Casting method of large ductile iron castings

Through the splicing structure of the main core and auxiliary core bones and the crowbar lever molding technology, the exhaust difficulties and molding impact problems in casting of large ductile iron parts are solved, and higher quality castings and longer core boxes are achieved Service life.

CN115533042BActive Publication Date: 2024-11-19ZHEJIANG OUYEDA MACHINE MFG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211290813.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-21
Publication Date
2024-11-19
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

During the casting process, large ductile iron parts have difficulties in exhaust gas and the molding method affects the quality of the sand core forming, resulting in the casting being prone to pore defects and inconsolidation of mass.

Method used

The splicing structure of the main core bone and the auxiliary core bone is adopted to achieve smooth exhaust through the multi-point exhaust pipe and airflow channel, and the lever principle of crowbar and core box is used to stabilize the mold starting, reducing the amount of sand used and improving the strength of the sand core.

Benefits of technology

It effectively reduces the incidence of defects such as air pores, shrinkage, shrinkage and slag inclusion, improves the quality density and uniformity of the castings, extends the service life of the core box, and improves the yield rate of the sand core.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115533042B_ABST
    Figure CN115533042B_ABST
Patent Text Reader

Abstract

The invention discloses a casting method for a large ductile iron casting, comprising the following steps: firstly placing a sand layer at the bottom of a core box, then splicing a main core bone and a secondary core bone according to the shape of a mold, winding an exhaust rope on the main core bone, then placing the spliced ​​main core bone and secondary core bone into the sand layer, and finally filling in molding sand for compaction; pressing an upper die downward on the molding sand in the core box, knocking the upper die from top to bottom, knocking the core box from outside to inside, pressing out the required sand core shape, and removing the air in the molding sand; after the sand core is hardened, opening the core box by using a lever principle with a crowbar, and taking out the sand core; placing the sand core in the mold cavity of a sand box, punching an exhaust hole on the box cover, first filling the base sand in the chamber between the mold cavity and the inner wall of the sand box to make it flat, then placing the secondary core bone, and finally filling the molding sand in the chamber; pouring; opening the box to drop the sand, and reusing the main core bone and the secondary core bone. The invention has the characteristics of being easy to exhaust, improving the demolding form, and improving the quality of finished castings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a casting method for an iron piece, in particular to a casting method for a large ductile iron piece. Background Art

[0002] Casting is an important manufacturing method in basic industries. Large and medium-sized iron castings are generally cast using the resin sand process. Currently, castings produced using the sand casting process account for more than 80% of the total casting output.

[0003] For some large and complex structures, such as cylinders, injection molding machines and other cast iron parts, the sand core structure is complex. When the molten iron is poured into the mold cavity, the sand mold and sand core are heated by the heat of the molten metal, and the resin sand is heated to produce a large amount of gas. The sand core is covered by molten iron or aluminum, and the contact area between the sand core and the outside world is small or non-connected. The large amount of gas generated by the sand core when heated cannot be completely discharged by the core head and sand mold alone. The gas that cannot be discharged enters the molten iron or aluminum, which will form a porosity defect in the casting, resulting in the scrapping of the casting. The simple exhaust rope and exhaust hole design currently used are often limited by the complex sand mold and cannot be used. For example, the sand core covered by molten metal cannot use this method. In addition, due to the influence of the strength and structure of the sand mold, the weight of a single piece ranges from hundreds of kilograms to tens of tons, which is not easy to operate, resulting in difficulty in exhaust, resulting in shrinkage, shrinkage, slag inclusions, porosity and other defects, and it is difficult to ensure the quality density and uniformity requirements of complex thin-walled cast iron parts.

[0004] Moreover, the sand cores of large castings are heavy, and are generally lifted to remove the cores from the mold. However, since the core box is a left-right structure, the lifting direction is inconsistent with the demolding direction. In order to ensure sequential demolding, the core box is generally turned over and stood up as a whole, and then lifted. The sand core is directly pressed on the core box, which can easily damage the core box and also affect the molding quality of the sand core.

[0005] Therefore, when the existing large ductile iron castings are core-made and molded, there are problems such as difficulty in exhausting and the mold-release method affecting the molding quality of the sand core. Summary of the invention

[0006] The purpose of the present invention is to provide a casting method for large ductile iron castings, which is characterized by convenient exhaust, improved demoulding form and improved quality of finished castings.

[0007] The technical solution of the present invention: A casting method for large ductile iron castings comprises the following steps: S1, core making:

[0008] a. First put a sand layer at the bottom of the core box, then splice the main core bone and the auxiliary core bone according to the shape of the mold, wrap the exhaust rope around the main core bone, then put the spliced ​​main core bone and auxiliary core bone into the sand layer, and finally fill in the molding sand for compaction;

[0009] b. Press the upper die down on the molding sand in the core box, knock the upper die from top to bottom, knock the core box from outside to inside, press out the required sand core shape, and remove the air in the molding sand;

[0010] c. After the sand core is hardened, use a crowbar to open the core box using the lever principle and take out the sand core;

[0011] S2. Molding: Place the sand core in the mold cavity of the sand box, pierce the exhaust hole on the box cover, first fill the cavity between the mold cavity and the inner wall of the sand box with base sand to make it flat, then put in the secondary core bone, and finally fill the cavity with molding sand;

[0012] S3, pouring;

[0013] S4. Unpack and remove sand, and reuse the main core bone and auxiliary core bone.

[0014] In the aforementioned casting method of large ductile iron castings, the main core bone is composed of multiple transverse ribs and longitudinal ribs connected together, a support rod is provided at the bottom of the main core bone, and the support rod is a conical structure with a larger top and a smaller bottom, and a first cross-shaped opening is provided at both ends and sides of the transverse ribs and longitudinal ribs.

[0015] In the aforementioned casting method of large ductile iron castings, a cross-shaped inner cavity is provided inside the auxiliary core bone, and a first cover and a second cover for sealing the cross-shaped inner cavity are respectively provided at both ends of the auxiliary core bone, a cross-shaped protrusion is provided on the first cover, and the second cover is provided with a second cross-shaped opening connected to the cross-shaped inner cavity.

[0016] In the aforementioned casting method of large ductile iron castings, the bottom of the secondary core bone is provided with an elongated groove connected to the cross-shaped inner cavity, a plurality of counterweight blocks are provided in the cross-shaped inner cavity, and the bottom of the counterweight block is provided with a sliding block extending out of the elongated groove.

[0017] In the aforementioned casting method of large ductile iron castings, the interior of the main core bone is provided with mutually connected air flow channels, the side of the main core bone is provided with a first microhole connected to the air flow channel, and the top of the main core bone is provided with a main exhaust pipe connected to the air flow channel; the side of the auxiliary core bone is provided with a second microhole connected to the cross-shaped inner cavity, and the top of the auxiliary core bone is provided with an auxiliary exhaust pipe connected to the cross-shaped inner cavity.

[0018] In the aforementioned casting method for large ductile iron castings, the molding sand comprises the following materials in parts by weight: 100 parts of silica sand, 0.8-1 parts of resin and 0.4-0.5 parts of curing agent, and the water content of the molding sand is less than 0.15%.

[0019] In the aforementioned casting method of large ductile iron castings, after the sand core is taken out, a coating is brushed on the surface of the sand core and on the inner wall of the sand box. The coating includes zircon powder coating and alcohol-based coating in a mass ratio of 1:1, and the coating ratio has a Baume degree of 28-35°Bé.

[0020] In the aforementioned casting method of large ductile iron castings, the core box includes a base plate, a left core box and a right core box. The left core box and the right core box are movably connected on the base plate. A force plate is provided on the side of the base plate. A plurality of positioning holes are provided on the force plate. A hanging handle with a T-shaped cross-section is provided on the side of the left core box and the right core box close to the base plate.

[0021] In the aforementioned casting method of large ductile iron castings, the inner diameter of the positioning hole is larger than the diameter of the crowbar, and a plurality of protrusions are provided on the inner wall of the positioning hole.

[0022] In the aforementioned casting method of large ductile iron castings, the bottom of the load-bearing plate is fixed to the base plate by a plurality of triangular ribs.

[0023] Compared with the prior art, the present invention can splice the main core bone and the auxiliary core bone according to the different required sand core shapes during the core making process, and put the main core bone and the auxiliary core bone that match the shape into the sand core, so that the structural strength of the whole sand core is evenly improved to avoid the occurrence of local tilting and cracking; at the same time, cavities and exhaust pipes are arranged in the main core bone and the auxiliary core bone, and the sand core is evenly vented at multiple points, the exhaust is smoother, and the probability of shrinkage holes, shrinkage, slag inclusions, air holes and other defects is reduced, so as to ensure the quality density and uniformity requirements of complex thin-walled iron castings. Moreover, the main core bone and the auxiliary core bone can replace a part of the molding sand in the core box or sand box, thereby reducing the amount of molding sand, and the main core bone and the auxiliary core bone can be reused;

[0024] Furthermore, the counterweight blocks can be added or removed in the secondary core frame as needed, thereby improving the strength and optimizing the weight, thereby providing a better alternative to molding sand.

[0025] A stress plate with stress holes is arranged at the bottom of the core box. When demoulding, the lower end of the crowbar is inserted into the positioning hole, one side of the crowbar is engaged with the hanging handle on the left core box or the right core box, and pressure is applied to the upper end of the crowbar. The left core box and the right core box are stably moved to both sides by utilizing the lever principle, so that the core box is opened and the sand core is taken out. The operation is flexible and convenient, with little damage to the core box, the service life is extended, and the quality of the sand core is improved. The yield rate of the sand core is as high as 99%.

[0026] Furthermore, under the premise that the sand mold and sand core reach the required strength, the molding sand used contains relatively less resin and curing agent and has a low water content, which can effectively reduce the gas generated by these substances at high temperatures and reduce the amount of gas evolution, thereby reducing quality defects such as shrinkage cavities, shrinkage, slag inclusions, and air holes. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of the structure of the main core bone;

[0028] Figure 2 It is a schematic diagram of the structure of the accessory core bone;

[0029] Figure 3 It is a cross-sectional view of the paracore bone;

[0030] Figure 4 It is a schematic diagram of the opening structure of the core box.

[0031] The markings in the attached drawings are: 1. main core bone; 11. transverse ribs; 12. longitudinal ribs; 13. first microhole; 14. first cross-shaped opening; 15. main exhaust pipe; 16. support rod; 2. auxiliary core bone; 21. cross-shaped inner cavity; 211. second microhole; 22. first cover; 23. second cover; 24. cross-shaped protrusion; 25. long groove; 26. counterweight; 27. slider; 28. auxiliary exhaust pipe; 3. core box; 31. crowbar; 32. bottom plate; 33. left core box; 34. right core box; 35. force plate; 36. positioning hole; 37. hanging handle; 38. triangular rib. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.

[0033] Example:

[0034] like Figure 1-4 As shown, the casting method of large ductile iron castings comprises the following steps:

[0035] S1. Core making:

[0036] a. First put a sand layer at the bottom of the core box 3, then splice the main core bone 1 and the auxiliary core bone 2 according to the shape of the mold, wind the exhaust rope on the main core bone 1, then put the spliced ​​main core bone 1 and the auxiliary core bone 2 into the sand layer, and finally fill in the molding sand for tamping;

[0037] The main core bone 1 is composed of a plurality of transverse ribs 11 and longitudinal ribs 12 connected together. A support rod 16 is provided at the bottom of the main core bone 1. The support rod 16 is a conical structure with a larger top and a smaller bottom, which is convenient for insertion into the sand layer. The first cross-shaped opening 14 is provided at both ends and sides of the transverse ribs 11 and the longitudinal ribs 12.

[0038] The inside of the transverse ribs 11 and the longitudinal ribs 12 are both provided with mutually connected airflow channels, the side of the transverse ribs 11 is provided with a first micro hole 13 connected with the airflow channel, and the top of the main core bone 1 is provided with a main exhaust pipe 15 connected with the airflow channel, the main exhaust pipe 15 extends out of the sand mold surface, and the diameter of the main exhaust pipe 15 is 100 to 300 mm. The main core bone 1 has the function of stable support in the sand core, improving the strength of the sand core and the smoothness of exhaust.

[0039] The auxiliary core bone 2 is provided with a cross-shaped inner cavity 21 inside, and the two ends of the auxiliary core bone 2 are respectively provided with a first cover 22 and a second cover 23 for sealing the cross-shaped inner cavity 21, the first cover 22 is provided with a cross-shaped protrusion 24, and the second cover 23 is provided with a second cross-shaped opening connected to the cross-shaped inner cavity 21. The cross-shaped protrusion 24 of the auxiliary core bone 2 is clamped with the first cross-shaped opening 14 of the main core bone 1 or the second cross-shaped opening of the auxiliary core bone 2, so as to realize the splicing between the auxiliary core bone 2 and the main core bone 1 and between the auxiliary core bones 2 and the auxiliary core bones 2, and can be combined into core bones of different shapes according to different cavity sizes and shapes, so that it is more flexible to use.

[0040] The bottom of the auxiliary core bone 2 is provided with an elongated groove 25 communicating with the cross-shaped inner cavity 21, a plurality of counterweights 26 are provided in the cross-shaped inner cavity 21, and a slider 27 extending out of the elongated groove 25 is provided at the bottom of the counterweights 26. The counterweights 26 are provided in the auxiliary core bone 2 to improve the strength, and the counterweights 26 can be increased or decreased in the auxiliary core bone 2 according to different requirements, and are easy to remove and install, thereby changing the weight of the core bone and better replacing the molding sand.

[0041] A second micro hole 211 communicating with the cross-shaped inner cavity 21 is provided on the side of the auxiliary core bone 2, and an auxiliary exhaust pipe 28 communicating with the cross-shaped inner cavity 21 is provided on the top of the auxiliary core bone 2. The auxiliary exhaust pipe 28 extends out of the sand mold surface, and the diameter of the auxiliary exhaust pipe 28 is 30-50 mm.

[0042] The core box 3 comprises a bottom plate 32, a left core box 33 and a right core box 34. The left core box 33 and the right core box 34 are movably connected on the bottom plate 32. A force-bearing plate 35 is provided on the side of the bottom plate 32. The bottom of the force-bearing plate 35 is fixed to the bottom plate 32 by a plurality of triangular ribs 38 to improve the strength of the force-bearing plate 35 and the firmness of the connection with the bottom plate 32. A plurality of positioning holes 36 are provided on the force-bearing plate 35. A hanging handle 37 with a T-shaped cross section is provided on the side of the left core box 33 and the right core box 34 close to the bottom plate 32.

[0043] b. Press the upper die downward onto the molding sand in the core box 3, knock the upper die from top to bottom, and knock the core box 3 from outside to inside to press out the desired sand core shape and remove the air in the molding sand;

[0044] c. After the sand core is hardened, the lower end of the crowbar 31 is inserted into the positioning hole 36. The inner diameter of the positioning hole 36 is larger than the diameter of the crowbar 31. A plurality of protrusions are provided on the inner wall of the positioning hole 36 to improve the connection stability with the crowbar 31 and prevent the crowbar 31 from being separated from the positioning hole 36. One side of the crowbar 31 is engaged with the hanging handle 37 on the left core box 33 or the right core box 34. Pressure is applied to the upper end of the crowbar 31, and the left core box 33 and the right core box 34 are stably moved to both sides by the lever principle, so that the core box 3 is opened and the sand core is taken out. The operation is flexible and convenient, with little damage to the core box 3, and the service life is extended. At the same time, the quality of the sand core is improved, and the yield rate of the sand core is as high as 99%.

[0045] S2. Modeling:

[0046] After the sand core is taken out, paint is applied on the surface of the sand core and on the inner wall of the sand box. The paint includes zircon powder paint and alcohol-based paint in a mass ratio of 1:1, and the paint ratio has a Baume degree of 28-35°Bé.

[0047] The sand core is placed in the mold cavity of the sand box, and an exhaust hole is punched on the box cover. The base sand is first filled in the chamber between the mold cavity and the inner wall of the sand box to make it flat, and then the auxiliary core bone 2 is placed. Finally, the molding sand is filled in the chamber to fill the gap between the auxiliary core bones 2. On the one hand, the auxiliary core bone 2 can enhance the strength of the molding sand, and exhaust is achieved through the second micropore 211 and the auxiliary exhaust pipe 28; on the other hand, it replaces the space of the molding sand, reduces the amount of molding sand, and reduces the cost; the auxiliary core bones 2 can also be spliced ​​in pairs through the cross-shaped protrusion 24 and the second cross-shaped mouth. The cross-shaped protrusion 24 can be disassembled, so that the first cross-shaped mouth 14 and the twenty-shaped mouth can be installed according to needs, and can be directly replaced after damage, which is low in cost.

[0048] S3, pouring: standardize pouring according to the products to be manufactured;

[0049] S4. Unpack and remove sand, and reuse the main core bone 1 and the auxiliary core bone 2.

[0050] The molding sand comprises the following materials by weight: 100 parts of silica sand, 0.8-1 parts of resin and 0.4-0.5 parts of curing agent, and the water content of the molding sand is less than 0.15%. The molding sand used has relatively less resin and curing agent and low water content, which can effectively reduce the gas generated by these substances at high temperature and reduce the amount of gas generated, thereby reducing shrinkage cavities, shrinkage, slag inclusions, pores and other quality defects.

Claims

1. Casting method of large ductile iron castings, Features: The following steps are involved: S1. Core making: a. First, a sand layer is placed at the bottom of the core box (3), and then the main core bone (1) and the auxiliary core bone (2) are spliced ​​according to the shape of the mold, and the exhaust rope is wound around the main core bone (1). Then, the spliced ​​main core bone (1) and the auxiliary core bone (2) are placed in the sand layer, and finally, the molding sand is filled in and compacted; b. Press the upper die downward onto the molding sand in the core box (3), knock the upper die from top to bottom, and knock the core box (3) from outside to inside to press out the desired sand core shape, and remove the air in the molding sand; c. After the sand core is hardened, the core box (3) is opened by using a crowbar (31) and the sand core is taken out by levering the core box (3); S2, molding: placing the sand core in the mold cavity of the sand box, punching an exhaust hole on the box cover, first filling the cavity between the mold cavity and the inner wall of the sand box with base sand to make it flat, then placing the secondary core bone (2), and finally filling the cavity with molding sand; S3, pouring; S4, unpacking and removing sand, and reusing the main core bone (1) and the auxiliary core bone (2); The main core bone (1) is composed of a plurality of transverse tendons (11) and longitudinal tendons (12) connected together. A support rod (16) is provided at the bottom of the main core bone (1). The support rod (16) is a conical structure with a larger top and a smaller bottom. Both ends and sides of the transverse tendons (11) and the longitudinal tendons (12) are provided with a first cross-shaped opening (14). The auxiliary core bone (2) is provided with a cross-shaped inner cavity (21) inside, and a first cover (22) and a second cover (23) for sealing the cross-shaped inner cavity (21) are provided at both ends of the auxiliary core bone (2), the first cover (22) is provided with a cross-shaped protrusion (24), and the second cover (23) is provided with a second cross-shaped opening connected to the cross-shaped inner cavity (21); the bottom of the auxiliary core bone (2) is provided with an elongated groove (25) connected to the cross-shaped inner cavity (21), and a plurality of counterweight blocks (26) are provided in the cross-shaped inner cavity (21), and the bottom of the counterweight blocks (26) is provided with a sliding block (27) extending out of the elongated groove (25); The main core bone (1) is provided with mutually connected air flow channels inside, the side of the main core bone (1) is provided with a first micro hole (13) connected to the air flow channel, and the top of the main core bone (1) is provided with a main exhaust pipe (15) connected to the air flow channel; the side of the auxiliary core bone (2) is provided with a second micro hole (211) connected to the cross-shaped inner cavity (21), and the top of the auxiliary core bone (2) is provided with an auxiliary exhaust pipe (28) connected to the cross-shaped inner cavity (21); The molding sand comprises the following materials in parts by weight: 100 parts of silica sand, 0.8-1 parts of resin and 0.4-0.5 parts of curing agent, and the water content of the molding sand is less than 0.15%.

2. The casting method of large ductile iron casting according to claim 1, Features: After the sand core is taken out, paint is applied on the surface of the sand core and on the inner wall of the sand box. The paint includes zircon powder paint and alcohol-based paint in a mass ratio of 1:1, and the paint ratio has a Baume degree of 28-35°Bé.

3. The casting method of large ductile iron casting according to claim 1, Features: The core box (3) comprises a bottom plate (32), a left core box (33) and a right core box (34); the left core box (33) and the right core box (34) are movably connected on the bottom plate (32); a force-bearing plate (35) is provided on the side of the bottom plate (32); a plurality of positioning holes (36) are provided on the force-bearing plate (35); and a hanging handle (37) with a T-shaped cross section is provided on one side of the left core box (33) and the right core box (34) close to the bottom plate (32).

4. The casting method of large ductile iron casting according to claim 3, Features: The inner diameter of the positioning hole (36) is greater than the diameter of the crowbar (31), and a plurality of protrusions are provided on the inner wall of the positioning hole (36).

5. The casting method of large ductile iron casting according to claim 3, Features: The bottom of the force-bearing plate (35) is fixed to the bottom plate (32) via a plurality of triangular ribs (38).