A fiber / hydrogel composite scaffold with stable interface and preparation method thereof
Through the combination of fibers containing polyphenol polymers on the surface and photo-crosslinkable polymer precursor solutions and ultraviolet light irradiation technology, the interface strength of fibers and hydrogels is improved, and the problem of deformation of fiber-hydrogel composites is solved. to solve the separation problem and achieve a stable fiber/hydrogel composite scaffold.
Patent Information
- Application Number
- CN202210984479.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-17
AI Technical Summary
Fiber and hydrogel composite materials are prone to phase separation during overall deformation, leading to overall failure of the scaffold. It is difficult to effectively improve the interface bonding force with existing technology.
The fiber assembly containing polyphenol polymers on the surface is combined with a photo-crosslinkable polymer precursor solution, and a hydrogel is formed through ultraviolet light irradiation. Free radicals and photoinitiators are used to promote the cross-linking reaction and improve the relationship between the fiber and the hydrogel. Interface strength and enhanced bonding force through van der Waals forces and hydrogen bonds.
The interface strength between the fiber and the hydrogel has been significantly improved, so that the fiber and the hydrogel do not separate during the overall deformation. The fiber and the hydrogel can break at the same time, solving the problem of poor interface bonding force and enhancing the strength of the composite material. mechanical properties.
Smart Images

Figure CN115531550B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fiber-reinforced hydrogel composite materials and relates to an interface-stable fiber / hydrogel composite scaffold and a preparation method thereof. Background Art
[0002] Hydrogels are currently receiving widespread attention in the biomedical field. Hydrogels have a structure similar to that of natural extracellular matrix, and have good biocompatibility and biodegradability. They are also highly functional and can be used in various fields such as drug release, medical dressings, bone repair, and soft tissue regeneration through the selection of materials and the introduction of drugs.
[0003] However, there have always been problems with the mechanical properties of hydrogels. Using natural materials to construct hydrogels meets the requirements of degradability, but the mechanical strength is insufficient. Using synthetic materials to construct hydrogels has strong mechanical properties, but is not degradable. Therefore, researchers added fibers to hydrogels to provide mechanical reinforcement for hydrogels.
[0004] Patent CN202111437537.0 uses a filtration method to embed the hydrogel into the fiber network to improve the interfacial bonding strength; Patent CN201610647658.0 uses casting and condensation to composite the interface.
[0005] However, due to the difference in mechanics between fibers and hydrogels, and the fact that fibers and hydrogels are two different materials with poor interface bonding, the two phases are easily separated during overall deformation, leading to overall failure of the scaffold. Summary of the invention
[0006] To solve the above problems, the present invention proposes an interface-stable fiber / hydrogel composite scaffold and a preparation method thereof. The scaffold is composed of fibers and hydrogels. The interface strength between the fibers and the hydrogel is large, and no phase separation occurs during overall deformation. The fibers and the hydrogel can break simultaneously rather than one after the other.
[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing an interface-stable fiber / hydrogel composite scaffold comprises adding a fiber assembly containing a polyphenol polymer on the surface into a hydrogel precursor solution and then irradiating the solution with ultraviolet light to form a hydrogel;
[0009] The hydrogel precursor solution includes a photocrosslinkable polymer precursor, a photoinitiator, a crosslinker and water, wherein the photocrosslinkable polymer precursor is a polymer that can be activated by free radicals I and II, free radicals I are generated by the polyphenol polymer under the irradiation of ultraviolet light, free radicals II are generated by the photoinitiator under the irradiation of ultraviolet light, and the crosslinker is used to connect the activated photocrosslinkable polymer precursor.
[0010] Under ultraviolet light irradiation, there are two kinds of free radicals in the system, which are recorded as free radical I and free radical II. Free radical I is provided by polyphenol polymers (after ultraviolet light is irradiated on polyphenol polymers, the aromatic ring in the polyphenol is cracked, and the phenol is oxidized to produce α, β-unsaturated aldehydes, carbon-centered free radicals, which then react with molecular oxygen to produce peroxides. These unstable intermediates can undergo single-molecule ring closure to produce bicycloalkoxy free radicals). Free radical I is concentrated around the fiber, that is, the concentration of free radical I near the fiber is higher than the concentration of free radical I at other positions. Free radical II is provided by photoinitiator, and free radical II is uniformly dispersed in the system, that is, the concentration of free radical II near the fiber is close to the concentration of free radical II at other positions, which ultimately leads to a higher free radical concentration around the fiber than at other positions. Therefore, the photocrosslinkable polymer precursor is concentrated around the fiber for crosslinking reaction, so that the degree of physical entanglement between the photocrosslinkable polymer precursor and the fiber is high, thereby improving the interface strength between the fiber and the hydrogel (mainly composed of photocrosslinkable polymer precursor and water). In addition, there are van der Waals forces (van der Waals forces are common between molecules, and are essentially the mutual attraction between charges) and hydrogen bonds (formed by polyphenol polymers and hydroxyl groups, amino groups, alkyl groups, carboxyl groups, ester groups, etc. in the hydrogel) between the hydrogel and the fiber, which can also improve the interface strength between the fiber and the hydrogel.
[0011] As the preferred technical solution:
[0012] In the method for preparing an interface-stable fiber / hydrogel composite scaffold as described above, when exposed to ultraviolet light, the hydrogel precursor solution is located in an aerobic environment (the aerobic environment is the atmospheric environment); the polyphenol polymer will produce unsaturated aldehydes, ketones or benzoquinones under the action of ultraviolet light and oxygen. When the hydrogel contains amino groups, it can produce Michael addition reactions and Schiff base reactions with the amino groups in the hydrogel to form covalent bonds, thereby further improving the interface strength between the fiber and the hydrogel.
[0013] In the method for preparing an interface-stable fiber / hydrogel composite scaffold as described above, the photo-crosslinkable polymer precursor is one or more of acrylamide and its derivatives, acrylic acid and its derivatives, gelatin derivatives, collagen derivatives, alginate derivatives, cellulose derivatives, dextran derivatives, hyaluronic acid derivatives, polyethylene glycol diacrylate and its derivatives;
[0014] The content of the photo-crosslinkable polymer precursor in each 1 mL of the hydrogel precursor solution is 10 to 400 mg;
[0015] The photoinitiator is one or more of benzoin, benzoin dimethyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, diphenyl acetone, α,α-dimethoxy-α-phenylacetophenone, α,α-diethoxyacetophenone, α-hydroxyalkyl phenone, α-aminoalkyl phenone, aromatic acyl phosphine oxide, bisbenzoylphenyl phosphine oxide, benzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, thiopropoxythioxanthone and isopropylthioxanthone;
[0016] The content of the photoinitiator in each 1 mL of the hydrogel precursor solution is 1 to 20 mg;
[0017] The cross-linking agent is one or more of N,N-methylenebisacrylamide, methacrylated gelatin, dimethyl diimide, N,N'-bisacrylcystamine, N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide;
[0018] The content of the cross-linking agent in each 1 mL of the hydrogel precursor solution is 1 to 20 mg.
[0019] In the method for preparing an interface-stable fiber / hydrogel composite scaffold as described above, the hydrogel precursor solution also includes a polymer, which is a polymer that can swell in water; when the hydrogel precursor solution contains both a photocrosslinkable polymer precursor and a polymer, the hydrogel finally formed has a double network structure and better stability. If the hydrogel precursor solution does not contain a polymer, the hydrogel finally formed has a single network structure and relatively poor stability.
[0020] As described above, the method for preparing an interface-stable fiber / hydrogel composite scaffold, the polymer is one or more of gelatin and its derivatives, collagen and its derivatives, alginate and its derivatives, cellulose and its derivatives, dextran and its derivatives, hyaluronic acid and its derivatives, polyvinyl alcohol and its derivatives; the content of the polymer in each 1 mL of hydrogel precursor solution is 5 to 300 mg.
[0021] In the method for preparing an interface-stable fiber / hydrogel composite scaffold as described above, the fiber assembly containing polyphenol polymers on the surface is prepared by immersing the fiber assembly in a polyphenol solution and shaking at 25 to 40° C. for 3 to 48 hours.
[0022] According to the method for preparing an interface-stable fiber / hydrogel composite scaffold as described above, the construction methods of the fiber assembly include but are not limited to weaving, knitting, braiding, melt-blowing, electrospinning, spunbonding, composite method, wet spinning, etc.; the thickness of the fiber assembly is 200 to 4000 microns; the polyphenol solution is an aqueous solution of polyphenol materials, the polyphenol materials are one or more of dopamine and its derivatives, tannic acid, catechol and its derivatives, and the content of polyphenol materials in each 1 mL of polyphenol solution is 0.1 to 500 mg; the bath ratio of the fiber assembly to the polyphenol material is 1:10 to 100.
[0023] In the method for preparing an interface-stable fiber / hydrogel composite scaffold as described above, the mass ratio of the fiber assembly containing polyphenol polymers on the surface to the hydrogel precursor solution is 1:5-20.
[0024] In the method for preparing the interface-stable fiber / hydrogel composite scaffold as described above, the wavelength of the ultraviolet light is 250 to 400 nm, and the irradiation time is 20 to 90 minutes.
[0025] The present invention also provides an interface-stable fiber / hydrogel composite scaffold, which is prepared by any of the preparation methods described above; the interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture.
[0026] Beneficial Effects
[0027] (1) The method for preparing an interface-stable fiber / hydrogel composite scaffold of the present invention has a simple process and a wide range of applications. It can enhance the binding ability of fiber assemblies of various materials and forms with hydrogels. The free radicals generated by the polyphenols on the fiber surface cause the hydrogel to form a tight physical entanglement around the fiber. At the same time, hydrogen bonds, covalent bonds, etc. are formed between the polyphenols on the fiber surface and the hydrogel, thereby increasing the binding force between the fiber and the hydrogel.
[0028] (2) The interface-stable fiber / hydrogel composite scaffold of the present invention has high bonding strength between the two phase interfaces, which solves the problem of easy stratification of the two phases in the fiber / hydrogel system. The fiber and hydrogel components can be made of a wide range of raw materials and can be applied in a variety of environments. It has broad prospects in the field of fiber-reinforced hydrogels. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The mechanical data diagram of the fiber being pulled out from the hydrogel in the composite scaffold of an interface-stable fiber / hydrogel composite scaffold of Examples 4, 5, 6, and 7 and the composite scaffold of Comparative Example 1;
[0030] Figure 2 This is a mechanical tensile comparison diagram of an interface-stable fiber / hydrogel composite scaffold of Example 4 and a composite scaffold of Comparative Example 1;
[0031] Figure 3 This is a bending diagram of an interface-stable fiber / hydrogel composite scaffold of Example 4. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0033] In the following embodiments and comparative examples, the fiber assembly used to prepare the composite scaffold is in a naturally straight state, without folding or curling. The length of the fiber assembly is 3 cm and the width is 4 mm. A partial length segment of the fiber assembly is exposed from the hydrogel precursor solution, and the length of the length segment is 1.5 cm. The prepared composite scaffold has a cubic structure as a whole, with a width of 5 mm, a thickness of 5 mm and a length of 3 cm. The length of the fiber assembly is parallel to the length of the cube. When testing the force of pulling the fiber out of the hydrogel, the upper and lower clamps of the stretching clamp respectively clamp the hydrogel and the fiber assembly, and stretch it at a speed of 100 mm / min to pull the fiber assembly out of the hydrogel.
[0034] In the following embodiments and comparative examples, the testing method of breaking strain is as follows: the sample is cut into a cubic structure, the width of the cube is 5 mm, the length is 5 cm, and the thickness is not limited (it can wrap the fiber assembly, and the test shows that the thickness of the hydrogel will not affect the breaking strain). Use a clamp to clamp the upper and lower ends of the sample with a clamping distance of 3 cm, and stretch the sample at a speed of 200 mm / min until it breaks.
[0035] Example 1
[0036] A method for preparing a fiber assembly, the specific process is as follows:
[0037] The weaving raw material is polyethylene terephthalate yarn, the yarn linear density is 100 denier, the woven fabric is prepared with a 1 / 1 plain weave structure, the warp density and weft density are 200 threads / cm, and the product thickness is 0.6 mm.
[0038] Example 2
[0039] A method for preparing a fiber assembly, the specific process is as follows:
[0040] The knitting raw material is polypropylene yarn with a yarn density of 50 denier. The knitted mesh is prepared with a closed warp flat structure. The padding yarn number is GB: 1-0 / 1-2 / / , the transverse density is 10wpc, the longitudinal density is 15cpc, and the product thickness is 0.5 mm.
[0041] Example 3
[0042] A method for preparing a fiber assembly, the specific process is as follows:
[0043] The electrospinning raw material was polycaprolactone (Aladdin, P299384) particles, which were dissolved in chloroform at a concentration of 0.12 g / ml. A 19G needle was used, the injection speed was 1.2 ml / h, the spinning was carried out at a voltage of 20 kV, the receiving distance was 15 cm, the drum speed was 30 rpm, and the product thickness was 0.2 mm.
[0044] Example 4
[0045] A method for preparing an interface-stable fiber / hydrogel composite scaffold, the specific steps are as follows:
[0046] (1) Preparation of raw materials:
[0047] The fiber assembly containing polyphenol polymer on the surface is prepared by: immersing the fiber assembly of Example 1 in an aqueous solution of polyphenol material at a bath ratio of 1:10 and shaking at 25° C. for 48 hours; the polyphenol material is dopamine (Merrill, M62581), and the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material is 5 mg;
[0048] The hydrogel precursor solution is composed of a photo-crosslinkable polymer precursor, a photoinitiator, a crosslinking agent, a high molecular weight polymer and water;
[0049] The photo-crosslinkable polymer precursor is acrylamide (Aladdin, A108470); the content of the photo-crosslinkable polymer precursor in each 1 mL of the hydrogel precursor solution is 300 mg;
[0050] The photoinitiator is benzoin (sigma, B8681); the content of the photoinitiator in each 1 mL of the hydrogel precursor solution is 3 mg;
[0051] The cross-linking agent is N,N-methylenebisacrylamide (Ron's reagent, R013208); the content of the cross-linking agent in each 1 mL of the hydrogel precursor solution is 5 mg;
[0052] The high molecular polymer is gelatin (McLean, G821281); the content of the high molecular polymer in each 1 mL of the hydrogel precursor solution is 100 mg;
[0053] (2) After adding the fiber assembly containing polyphenol polymers on the surface into the hydrogel precursor solution, the fiber assembly is irradiated with ultraviolet light with a wavelength of 250 nm for 90 minutes in an aerobic environment to form a hydrogel; the mass ratio of the fiber assembly containing polyphenol polymers on the surface to the hydrogel precursor solution is 1:5.
[0054] The resulting interface-stable fiber / hydrogel composite scaffold did not delaminate when stretched to fracture, with a fracture strain of 200%. Figure 3 As shown, the final interface-stable fiber / hydrogel composite scaffold does not delaminate even when bent significantly.
[0055] Comparative Example 1
[0056] A method for preparing a composite scaffold is basically the same as that of Example 4, except that in the preparation of raw materials in step (1), the fiber aggregate prepared is not a fiber aggregate containing polyphenol polymers on the surface, but an untreated fiber aggregate.
[0057] The fracture strain of the composite scaffold finally obtained is 200%. Figure 2 Shown is a mechanical stretching comparison diagram of an interface-stable fiber / hydrogel composite scaffold of Example 4 and the composite scaffold of Comparative Example 1. The stretching curve of Comparative Example 2 fluctuates, indicating that the fiber and the hydrogel are broken separately, and the curve of Example 4 is smooth, indicating that the fiber and the hydrogel are broken. It can be seen that the composite scaffold of Comparative Example 1 is stratified during the stretching process.
[0058] Example 5
[0059] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as that of Example 4, except that the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material in step (1) of Example 5 is 9 mg.
[0060] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0061] Example 6
[0062] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as that of Example 4, except that the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material in step (1) of Example 6 is 11 mg.
[0063] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0064] Example 7
[0065] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as that of Example 4, except that the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material in step (1) of Example 7 is 13 mg.
[0066] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0067] like Figure 1 As shown, it is a mechanical data diagram of the fiber pulled out from the hydrogel in Comparative Example 1 and Examples 4, 5, 6, and 7, and the magnitudes of the forces are 2.2N, 5.9N, 6.6N, 6.7N, and 6.5N, respectively. It can be seen from the figure that the introduction of polyphenol materials into the fiber material can enhance the binding force between the fiber and the hydrogel. As the concentration of the polyphenol materials increases, the binding force between the fiber and the hydrogel is enhanced. The increase in the binding force caused by the polyphenol materials has a maximum value. When the maximum value is reached, the increase in concentration will not lead to a further increase in the binding force. This is because the free radicals required for the formation of the hydrogel have a maximum value. Therefore, it can be concluded that the introduction of the polyphenol materials leads to an increase in the binding force between the fiber and the hydrogel.
[0068] Example 8
[0069] A method for preparing an interface-stable fiber / hydrogel composite scaffold, the specific steps are as follows:
[0070] (1) Preparation of raw materials:
[0071] The fiber assembly containing polyphenol polymer on the surface is prepared by: immersing the fiber assembly of Example 2 in an aqueous solution of polyphenol material at a bath ratio of 1:20 and shaking at 27° C. for 40 hours; the polyphenol material is a dopamine derivative (sigma, H8502), and the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material is 15 mg;
[0072] The hydrogel precursor solution is composed of a photo-crosslinkable polymer precursor, a photoinitiator, a crosslinking agent, a high molecular weight polymer and water;
[0073] The photo-crosslinkable polymer precursor is an acrylamide derivative (sigma, 109606); the content of the photo-crosslinkable polymer precursor in each 1 mL of the hydrogel precursor solution is 250 mg;
[0074] The photoinitiator is benzoin dimethyl ether (Jiuding Chemical, BE337); the content of the photoinitiator in each 1 mL of the hydrogel precursor solution is 4 mg;
[0075] The cross-linking agent is methacrylated gelatin (source leaf, S29881); the content of the cross-linking agent in each 1 mL of the hydrogel precursor solution is 10 mg;
[0076] The high molecular polymer is a gelatin derivative (Aladdin, M398240); the content of the high molecular polymer in each 1 mL of the hydrogel precursor solution is 120 mg;
[0077] (2) After adding the fiber assembly containing polyphenol polymers on the surface into the hydrogel precursor solution, the fiber assembly is irradiated with ultraviolet light with a wavelength of 260 nm for 80 minutes in an aerobic environment to form a hydrogel; the mass ratio of the fiber assembly containing polyphenol polymers on the surface to the hydrogel precursor solution is 1:7.
[0078] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 300%.
[0079] Example 9
[0080] A method for preparing an interface-stable fiber / hydrogel composite scaffold, the specific steps are as follows:
[0081] (1) Preparation of raw materials:
[0082] The fiber assembly containing polyphenol polymer on the surface is prepared by: immersing the fiber assembly of Example 3 in an aqueous solution of polyphenol material at a bath ratio of 1:40 and shaking at 30° C. for 32 hours; the polyphenol material is dopamine (Merrill, M62581), and the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material is 100 mg;
[0083] The hydrogel precursor solution is composed of a photo-crosslinkable polymer precursor, a photoinitiator, a crosslinking agent, a high molecular weight polymer and water;
[0084] The photo-crosslinkable polymer precursor is acrylic acid (Aladdin, A103526); the content of the photo-crosslinkable polymer precursor in each 1 mL of the hydrogel precursor solution is 380 mg;
[0085] The photoinitiator is benzoin ethyl ether (McLean, B824728); the content of the photoinitiator in each 1 mL of the hydrogel precursor solution is 5 mg;
[0086] The cross-linking agent was dimethyl diimide (Henan Weitixi Chemical Technology Co., Ltd., ALFA-); the content of the cross-linking agent in each 1 mL of the hydrogel precursor solution was 5 mg;
[0087] The high molecular polymer is alginate (Aladdin, A110570); the content of the high molecular polymer in each 1 mL of the hydrogel precursor solution is 50 mg;
[0088] (2) After adding the fiber assembly containing polyphenol polymers on the surface into the hydrogel precursor solution, the fiber assembly is irradiated with ultraviolet light with a wavelength of 270 nm for 70 minutes in an aerobic environment to form a hydrogel; the mass ratio of the fiber assembly containing polyphenol polymers on the surface to the hydrogel precursor solution is 1:10.
[0089] The finally obtained interface-stable fiber / hydrogel composite scaffold did not delaminate when stretched to fracture, and the fracture strain was 250%.
[0090] Example 10
[0091] A method for preparing an interface-stable fiber / hydrogel composite scaffold, the specific steps are as follows:
[0092] (1) Preparation of raw materials:
[0093] The fiber assembly containing polyphenol polymer on the surface is prepared by: immersing the fiber assembly of Example 1 in an aqueous solution of polyphenol material at a bath ratio of 1:50 and shaking at 32° C. for 24 hours; the polyphenol material is tannic acid (Ron's reagent, R071388), and the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material is 130 mg;
[0094] The hydrogel precursor solution is composed of a photo-crosslinkable polymer precursor, a photoinitiator, a crosslinking agent, a high molecular weight polymer and water;
[0095] The photo-crosslinkable polymer precursor is an acrylic acid derivative (sigma, 155721); the content of the photo-crosslinkable polymer precursor in each 1 mL of the hydrogel precursor solution is 280 mg;
[0096] The photoinitiator is benzoin isopropyl ether (Ron's reagent, R052702); the content of the photoinitiator in each 1 mL of the hydrogel precursor solution is 5 mg;
[0097] The cross-linking agent is N,N'-bisacrylcystamine (Jiuding Chemical, B-AX257); the content of the cross-linking agent in each 1 mL of the hydrogel precursor solution is 8 mg;
[0098] The high molecular polymer is an alginate derivative (Aladdin, M303578); the content of the high molecular polymer in each 1 mL of the hydrogel precursor solution is 45 mg;
[0099] (2) After adding the fiber aggregate containing polyphenol polymers on the surface into the hydrogel precursor solution, the fiber aggregate is irradiated with ultraviolet light with a wavelength of 300 nm for 60 minutes in an aerobic environment to form a hydrogel; the mass ratio of the fiber aggregate containing polyphenol polymers on the surface to the hydrogel precursor solution is 1:12.
[0100] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 300%.
[0101] Embodiment 11
[0102] A method for preparing an interface-stable fiber / hydrogel composite scaffold, the specific steps are as follows:
[0103] (1) Preparation of raw materials:
[0104] The fiber assembly containing polyphenol polymer on the surface is prepared by: immersing the fiber assembly of Example 2 in an aqueous solution of polyphenol material at a bath ratio of 1:60 and shaking at 35° C. for 18 hours; the polyphenol material is catechol (sigma, PHL82372), and the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material is 200 mg;
[0105] The hydrogel precursor solution is composed of a photo-crosslinkable polymer precursor, a photoinitiator, a crosslinking agent, a high molecular weight polymer and water;
[0106] The photo-crosslinkable polymer precursor is an alginate derivative (Shenzhen Huanuo Biotechnology Co., Ltd. HN-ALM-RGD); the content of the photo-crosslinkable polymer precursor in each 1 mL of the hydrogel precursor solution is 100 mg;
[0107] The photoinitiator is benzoin butyl ether (Huaxia Chemical, 11755); the content of the photoinitiator in each 1 mL of the hydrogel precursor solution is 10 mg;
[0108] The cross-linking agent is N,N'-dicyclohexylcarbodiimide (Jiuding Chemical, N001R); the content of the cross-linking agent in each 1 mL of the hydrogel precursor solution is 7 mg;
[0109] The high molecular polymer is cellulose (Aladdin, C104844); the content of the high molecular polymer in each 1 mL of the hydrogel precursor solution is 120 mg;
[0110] (2) After adding the fiber aggregate containing polyphenol polymers on the surface into the hydrogel precursor solution, the fiber aggregate is irradiated with ultraviolet light of a wavelength of 330 nm for 40 minutes in an aerobic environment to form a hydrogel; the mass ratio of the fiber aggregate containing polyphenol polymers on the surface to the hydrogel precursor solution is 1:15.
[0111] The finally obtained interface-stable fiber / hydrogel composite scaffold did not delaminate when stretched to fracture, and the fracture strain was 250%.
[0112] Example 12
[0113] A method for preparing an interface-stable fiber / hydrogel composite scaffold, the specific steps are as follows:
[0114] (1) Preparation of raw materials:
[0115] The fiber assembly containing polyphenol polymer on the surface is prepared by: immersing the fiber assembly of Example 3 in an aqueous solution of polyphenol material at a bath ratio of 1:80 and shaking at 37° C. for 10 hours; the polyphenol material is tannic acid (Ron's reagent, R071388), and the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material is 50 mg;
[0116] The hydrogel precursor solution is composed of a photo-crosslinkable polymer precursor, a photoinitiator, a crosslinking agent, a high molecular weight polymer and water;
[0117] The photo-crosslinkable polymer precursor is a gelatin derivative (Sigma, 900629); the content of the photo-crosslinkable polymer precursor in each 1 mL of the hydrogel precursor solution is 200 mg;
[0118] The photoinitiator is diphenylacetophenone (Jiuding Chemical, PI570); the content of the photoinitiator in each 1 mL of the hydrogel precursor solution is 12 mg;
[0119] The cross-linking agent is N,N'-diisopropylcarbodiimide (Jiuding Chemical, N005A); the content of the cross-linking agent in each 1 mL of the hydrogel precursor solution is 15 mg;
[0120] The high molecular polymer is a cellulose derivative (Aladdin, C104844); the content of the high molecular polymer in each 1 mL of the hydrogel precursor solution is 65 mg;
[0121] (2) After adding the fiber assembly containing polyphenol polymers on the surface into the hydrogel precursor solution, the fiber assembly is irradiated with ultraviolet light of a wavelength of 360 nm for 30 minutes in an aerobic environment to form a hydrogel; the mass ratio of the fiber assembly containing polyphenol polymers on the surface to the hydrogel precursor solution is 1:17.
[0122] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0123] Embodiment 13
[0124] A method for preparing an interface-stable fiber / hydrogel composite scaffold, the specific steps are as follows:
[0125] (1) Preparation of raw materials:
[0126] The fiber assembly containing polyphenol polymer on the surface is prepared as follows: according to a bath ratio of 1:100, the fiber assembly of Example 3 is immersed in an aqueous solution of a polyphenol material and shaken at 40° C. for 3 hours; the polyphenol material is a catechol derivative (sigma, M13203), and the content of the polyphenol material in each 1 mL of the aqueous solution of the polyphenol material is 70 mg;
[0127] The hydrogel precursor solution is composed of a photo-crosslinkable polymer precursor, a photoinitiator, a crosslinking agent, a high molecular weight polymer and water;
[0128] The photo-crosslinkable polymer precursor is a collagen derivative (Xi'an Qiyue Biotechnology Co., Ltd., ColMA Kit); the content of the photo-crosslinkable polymer precursor in each 1 mL of the hydrogel precursor solution is 50 mg;
[0129] The photoinitiator is α,α-dimethoxy-α-phenylacetophenone (source leaf, S45044); the content of the photoinitiator in each 1 mL of the hydrogel precursor solution is 15 mg;
[0130] The cross-linking agent is 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride (Aladdin, E106172); the content of the cross-linking agent in each 1 mL of the hydrogel precursor solution is 11 mg;
[0131] The high molecular weight polymer is dextran (Aladdin, D400777); the content of the high molecular weight polymer in each 1 mL of the hydrogel precursor solution is 50 mg;
[0132] (2) After adding the fiber assembly containing polyphenol polymers on the surface into the hydrogel precursor solution, the fiber assembly is irradiated with ultraviolet light with a wavelength of 400 nm for 20 minutes in an aerobic environment to form a hydrogel; the mass ratio of the fiber assembly containing polyphenol polymers on the surface to the hydrogel precursor solution is 1:20.
[0133] The resulting interface-stable fiber / hydrogel composite scaffold did not delaminate when stretched to fracture, with a fracture strain of 220%.
[0134] Embodiment 14
[0135] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as that of Example 4, except that the hydrogel precursor solution of Example 14 does not contain a high molecular weight polymer.
[0136] The resulting interface-stable fiber / hydrogel composite scaffold did not delaminate when stretched to fracture, with a fracture strain of 180%.
[0137] Embodiment 15
[0138] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the ultraviolet light irradiation in Example 15 is performed in an oxygen-free environment.
[0139] The resulting interface-stable fiber / hydrogel composite scaffold did not delaminate when stretched to fracture, 5.5 N was required to pull the fiber out of the hydrogel, and the fracture strain of the composite scaffold was 200%.
[0140] Compared with Example 4, the pull-out force of the fiber in Example 15 from the hydrogel is much smaller than that in Example 4. This is because the ultraviolet light irradiation in Example 4 is carried out in an aerobic environment, and dopamine (Merrel, M62581) will produce unsaturated aldehydes, ketones or benzoquinones under the action of ultraviolet light and oxygen, which will produce Michael addition reactions and Schiff base reactions with the amino groups in the hydrogel to form covalent bonds, further improving the interface strength between the fiber and the hydrogel.
[0141] Example 16
[0142] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photoinitiator is α,α-diethoxyacetophenone (Sigma, 227102), the cross-linking agent is N-hydroxysuccinimide (Aladdin, H109330), and the high molecular weight polymer is a dextran derivative (Sigma, 86524).
[0143] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0144] Embodiment 17
[0145] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photoinitiator is α-hydroxyalkyl phenone (Sigma, 405655), the crosslinker is a mixture of N,N-methylenebisacrylamide (Sigma, 1108970050) and methacrylated gelatin (Source Leaf, S29881) in a mass ratio of 1:1, and the high molecular weight polymer is hyaluronic acid (McLean H909938).
[0146] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0147] Embodiment 18
[0148] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photoinitiator is α-aminoalkylphenone (Sigma, 405639) and the high molecular polymer is a hyaluronic acid derivative (Aladdin A293527).
[0149] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0150] Embodiment 19
[0151] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photocrosslinkable polymer precursor is a cellulose derivative (Xi'an Qiyue Biotechnology Co., Ltd., CMC-g-AE), the photoinitiator is an aromatic acylphosphine oxide (Sigma, 415952), and the high molecular polymer is polyvinyl alcohol (McLean, P816862).
[0152] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0153] Embodiment 20
[0154] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photoinitiator is bisbenzoylphenylphosphine oxide (Sigma, 511447) and the high molecular polymer is a polyvinyl alcohol derivative (Sigma, P110010).
[0155] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0156] Embodiment 21
[0157] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photoinitiator is benzophenone (sigma, B9300) and the high molecular polymer is collagen (sigma, C9791).
[0158] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0159] Embodiment 22
[0160] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photocrosslinkable polymer precursor is a dextran derivative, the photoinitiator is 2,4-dihydroxybenzophenone (Aladdin, D110121), and the high molecular polymer is a collagen derivative (Sigma, C4361);
[0161] The preparation steps of the dextran derivatives are as follows:
[0162] (1) Dissolve dextran in 90 ml of dimethyl sulfoxide (sigma, D2650) to form solution I with a glucose concentration of 0.11 g / ml;
[0163] (2) adding glycidyl methacrylate (sigma, 151238) and 4-(N,N-dimethylamino)pyridine (sigma, 107700) to solution I to form solution II; wherein the concentration of glycidyl methacrylate in solution II is 0.016 g / ml, and the concentration of 4-(N,N-dimethylamino)pyridine in solution II is 0.02 g / ml;
[0164] (3) stirring solution II at 30° C. for 30 hours to obtain a reaction solution;
[0165] (4) The reaction solution of step (3) was added dropwise to 400 ml of anhydrous ethanol (Sigma, 1070172511), allowed to stand and filtered to obtain a white precipitate;
[0166] (5) The white precipitate was dissolved in distilled water, the pH was adjusted to 7, dialyzed in deionized water at 4° C. for 4 days, and freeze-dried to obtain a dextran derivative.
[0167] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0168] Embodiment 23
[0169] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photoinitiator is Michler's ketone (Source Leaf, S19213).
[0170] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0171] Embodiment 24
[0172] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photocrosslinkable polymer precursor is a hyaluronic acid derivative (Shanghai Zhenzhun Biotechnology Co., Ltd., ZCR-HA-301) and the photoinitiator is thiopropoxythioxanthone (B&K Technology, 513069).
[0173] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0174] Embodiment 25
[0175] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photocrosslinkable polymer precursor is polyethylene glycol diacrylate (Source Leaf, S28835) and the photoinitiator is isopropylthioxanthone (Sigma, 34222).
[0176] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
[0177] Embodiment 26
[0178] A method for preparing an interface-stable fiber / hydrogel composite scaffold is basically the same as Example 4, except that the photocrosslinkable polymer precursor is a polyethylene glycol diacrylate derivative (Sigma, 463183), and the photoinitiator is a mixture of Michler's ketone (Source Leaf, S19213) and isopropylthioxanthone (Sigma, 34222) in a mass ratio of 1:1.
[0179] The finally obtained interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture, and the fracture strain is 200%.
Claims
1. A method for preparing an interface-stable fiber / hydrogel composite scaffold, characterized in that: Adding a fiber assembly containing polyphenol polymers on the surface into a hydrogel precursor solution and irradiating the solution with ultraviolet light until a hydrogel is formed; The preparation process of the fiber assembly containing polyphenol polymer on the surface is as follows: immersing the fiber assembly in a polyphenol solution and shaking at 25-40° C. for 3-48 hours, wherein the polyphenol solution is an aqueous solution of a polyphenol material, and the polyphenol material is one or more of dopamine and its derivatives, tannic acid, catechol and its derivatives; The hydrogel precursor solution comprises a photo-crosslinkable polymer precursor, a photoinitiator, a crosslinking agent, a high molecular weight polymer and water; The photo-crosslinkable polymer precursor is one or more of acrylamide and its derivatives, acrylic acid and its derivatives; The photoinitiator is one or more of benzoin, benzoin dimethyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, diphenyl acetone, α,α-dimethoxy-α-phenylacetophenone, α,α-diethoxyacetophenone, α-hydroxyalkyl phenone, α-aminoalkyl phenone, aromatic acyl phosphine oxide, bisbenzoylphenyl phosphine oxide, benzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, thiopropoxythioxanthone and isopropylthioxanthone; The cross-linking agent is one or more of N,N-methylenebisacrylamide, N,N'-bisacrylcystamine, N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide; The cross-linking agent is used to connect the activated photo-cross-linkable polymer precursor; The high molecular weight polymer is one or more of gelatin and its derivatives, collagen and its derivatives.
2. The method for preparing an interface-stable fiber / hydrogel composite scaffold according to claim 1, characterized in that: When irradiated with ultraviolet light, the hydrogel precursor solution is in an oxygen environment.
3. The method for preparing an interface-stable fiber / hydrogel composite scaffold according to claim 1, characterized in that: The content of the photo-crosslinkable polymer precursor in each 1 mL of the hydrogel precursor solution is 10-400 mg; the content of the photoinitiator in each 1 mL of the hydrogel precursor solution is 1-20 mg; and the content of the crosslinking agent in each 1 mL of the hydrogel precursor solution is 1-20 mg.
4. The method for preparing an interface-stable fiber / hydrogel composite scaffold according to claim 1, characterized in that: The content of the high molecular weight polymer in each 1 mL of the hydrogel precursor solution is 5-300 mg.
5. The method for preparing an interface-stable fiber / hydrogel composite scaffold according to claim 4, characterized in that: The thickness of the fiber assembly is 200-4000 microns; the content of the polyphenol material in each 1 mL of the polyphenol solution is 0.1-500 mg; and the bath ratio of the fiber assembly to the polyphenol material is 1:10-100.
6. The method for preparing an interface-stable fiber / hydrogel composite scaffold according to claim 1, characterized in that: The mass ratio of the fiber assembly containing polyphenol polymers on the surface to the hydrogel precursor solution is 1:5~20.
7. The method for preparing an interface-stable fiber / hydrogel composite scaffold according to claim 1, characterized in that: The wavelength of ultraviolet light is 250~400nm, and the irradiation time is 20~90 minutes.
8. An interface-stable fiber / hydrogel composite scaffold, characterized in that: The fiber / hydrogel composite scaffold is prepared by the preparation method according to any one of claims 1 to 7; the interface-stable fiber / hydrogel composite scaffold does not delaminate when stretched to fracture.
Citation Information
Patent Citations
Double-layer composite hydrogel for repairing bone and cartilage tissues as well as preparation method and application of double-layer composite hydrogel
CN106267357A
Hydrogel / nanofiber bionic double-layer dressing and preparation method thereof
CN114191599A
Amorphous silver-containing long-acting antibacterial hydrogel dressing with photo-crosslinking curing function and preparation method thereof
CN113980185A
Aramid nanofiber strengthening and toughening hydrogel and preparation method thereof
CN114437372A