9 to 9:1.

[0016] Preferably, the volume ratio of argon to hydrogen in the mixed atmosphere is 4:1.

[0017] The beneficial effects of the present invention are:

[0018] 1. The present invention discloses a catalyst for electrochemical nitrate conversion to ammonia, which is a Cu / M-TiO2 electrocatalyst (M is any one of Fe, Ni, Co, Pt, Ru or Ir), and the Cu / M heterogeneous phase interface is anchored on the TiO2 surface. The catalyst of the present invention has a good catalytic effect and can greatly improve the efficiency of electrochemical nitrate conversion to ammonia.

[0019] 2. The present invention also discloses a method for preparing an electrochemical nitrate conversion catalyst for synthesizing ammonia, which is mainly prepared by ion exchange and high-temperature calcination. The preparation method is simple and convenient, suitable for large-scale preparation, and is conducive to the industrial application of the catalyst. It has certain universality and is suitable for preparing other Cu / M (M=Fe, Ni, Co, Pt, Ru, Ir, etc.) catalyst preparation methods.

[0020] 3. The present invention proposes a new adaptive site switching mechanism. Along this path, the potential barrier of the reaction can be effectively reduced and the reaction can be accelerated. The reason is that: when the electrochemical nitrate conversion ammonia synthesis catalyst of the present invention is used, the nitrate reduction process is not carried out only on a single heterogeneous interface, but on NO3 - First, it is adsorbed on the metal M in the surface, and then the adsorbed NO3 - Migrate to the Cu / M interface to generate NO3 - Reduction, followed by the gradual transfer of adsorbed *NH3 to the Cu in the surface, which accelerates the removal of NH3 and realizes NO3- Efficient conversion to NH3.

[0021] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0023] Figure 1 Schematic diagram of the synthesis of Cu / Fe-TiO2 catalyst in Example 1;

[0024] Figure 2 TEM images of the Cu / Fe-TiO2 catalyst prepared in Example 1, wherein a and b are at different magnifications;

[0025] Figure 3 The selected area electron diffraction pattern of the Cu / Fe-TiO2 catalyst prepared in Example 1;

[0026] Figure 4 It is a high-magnification TEM image, where a and b are different magnifications;

[0027] Figure 5 HAADF mapping of the Cu / Fe-TiO2 catalyst prepared in Example 1

[0028] Figure 6 This is a diagram showing the mechanism of action of the nitrate conversion to ammonia synthesis catalyst (Cu / Fe-TiO2 electrocatalyst) prepared in the present invention. DETAILED DESCRIPTION

[0029] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.

[0030] Example 1

[0031] A method for preparing a nitrate conversion ammonia synthesis catalyst (Cu / Fe-TiO2 catalyst), the synthesis schematic diagram of which is as follows Figure 1 The specific method is as follows:

[0032] (1) Preparation of Na2Ti3O7 nanorods: 2.0 g of P25 titanium dioxide was added to 30 mL of 10 M NaOH solution, and the mixture was fully dispersed by strong ultrasonication and then treated in a high pressure hydrothermal reactor at 180° C. for 12 h. The Na2Ti3O7 nanorods were then centrifuged, washed, and dried to obtain the Na2Ti3O7 nanorods for later use.

[0033] (2) Preparation of Cu / Fe-TiO2 catalyst: 5.03 g of Na2Ti3O7 nanorods prepared in step (1) were added to 20 mL of a solution containing 10 mmol FeCl3·6H2O and 10 mmol CuCl2·2H2O, and the nanorods were fully dispersed by strong ultrasound. The nanorods were then transferred to an oscillating reactor for ion exchange treatment for 24 h. After centrifugation, washing, and drying, the nanorods were calcined at 750°C for 100 min in an atmosphere of Ar and H2 in a volume ratio of 4:1 to obtain Cu / Fe-TiO2 (wherein the molar ratio of Cu to Fe is 1:1) containing a Cu / Fe heterogeneous phase interface.

[0034] Figure 2 TEM images of the Cu / Fe-TiO2 catalyst prepared in Example 1, wherein a and b are at different magnifications; Figure 3 The selected area electron diffraction pattern of the Cu / Fe-TiO2 catalyst prepared in Example 1; Figure 4 It is a high-magnification TEM image, where a and b are different magnifications; Figure 5 This is the HAADF mapping diagram of the Cu / Fe-TiO2 catalyst prepared in Example 1.

[0035] From the above Figure 2 to Figure 5 It can be seen from the test results in that the preparation method of the present invention can indeed construct a Cu / Fe heterogeneous phase interface and anchor it on the TiO2 surface.

[0036] Example 2

[0037] A method for preparing a nitrate conversion ammonia synthesis catalyst (Cu / Fe-TiO2 catalyst), the specific method is as follows:

[0038] (1) Preparation of Na2Ti3O7 nanorods: 2.0 g of P25 titanium dioxide was added to 300 mL of 10 M NaOH solution, and the mixture was fully dispersed by strong ultrasonication and then treated in a high pressure hydrothermal reactor at 150° C. for 10 h. The Na2Ti3O7 nanorods were then centrifuged, washed, and dried to obtain the Na2Ti3O7 nanorods for later use.

[0039] (2) Preparation of Cu / Fe-TiO2 catalyst: 50.3 g of the Na2Ti3O7 nanorods prepared in step (1) were added to 20 mL of a solution containing 1.1 mmol FeCl3·6H2O and 10 mmol CuCl2·2H2O, and the nanorods were fully dispersed by strong ultrasound. The nanorods were then transferred to an oscillating reactor for ion exchange treatment for 24 h. After centrifugation, washing, and drying, the nanorods were calcined at 850°C for 200 min in an atmosphere of Ar and H2 in a volume ratio of 4:1 to obtain Cu / Fe-TiO2 containing a Cu / Fe heterogeneous phase interface (wherein the molar ratio of Cu to Fe is 1:9).

[0040] Example 3

[0041] A method for preparing a nitrate conversion ammonia synthesis catalyst (Cu / Fe-TiO2 catalyst), the specific method is as follows:

[0042] (1) Preparation of Na2Ti3O7 nanorods: 2.0 g of P25 titanium dioxide was added to 300 mL of 10 M NaOH solution, and the mixture was fully dispersed by strong ultrasonication and then treated in a high pressure hydrothermal reactor at 150° C. for 10 h. The Na2Ti3O7 nanorods were then centrifuged, washed, and dried to obtain the Na2Ti3O7 nanorods for later use.

[0043] (2) Preparation of Cu / Fe-TiO2 catalyst: 50.3 g of the Na2Ti3O7 nanorods prepared in step (1) were added to 20 mL of a solution containing 90 mmol FeCl3·6H2O and 10 mmol CuCl2·2H2O, and the nanorods were fully dispersed by strong ultrasound. The nanorods were then transferred to an oscillating reactor for ion exchange treatment for 24 h. After centrifugation, washing, and drying, the nanorods were calcined at 750°C for 300 min in an atmosphere of Ar and H2 in a volume ratio of 4:1 to obtain Cu / Fe-TiO2 containing a Cu / Fe heterogeneous phase interface (wherein the molar ratio of Cu to Fe is 9:1).

[0044] Example 4

[0045] A Cu / Ni-TiO2 catalyst was prepared according to the method of Example 1, i.e., the FeCl3·6H2O added in step (2) of Example 1 was replaced by NiCl2, and the other conditions remained unchanged, to obtain a Cu / Ni-TiO2 catalyst (wherein the molar ratio of Cu to Ni was 1:1).

[0046] Example 5

[0047] A Cu / Pt-TiO2 catalyst was prepared according to the method of Example 1, i.e., the FeCl3·6H2O added in step (2) of Example 1 was replaced by PtCl4, and the other conditions remained unchanged, to obtain a Cu / Pt-TiO2 catalyst (wherein the molar ratio of Cu to Pt was 1:1).

[0048] Example 6

[0049] The nitrate-to-ammonia conversion catalyst (Cu / Fe-TiO2 electrocatalyst) prepared in Example 1 was used to catalyze the reaction of nitrate-to-ammonia conversion, and its catalytic efficiency was compared with that of other catalysts. The catalytic efficiency of the Cu / Fe-TiO2 electrocatalyst prepared in Example 1 was 4.68 times that of Cu-TiO2 and 2.82 times that of Fe-TiO2. At the same time, Cu / Fe-TiO2 also exhibited excellent ammonia production selectivity (90.9±0.5%) and long-term cycle stability.

[0050] Similarly, the performance of the Cu / Fe-TiO2 electrocatalysts prepared in Example 2 and Example 3 was tested, and the results were similar to those in Example 1. Compared with Cu-TiO2 and Fe-TiO2, both can improve the efficiency of nitrate conversion to synthesize ammonia, indicating that the high activity center of the catalyst prepared by the present invention originates from the Cu / Fe heterogeneous phase interface.

[0051] The nitrate-to-ammonia conversion catalyst (Cu / Ni-TiO2 electrocatalyst) prepared in Example 4 was used to catalyze the reaction of nitrate-to-ammonia conversion, and its catalytic efficiency was compared with that of other catalysts. The catalytic efficiency of the Cu / Ni-TiO2 electrocatalyst prepared in Example 2 was 3.53 times that of Cu-TiO2 and 2.21 times that of Ni-TiO2. At the same time, Cu / Fe-TiO2 also exhibited excellent ammonia production selectivity (88%) and long-term cycle stability.

[0052] The nitrate-to-ammonia conversion catalyst (Cu / Pt-TiO2 electrocatalyst) prepared in Example 5 was used to catalyze the reaction of nitrate-to-ammonia conversion, and its catalytic efficiency was compared with that of other catalysts. The catalytic efficiency of the Cu / Pt-TiO2 electrocatalyst prepared in Example 2 was 3.85 times that of Cu-TiO2 and 3.14 times that of Pt-TiO2. At the same time, Cu / Pt-TiO2 also exhibited excellent ammonia production selectivity (84%) and long-term cycle stability.

[0053] Similarly, replacing the above Fe, Ni and Pt with any one of Co, Ru or Ir can still obtain an electrocatalyst with excellent catalytic performance and stability. It can be seen that the Cu / M-TiO2 electrocatalyst (M is any one of Fe, Ni, Co, Pt, Ru or Ir) prepared by the present invention has good catalytic efficiency.

[0054] In addition, the nitrate conversion ammonia synthesis catalyst (Cu / Fe-TiO2 electrocatalyst) prepared by the present invention also exhibits excellent ammonia production selectivity (90.9±0.5%) and long-term cycle stability.

[0055] In addition, the obtained materials were subjected to NO3 - In the RR performance test, in just two hours, the nitrate nitrogen removal rate reached 93.1±1.1%, and the ammonia selectivity was as high as 90.9±0.5%, which was significantly better than most of the related reports of existing technologies. At the same time, the material also has excellent cycle stability. Then, in order to explore the source of high activity, a series of comparative experiments were carried out, and it was found that the high performance of Cu / Fe-TiO2 is likely to come from the Cu / Fe heterogeneous interface.

[0056] In view of the above conclusions, the mechanism of action of the nitrate conversion ammonia synthesis catalyst (Cu / Fe-TiO2 electrocatalyst) of the present invention is analyzed as follows:

[0057] A new adaptive site switching mechanism (protection) is proposed for the first time: the nitrate reduction process does not take place only on a single heterogeneous interface, but on NO3 - First, it is adsorbed on the Fe in the surface, and then the adsorbed NO3 - Migrate to the Cu / Fe interface to generate NO3 - Reduction, followed by the gradual transfer of adsorbed *NH3 to the Cu in the surface, which accelerates the removal of NH3 and realizes NO3 - Efficient conversion to NH3, such as Figure 6 shown.

[0058] The reaction process was further simulated using density functional theory (DFT), and the results confirmed that it was consistent with the new adaptive site switching mechanism proposed above.

[0059] In summary, the present invention discloses a catalyst for electrochemical nitrate conversion to ammonia synthesis, which is a Cu / Fe-TiO2 electrocatalyst, wherein the Cu / Fe heterogeneous phase interface is anchored on the TiO2 surface. The catalyst of the present invention has a good catalytic effect and can greatly improve the efficiency of electrochemical nitrate conversion to ammonia synthesis. In addition, the present invention also discloses a method for preparing an electrochemical nitrate conversion to ammonia synthesis catalyst, which is mainly prepared by ion exchange and high-temperature calcination. The preparation method is simple and convenient, suitable for mass preparation, and is conducive to the industrial application of the catalyst.

[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. An electrochemical nitrate conversion ammonia synthesis catalyst, characterized in that: The catalyst is a Cu / M-TiO2 electrocatalyst, in which the Cu / M heterogeneous phase interface is anchored on the TiO2 surface; Wherein M is any one of Fe, Ni, Co, Pt, Ru or Ir; The molar ratio of Cu to M is 1:9 to 9:

1.

2. The catalyst according to claim 1, characterized in that The molar ratio of Cu to TiO2 is 1:5 to 1:

50.

3. The method for preparing the electrochemical nitrate conversion ammonia synthesis catalyst according to any one of claims 1 to 2, characterized in that: The preparation method is specifically as follows: (1) Preparation of Na2Ti3O7 nanorods: titanium dioxide is added to a sodium hydroxide solution, ultrasonically dispersed to make it uniform, treated in a high pressure hydrothermal reactor at 150-180°C for more than 10 hours, centrifuged, washed, and dried to obtain Na2Ti3O7 nanorods for use; (2) Preparation of catalyst: The Na2Ti3O7 nanorods prepared in step (1) are added to a solution containing M halide and CuCl2, and are evenly dispersed by ultrasonication. The nanorods are then transferred to an oscillating reactor for ion exchange treatment for more than 24 hours. The nanorods are centrifuged, washed, and dried, and then calcined at 750-850°C for 200-300 minutes in a mixed atmosphere of argon and hydrogen to obtain a catalyst.

4. The preparation method according to claim 3, characterized in that: The mass molar ratio of the titanium dioxide to the sodium hydroxide is 2:0.3-3, g:mol.

5. The preparation method according to claim 3, characterized in that: The molar ratio of the Na2Ti3O7 nanorods to CuCl2 is 5 to 50:3; The molar ratio of M to CuCl2 in the M halide is 1:9 to 9:

1.

6. The preparation method according to claim 3, characterized in that: The volume ratio of argon to hydrogen in the mixed atmosphere is 4:1.